An energetic sealing structure and its preparation process
By designing an energetic sealing structure in underwater weapons and using an energetic compression layer formed by polyurethane-based energetic composite materials and fluororubber/polytetrafluoroethylene/ADN composite particles, the energy loss and safety hazards of explosives in the underwater environment are solved. solve the problem and achieve efficient waterproofing and high-security sealing effect.
Patent Information
- Application Number
- CN202211632567.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-19
AI Technical Summary
Existing underwater weapon sealing structures suffer from serious energy loss in the underwater environment. Traditional sealing measures cannot effectively prevent explosives from contacting seawater, and there are potential safety hazards during maintenance.
An energetic sealing structure is designed, including a metal shell, a protective layer, an energetic compression layer and a water-displacing layer. The protective layer is in contact with the main charge. The energetic compression layer is composed of polyurethane-based energetic composite materials. The water-displacing layer It is connected to the metal shell and prepared by spray drying to form a suspension of composite particles of polyurethane-based energetic composite material and fluororubber/polytetrafluoroethylene/ADN.
It achieves high-efficiency waterproofing of explosives. The coating and the main charge are detonated collaboratively. It has high safety, can maintain sealing performance under high and low temperature impacts, and meets the high-pressure water and temperature change requirements of underwater weapons.
Smart Images

Figure CN115979077B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of warheads, and relates to an energetic sealing structure and a preparation process thereof, and specifically to a composite structure and a preparation process thereof for sealing and waterproofing explosive products such as underwater weapons, underwater welding, and underwater cutting. Background Art
[0002] Underwater weapons mainly refer to weapons that damage targets in water. Traditional underwater weapons mainly include torpedoes, mines, depth charges, etc. Since underwater weapons are used in underwater environments, sealing technology has always been a basic and important technology that the industry attaches great importance to. The warhead of an underwater weapon is the final effective action unit of the underwater weapon. If the warhead charge is in contact with water for a long time, it will directly affect the explosive power of the warhead. Therefore, the sealing performance of the warhead directly affects the damage effect of the underwater weapon on the target. The quality of its sealing performance directly determines the underwater damage effect of the underwater weapon and even the success or failure of the mission. Therefore, good sealing of the underwater weapon warhead has become an important indicator of the design quality of underwater weapons.
[0003] The warhead charge of underwater weapons in service often uses cast explosive charge. Since the shell of the underwater weapon warhead is a cylinder plus annular ribs, there will be side gaps in the warhead charge, and there will be gaps between the warhead charge and the seawater. Therefore, it is necessary to ensure the sealing of the warhead charge. The waterproofing of explosive charge for underwater weapons is very important.
[0004] Traditional underwater weapon seals mainly rely on rubber sealing rings between metal shell components and shell components. During the maintenance and support of underwater weapons, the shell components need to be repeatedly disassembled and assembled. If water is found inside after disassembly, the underwater weapon needs to be destroyed. Moreover, once the internal explosive charge comes into contact with water, there is a great danger when disassembling the shell component, which poses a potential hazard to product maintenance. To alleviate this problem, the industry practice is to densely pack the explosive charge to reduce the amount of water contact. One method is to load low-energy explosives containing a large amount of high-molecular inert bodies, and the second is to wrap high-energy explosives with a large amount of high-molecular elastomers. Both methods ensure product safety by sacrificing energy.
[0005] In order to meet the sealing requirements in high-pressure water, similar fields outside the industry mainly use polymers to make seals to seal between strength components such as shell components. Its seals usually use polymer materials with high hardness and good wear resistance as the base material of the sealing product. For example, the document "Development of High-Hardness High-Pressure Water-Resistant Sealing Products" (Zhang Yangruyi, Xiang Yu. [J]. Rubber Science and Technology, 2020, 18(01): 23-26) proposed the use of composite structural materials with nylon cloth as reinforcement and nitrile rubber as rubber matrix to develop high-hardness high-pressure water-resistant sealing products. However, this type of process is only suitable for free space or local closed sealing, and is not suitable for body sealing in closed spaces. Summary of the invention
[0006] In order to solve the sealing problem of serious energy loss in the existing underwater weapon sealing structure, the present invention provides an energetic sealing and waterproof composite structure and a preparation process thereof.
[0007] To achieve the above object, the present invention discloses the following technical solutions:
[0008] An energetic sealing structure comprises a metal shell, a main charge is contained inside the shell, and a protective layer, an energetic compression layer and a water-displacing layer are sequentially arranged between the main charge and the shell;
[0009] The protective layer is in contact with the main charge and has a thickness of ≤0.5 mm;
[0010] The energetic compression layer is composed of a polyurethane-based energetic composite material; the thickness is ≥3.0 mm;
[0011] The water-displacing layer is connected to the metal shell and has a thickness of ≤0.5 mm.
[0012] Furthermore, the polyurethane-based energetic composite material comprises composite particles of fluororubber / polytetrafluoroethylene / ADN and a polyurethane matrix, and the mass ratio of the composite particles of fluororubber / polytetrafluoroethylene / ADN to the polyurethane matrix is 1:(3-4).
[0013] Furthermore, the fluororubber / polytetrafluoroethylene / ADN composite particles include preparing composite ADN balls by mechanically grinding ADN and polytetrafluoroethylene powder, then dissolving the fluororubber in ethyl acetate to form a solution, then blending the solution with the composite ADN balls to form a suspension, and finally spray drying the suspension.
[0014] Furthermore, the mass ratio of the ADN to the polytetrafluoroethylene powder is (18-22):1, and the mass ratio of the composite ADN ball to the fluororubber is (8-12):1.
[0015] Furthermore, the polyurethane matrix comprises preparing a mixed liquid by mixing DOA, polyazide glycidyl ether and polyisocyanate, and then curing the mixed liquid.
[0016] Furthermore, the mass ratio of the DOA, polyazide glycidyl ether and polyisocyanate is (12-13):(10-12):1.
[0017] The present invention also discloses a preparation process of an energetic sealing structure, which process comprises:
[0018] The inner wall of the metal shell is coated with a water-repellent layer, and the surface of the main charge is coated with a protective layer. Then, an energetic compression layer prepolymer is poured into the metal shell, and then the main charge coated with the protective layer is placed, until the energetic compression layer prepolymer overflows, so that the energetic compression layer prepolymer fills the inner space of the metal shell, and finally a plugging cover of the metal shell is assembled, and the energetic compression layer prepolymer is allowed to stand at room temperature to solidify into a polyurethane-based energetic composite material to form an energetic compression layer;
[0019] The protective layer comprises room temperature vulcanized silicone rubber with a thickness of ≤0.5 mm;
[0020] The thickness of the energetic compression layer is ≥3.0 mm;
[0021] The water-displacing layer comprises anaerobic adhesive and room temperature vulcanized silicone rubber, and has a thickness of ≤0.5 mm.
[0022] Specifically, the preparation of the compression layer prepolymer includes the following steps:
[0023] Step 1: ADN and polytetrafluoroethylene powder are mechanically ground into composite ADN balls, and then fluororubber is dissolved in ethyl acetate to form a solution, and then mixed with the composite ADN balls to form a suspension, and finally the suspension is spray-dried to obtain composite particles of fluororubber / polytetrafluoroethylene / ADN;
[0024] Step 2: DOA, polyazide glycidyl ether and polyisocyanate are mixed and stirred to prepare a mixed solution;
[0025] Step 3: Add the composite particles of fluororubber / polytetrafluoroethylene / ADN obtained in step 1 to the mixed solution of step 2, and stir to obtain a compression layer prepolymer. The mass ratio of the composite particles of fluororubber / polytetrafluoroethylene / ADN to the mixed solution is 1:(3-4).
[0026] More specifically, the mass ratio of ADN to polytetrafluoroethylene powder in step 1 is (18-22):1, and the mass ratio of the composite ADN ball to fluororubber is (8-12):1; the ADN particle size is less than 20 microns;
[0027] The mass ratio of DOA, polyazide glycidyl ether and polyisocyanate in step 2 is (12-13): (10-12): 1.
[0028] Preferably, in step 1, the mass ratio of ADN to polytetrafluoroethylene powder is 20:1, and the mass ratio of the composite ADN ball to fluororubber is 10:1;
[0029] The mass ratio of DOA, polyazide glycidyl ether and polyisocyanate in step 2 is 12.5:11.5:1.
[0030] Compared with the prior art, the present invention has the following technical effects:
[0031] The energetic sealing structure of the present invention (1) can achieve the purpose of waterproofing the charge; (2) the coating and the main charge have a synergistic detonation effect and have energy contribution; (3) high safety: the coating has low mechanical sensitivity; (4) it meets the requirements of high and low temperature impact. In addition, the preparation process of the energetic sealing structure of the present invention has simple steps and is easy to operate. It is a composite structure used for sealing and waterproofing explosive products such as underwater weapons, underwater welding, and underwater cutting.
[0032] The present invention is further described in detail below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the structure of the present invention;
[0034] Figure 2 It is a schematic diagram of the microstructure of the polyurethane-based energetic composite material of the present invention;
[0035] Figure 3 It is a schematic diagram of the waterproof test of the present invention;
[0036] Figure 4 is a scanning electron microscope image of the energetic compression layer of the present invention;
[0037] Figure 5 It is the CT result after the high and low temperature shock of the present invention;
[0038] Figure 6 This is a diagram of the filter paper state after the test of Comparative Example 3;
[0039] Among them, 1-protective layer, 2-energetic compression layer, 3-water-displacing layer, 4-main charge, 5-metal shell, 6-ADN, 7-fluororubber, 8-polytetrafluoroethylene, 9-polyurethane matrix, 10-interface gap, 11-cylinder, 12-plugging cover, 13-waterproof coating, 14-inner support, 15-filter paper, 16-water permeable hole, 17-inner hole, 18-composite particles of fluororubber / polytetrafluoroethylene / ADN. DETAILED DESCRIPTION
[0040] Any structural modification, proportional change or size adjustment should still fall within the scope of the technical content disclosed by the present invention without affecting the effects and purposes that can be achieved by the present invention.
[0041] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. All equivalent changes made on the basis of the technical scheme of this application fall within the protection scope of the present invention.
[0042] The concept of the present invention: Because it is impossible to solve the problem of efficient waterproofing of explosives directly, the existing waterproofing measures mainly rely on shell sealing. To solve the sealing problem of severe energy loss in the sealing structure of underwater weapons, it is necessary to meet the requirements of waterproofing, temperature shock, safety, etc. of underwater weapons at the same time, including: (1) The waterproof structure can withstand the static pressure impact of high-pressure water without leakage; (2) No gaps are generated under the impact of high and low temperatures, and the thermal expansion coefficient does not exceed that of the main charge. In the actual implementation process, the linear expansion coefficient of the general polymer seal can reach 10 -3 ~10 -4 / K, far exceeding the main explosive. If dense filling is used, under high temperature, the main charge and the seal will expand together, resulting in increased internal stress, which poses a safety risk; if a compressible structure is used, a large number of holes or vacuum holes are required, which increases the risk of leakage. If a structure is designed that has a certain compression space when there is no water seepage, it can meet the needs of use and maintenance of underwater weapons in high and low temperature environments, and can have a sealing function when encountering water. It can also be designed into a membrane structure that can be bonded to the main charge and the metal shell to meet the compatibility requirements of the main charge. This can solve the problem of efficient waterproofing of the main charge for underwater weapons.
[0043] Based on the above concept, the design idea of the present invention is to design an energetically sealed and waterproof composite structure and its preparation process. The structure is divided into three layers: protective layer, energetic compression layer and water-displacing layer. The protective layer is in contact with the main charge and meets the compatibility requirements with the explosives. The thickness is ≤0.5mm. The protective layer is based on the compatibility results of the energetic compression layer and the main charge. When the two are incompatible, an adhesive compatible with the main charge is selected to isolate the main charge and the energetic compression layer by coating and sealing. The energetic compression layer is an energetic compressible structure with a thickness of ≥3.0mm; the water-displacing layer is connected to the metal shell, ≤0.5mm, and anaerobic adhesive, room temperature vulcanized silicone rubber or other sealants can be selected.
[0044] The core technology of the present invention is the energetic compression layer in the structure. The energetic compression layer is a composite structure composed of a strong oxidizing energetic material and a polyurethane adhesive, wherein the strong oxidizing energetic material is coated with polytetrafluoroethylene and fluororubber. Due to the surface effect, there is a vacuum hole between the polytetrafluoroethylene coating and the polyurethane adhesive, which ensures that the internal stress of the main charge is released during high and low temperature impact. The strong oxidizing energetic material is selected from ammonium dinitramide (codenamed ADN). ADN is very easy to hydrolyze, and the density increases after hydrolysis. It forms a liquid capsule structure with fluororubber to increase the safety under the action of thermal expansion. Fluororubber can form a strong coating structure with ADN to protect ADN. At the same time, the chemical structure of fluororubber and polyurethane is stable, and a continuous phase structure with stable continuous phase can be formed. Polyurethane adopts an energetic binder matrix polyazide glycidyl ether (GAP), and the matrix structure is stable. DOA is dioctyl adipate, a plasticizer, which improves process stability; polyisocyanate (N100) and GAP can undergo a cross-linking reaction to form a polyurethane matrix.
[0045] In the present invention, the preparation of the compression layer prepolymer comprises the following steps:
[0046] Step 1: ADN and polytetrafluoroethylene powder are mechanically ground into composite ADN balls, and then fluororubber is dissolved in ethyl acetate to form a solution, and then mixed with the composite ADN balls to form a suspension, and finally the suspension is spray-dried to obtain composite particles of fluororubber / polytetrafluoroethylene / ADN;
[0047] Step 2: DOA, polyazide glycidyl ether and polyisocyanate are mixed and stirred to prepare a mixed solution;
[0048] Step 3: Add the composite particles of fluororubber / polytetrafluoroethylene / ADN obtained in step 1 to the mixed solution of step 2, and stir to obtain a compression layer prepolymer. The mass ratio of the composite particles of fluororubber / polytetrafluoroethylene / ADN to the mixed solution is 1:(3-4).
[0049] In step 1, the mass ratio of ADN to polytetrafluoroethylene powder is (18-22):1, and the mass ratio of composite ADN ball to fluororubber is (8-12):1; the ADN particle size is less than 20 microns;
[0050] In step 2, the mass ratio of DOA, polyazide glycidyl ether and polyisocyanate is (12-13): (10-12): 1.
[0051] Embodiment 1:
[0052] Combination Figures 1-2As shown, this embodiment is loaded with simulated underwater weapons, the main charge is JH-14, and the metal shell is made of 45# steel. The energetic sealing structure of this embodiment includes a metal shell 5, and the metal shell 5 is filled with a main charge 4. A protective layer 1, an energetic compression layer 2 and a water-displacing layer 3 are arranged in sequence between the main charge 4 and the metal shell 5;
[0053] The protective layer 1 is in contact with the main charge 4, and its thickness is ≤0.5mm; the material is room temperature vulcanized silicone rubber;
[0054] The energetic compression layer 2 is composed of a polyurethane-based energetic composite material; the thickness is ≥3.0 mm; the thickness of the energetic compression layer in this embodiment is 4.0 mm;
[0055] The water-displacing layer 3 is connected to the metal shell 5, has a thickness of ≤0.5 mm, and is made of room temperature vulcanized silicone rubber.
[0056] As a preferred embodiment of the present invention, the polyurethane-based energetic composite material includes composite particles of fluororubber / polytetrafluoroethylene / ADN and a polyurethane matrix, and the mass ratio of the composite particles of fluororubber / polytetrafluoroethylene / ADN to the polyurethane matrix is 1:(3-4). The particle size of ADN is less than 20 microns. ADN is coated with polytetrafluoroethylene and fluororubber, and there is an interface gap between the coating layer and the polyurethane matrix, such as Figure 2 shown.
[0057] As a preferred method of this embodiment, the composite particles of fluororubber / polytetrafluoroethylene / ADN include preparing composite ADN balls by mechanically grinding ADN and polytetrafluoroethylene powder, dissolving fluororubber in ethyl acetate to form a solution, blending the solution with the composite ADN balls to form a suspension, and finally spray drying the suspension.
[0058] As a preferred embodiment of the present invention, the mass ratio of ADN to polytetrafluoroethylene powder is (18-22):1, and the mass ratio of composite ADN ball to fluororubber is (8-12):1.
[0059] As a preferred embodiment of the present invention, the polyurethane matrix comprises preparing a mixed liquid by mixing DOA, polyazide glycidyl ether and polyisocyanate, and then curing the mixed liquid.
[0060] As a preferred embodiment of this embodiment, the mass ratio of DOA, polyazide glycidyl ether and polyisocyanate is (12-13): (10-12): 1.
[0061] This embodiment also discloses a preparation process of an energetic sealing structure, the process comprising:
[0062] A water-repelling layer is coated on the inner wall of the metal shell, and a protective layer is coated on the surface of the main charge. Then, an energetic compression layer prepolymer is poured into the metal shell, and then the main charge coated with the protective layer is placed in the metal shell until the energetic compression layer prepolymer overflows and fills the inner space of the metal shell with the energetic compression layer prepolymer. Finally, a plugging cover of the metal shell is assembled and allowed to stand at room temperature for more than 6 hours to allow the energetic compression layer prepolymer to cure into a polyurethane-based energetic composite material to form an energetic compression layer; the protective layer is made of room temperature vulcanized silicone rubber with a thickness of ≤0.5mm; the thickness of the energetic compression layer is 4.0mm; the water-repelling layer is made of room temperature vulcanized silicone rubber with a thickness of ≤0.5mm.
[0063] Specifically, the protective layer structure design: According to GJB772A-97 method 501.2, the compatibility of the energetic compression layer and JH-14 is tested, 40h, 100℃ gas release, when the gas release volume is ≤1.0mL, the protective layer thickness is 0mm; when the gas release volume is 1.0mm<≤3.0ml, the protective layer thickness is ≤0.5mm; when the gas release volume is greater than 3ml, the structure is not applicable. The protective layer selects a polymer coating that is compatible with the main charge.
[0064] In this embodiment, the degassing volume measured according to the above test method is 1.2 mL, and the thickness of the protective layer is selected to be 0.5 mm. The material of the protective layer is selected to be room temperature vulcanized silicone rubber compatible with the main charge.
[0065] Further, the preparation of the compression layer prepolymer comprises the following steps:
[0066] Step 1: ADN and polytetrafluoroethylene powder are mechanically ground into composite ADN balls, and then fluororubber is dissolved in ethyl acetate to form a solution, which is then blended with the composite ADN balls to form a suspension, and finally the suspension is injected into a spray dryer for spray drying to obtain composite particles of fluororubber / polytetrafluoroethylene / ADN;
[0067] The mass ratio of ADN to polytetrafluoroethylene powder is 20:1, and the mass ratio of composite ADN ball to fluororubber is 10:1. For example, weigh 1000g of composite particles of fluororubber / polytetrafluoroethylene / ADN and 100g of fluororubber;
[0068] Step 2: DOA, polyazide glycidyl ether and polyisocyanate are mixed and stirred to prepare a mixed solution;
[0069] Step 3: Add the fluororubber / polytetrafluoroethylene / ADN composite particles obtained in step 1 to the mixed solution of step 2, stir at 180 r / min for 10 to 20 minutes and then discharge to obtain the compression layer prepolymer. The mass ratio of the fluororubber / polytetrafluoroethylene / ADN composite particles to the mixed solution is 1:4, such as 4800 g of fluororubber / polytetrafluoroethylene / ADN composite particles and 1200 g of the mixed solution.
[0070] The mass ratio of DOA, polyazide glycidyl ether and polyisocyanate in step 2 is 12.5:11.5:1
[0071] Example 2
[0072] This embodiment uses a simulation device to carry out a waterproof test. The experimental device is designed as follows: Figure 3 As shown, the cylinder 11, the plug cover 12, and the inner support 14 are made of aluminum alloy, the cylinder 11 is provided with a water-permeable hole 16, and the inner support 14 is provided with an inner hole 17. The number of the water-permeable holes 16 is 6, and the diameter is 5 mm, simulating the water leakage condition of the shell 5; the number of the inner holes 17 is 40, and the diameter is 2 mm; the inner support 14 is filled with dried filter paper.
[0073] This embodiment includes a protective layer 1, an energetic compression layer 2 and a water-repelling layer 3. The protective layer 1 contacts the inner support 14, has a thickness of ≤0.5 mm, and is made of room temperature vulcanized silicone rubber; the energetic compression layer 2 is an energetic compressible structure, with a thickness of 3.0 mm; the water-repelling layer 3 is a water-repelling coating, connected to the cylinder 11, has a thickness of ≤0.5 mm, and is made of room temperature vulcanized silicone rubber, such as Figure 1 shown.
[0074] The preparation of the energetic compression layer prepolymer of this embodiment is the same as that of embodiment 1;
[0075] During the waterproof test: use transparent tape to seal the water permeable hole 16 on the outside of the cylinder 11, and use a manual brushing process to apply room temperature vulcanized silicone rubber to the cylinder 11, the inner wall of the plugging cover 12 and the surface of the inner support 14, with a thickness of ≤0.5mm; pour the energetic compression layer prepolymer prepared in step 3 into the cylinder 11, and put in the inner support 14 coated with room temperature vulcanized silicone rubber; the energetic compression layer prepolymer overflows naturally and fills the internal space, and finally the plugging cover is assembled and left to stand at room temperature for more than 6 hours to allow the energetic compression layer prepolymer to cure into a polyurethane-based energetic composite material to form an energetic compression layer.
[0076] Comparative Example 1
[0077] The difference between this comparative example and Example 2 is that there is no protective layer.
[0078] Comparative Example 2
[0079] The difference between this comparative example and Example 2 is that there is no water-displacing layer.
[0080] Comparative Example 3
[0081] This comparative example is based on the reference example and is completely filled with room temperature vulcanized silicone rubber.
[0082] Implementation effect evaluation
[0083] (1) The scanning electron microscopy of the energetic compression layer prepared in Example 1 after curing is as follows Figure 4As shown, composite particles 18 of fluororubber / polytetrafluoroethylene / ADN are attached to the polyurethane matrix 9, wherein an interface gap 10 exists between the composite particles 18 of fluororubber / polytetrafluoroethylene / ADN and the polyurethane matrix 9, thus realizing the structure designed by the present invention.
[0084] (2) The impact sensitivity of the energetic compression layer after curing in Example 1 was tested according to GJB772A-97 method 601.1. The test value was 10%, which is far lower than the safety index requirement of 40% for ordinary charges.
[0085] (3) Example 1 was subjected to high and low temperature impact tests, with a high temperature of 75°C and a low temperature of -40°C for three consecutive impacts. The CT scan after the impact was as follows: Figure 5 As shown, the structure is complete.
[0086] (4) According to the explosive detonation theory, the energy contribution of the composite structure of Example 1 is calculated. The energy contribution of the completely inert material is 5500 kJ, and the explosive heat contribution of Example 1 is 21600 kJ, which is an energy increase of 3.92 times.
[0087] (5) Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were placed in a water tank with a water pressure of 0.2 MPa and left for 10 days. After being taken out, the weight gain of the filter papers in Example 2, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were ≤1%, ≤1%, 26%, and 46%, respectively. Comparative Example 2 and Comparative Example 3 were moldy. The state of the filter paper in Comparative Example 3 after the test was as follows: Figure 6 shown.
[0088] It can be seen from the implementation effect that the present invention can achieve the purpose of waterproofing the charge, the coating and the main charge have a synergistic detonation effect and have energy contribution, the coating has low mechanical sensitivity and meets the requirements of high and low temperature impact.
[0089] In the above-listed embodiments, the purpose, technical solutions and advantages of the present invention are further described in detail. It should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0090] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0091] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0092] In addition, the various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the content invented by the present disclosure.
Claims
1. An energetic sealing structure, comprising a metal shell (5), wherein a main charge (4) is contained in the metal shell (5), characterized in that: A protective layer (1), an energetic compression layer (2) and a water-displacing layer (3) are sequentially arranged between the main charge (4) and the metal shell (5); The protective layer (1) is in contact with the main charge (4) and has a thickness of ≤0.5 mm; The energetic compression layer (2) is composed of a polyurethane-based energetic composite material; Thickness ≥3.0mm; The water-displacing layer (3) is connected to the metal shell (5) and has a thickness of ≤0.5 mm.
2. The energetic sealing structure according to claim 1, characterized in that: The polyurethane-based energetic composite material comprises composite particles of fluororubber / polytetrafluoroethylene / ADN and a polyurethane matrix, and the mass ratio of the composite particles of fluororubber / polytetrafluoroethylene / ADN to the polyurethane matrix is 1:(3-4).
3. The energetic sealing structure according to claim 2, characterized in that: The fluororubber / polytetrafluoroethylene / ADN composite particles include preparing composite ADN balls by mechanically grinding ADN and polytetrafluoroethylene powder, dissolving fluororubber in ethyl acetate to form a solution, blending the solution with the composite ADN balls to form a suspension, and finally spray drying the suspension.
4. The energetic sealing structure according to claim 3, characterized in that: The mass ratio of the ADN to the polytetrafluoroethylene powder is (18-22):1, and the mass ratio of the composite ADN ball to the fluororubber is (8-12):
1.
5. The energetic sealing structure according to claim 2, characterized in that: The polyurethane matrix comprises DOA, polyazide glycidyl ether and polyisocyanate, which are mixed and stirred to prepare a mixed liquid, and then the mixed liquid is cured to obtain the polyurethane matrix.
6. The energetic sealing structure according to claim 5, characterized in that: The mass ratio of the DOA, polyazide glycidyl ether and polyisocyanate is (12-13): (10-12):
1.
7. The process for preparing the energetic sealing structure according to any one of claims 1 to 6, characterized in that: The process includes: The inner wall of the metal shell is coated with a water-repellent layer, and the surface of the main charge is coated with a protective layer. Then, an energetic compression layer prepolymer is poured into the metal shell, and then the main charge coated with the protective layer is placed, until the energetic compression layer prepolymer overflows, so that the energetic compression layer prepolymer fills the inner space of the metal shell, and finally a plugging cover of the metal shell is assembled, and the energetic compression layer prepolymer is allowed to stand at room temperature to solidify into a polyurethane-based energetic composite material to form an energetic compression layer; The protective layer comprises room temperature vulcanized silicone rubber with a thickness of ≤0.5 mm; The thickness of the energetic compression layer is ≥3.0 mm; The water-displacing layer comprises anaerobic adhesive and room temperature vulcanized silicone rubber, and has a thickness of ≤0.5 mm.
8. The process for preparing the energetic sealing structure according to claim 7, characterized in that: The preparation of the energetic compression layer prepolymer comprises the following steps: Step 1: ADN and polytetrafluoroethylene powder are mechanically ground into composite ADN balls, and then fluororubber is dissolved in ethyl acetate to form a solution, and then mixed with the composite ADN balls to form a suspension, and finally the suspension is spray-dried to obtain composite particles of fluororubber / polytetrafluoroethylene / ADN; Step 2: DOA, polyazide glycidyl ether and polyisocyanate are mixed and stirred to prepare a mixed solution; Step 3: Add the composite particles of fluororubber / polytetrafluoroethylene / ADN obtained in step 1 to the mixed solution of step 2, and stir to obtain an energetic compression layer prepolymer. The mass ratio of the composite particles of fluororubber / polytetrafluoroethylene / ADN to the mixed solution is 1:(3~4).
9. The process for preparing the energetic sealing structure according to claim 8, characterized in that: The mass ratio of ADN to polytetrafluoroethylene powder in step 1 is (18-22):1, and the mass ratio of the composite ADN ball to fluororubber is (8-12):1; the ADN particle size is less than 20 microns; The mass ratio of DOA, polyazide glycidyl ether and polyisocyanate in step 2 is (12-13): (10-12):
1.
10. The process for preparing an energetic sealing structure according to claim 8, characterized in that: In step 1, the mass ratio of ADN to polytetrafluoroethylene powder is 20:1, and the mass ratio of the composite ADN ball to fluororubber is 10:1; The mass ratio of DOA, polyazide glycidyl ether and polyisocyanate in step 2 is 12.5:11.5:1.