Two-dimensional layered porous carbon material and its preparation method and application in lithium battery negative electrode material
Two-dimensional layered porous carbon materials were prepared by microwave heating composite solution agitation method and Schiff base reaction. The lithium dendrites caused by the cumbersome preparation of existing porous carbon materials and the volume changes of lithium batteries were solved by using nitrogen atom doping and Zn-N bonds. The problem is that efficient preparation of negative electrode materials for lithium-ion batteries is achieved, and the cycle performance and rate performance of the battery is improved.
Patent Information
- Application Number
- CN202211714241.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The existing preparation methods of porous carbon materials are cumbersome and dangerous, which limits the development of the negative electrode materials of lithium-ion batteries. The large volume changes during the cycle of lithium batteries lead to the formation of lithium dendrites and the reduction of battery capacity.
The microwave heating composite solution stirring method and the Schiff base reaction dehydration and condensation are used to form covalent organic frame COF. Combined with melamine and zinc nitrate hexahydrate, two-dimensional layered porous carbon material is prepared by microwave heating and high-temperature pyrolysis, and nitrogen atom doping and Zn-N bonds improve the conductivity and electrochemical properties of the material.
The negative electrode material of lithium-ion battery with high specific capacity and long cycle life is achieved, which simplifies the preparation process, saves time and effort, improves the circulation and rate performance of lithium-ion batteries, and reduces the generation of lithium dendrites.
Smart Images

Figure CN115986113B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of preparation of lithium battery negative electrode materials, and specifically relates to two-dimensional layered porous carbon materials and preparation methods thereof and their applications in lithium battery negative electrode materials. Background Art
[0002] The challenges faced by the development of lithium-ion batteries mainly include the formation of lithium dendrites and the corresponding problems, large volume changes during charging and discharging, etc. During the cycle process, lithium ion nuclei are continuously deposited as the current changes to form lithium dendrites, and some dendrites break to form "dead lithium", resulting in a decrease in battery capacity. If dendrites continue to grow, they will pierce the diaphragm, causing a short circuit inside the battery, thereby causing safety accidents such as thermal runaway and battery explosion.
[0003] During the cycle of lithium batteries, the volume of the negative electrode material will change greatly. The change in volume makes the SEI film uneven, resulting in uneven lithium deposition on the electrode, which aggravates the growth of lithium dendrites. In addition, during the cycle, large volume changes will cause degradation of active materials and electrodes, shortening the cycle life of the battery. The negative electrode material is one of the main factors affecting the performance of lithium-ion batteries, so it is particularly important to develop negative electrode materials with high specific capacity and long cycle life.
[0004] Porous carbon materials have attracted extensive attention from researchers in recent years due to their rich porous structure, excellent conductivity and large specific surface area. Their large specific surface area and excellent conductivity can effectively accelerate the transmission speed of lithium ions and provide a larger electrode / electrolyte interface for charge transfer reactions, making the deposition of lithium ions more uniform, thereby effectively reducing the generation of lithium dendrites. In addition, their rich porous structure can effectively shorten the transmission distance of lithium ions and provide sufficient buffer space for the large volume change of the electrode during the cycle. Therefore, they are regarded by researchers as one of the excellent negative electrode materials for lithium-ion batteries.
[0005] However, the current synthesis method of porous carbon is mostly hard template method, that is, mesoporous silica or zeolite molecular sieve is used as hard template, and then it is removed by strong acid or strong base in the subsequent step; that is, after the hard template such as silica, zeolite molecular sieve is fully mixed with the carbon source, it is pyrolyzed at high temperature, and then the pyrolyzed material is removed by acid such as hydrofluoric acid or strong base, and then the material treated with strong acid or strong base needs to be washed and dried; it can be seen that the hard template method has cumbersome operation steps, time-consuming and certain dangers, which greatly limits the preparation of porous carbon materials and also hinders the development of negative electrode materials for lithium-ion batteries to a certain extent. Therefore, it is necessary to study more efficient and simple methods for preparing porous carbon materials.
[0006] In view of this, this application is hereby filed. Summary of the invention
[0007] In order to solve one of the above-mentioned technical defects, the embodiments of the present application provide a two-dimensional layered porous carbon material, a preparation method thereof, and an application in lithium battery negative electrode materials.
[0008] According to the first aspect of the embodiment of the present application, a two-dimensional layered porous carbon material is provided, which has an extremely thin two-dimensional layered structure; the voids of the porous carbon material are unevenly distributed between the layers and present an irregular network; the two-dimensional layered porous carbon material is doped with rich nitrogen atoms; the nitrogen atoms exist in the forms of pyridine nitrogen, pyrrole nitrogen, Zn-N bonds and graphitic nitrogen.
[0009] The obtained two-dimensional layered porous carbon material has a large number of porous structures and a high specific surface area, which can shorten the transport length of lithium ions and provide a larger electrode / electrolyte interface for the charge transfer reaction. It has a continuous electron path and improves the specific capacity and stability of lithium-ion batteries.
[0010] According to a second aspect of the embodiment of the present application, a method for preparing a two-dimensional layered porous carbon material is provided, which is used to prepare the above-mentioned two-dimensional layered porous carbon material; the method comprises the following steps:
[0011] For the first time, microwave heating composite solution stirring method and Schiff base reaction dehydration condensation were used to generate covalent organic framework COF;
[0012] The acetonitrile solution of COF and the aqueous solution of melamine and zinc nitrate hexahydrate are mixed by microwave heating the composite solution again and stirring to obtain suspension A;
[0013] The suspension A is subjected to microwave heating for the second time and then dried to obtain a burnt brown solid precipitate B;
[0014] The solid precipitate B is placed in a Joule heating device for pore formation and carbon layer stripping to obtain a solid material C;
[0015] Material C is pyrolyzed at high temperature to prepare the target two-dimensional layered porous carbon material.
[0016] The embodiment of the present application uses Schiff base COF as a precursor and combines it with microwave treatment to prepare a two-dimensional layered porous carbon method, which fully utilizes the characteristics of Schiff base COF with a layered stacking structure and rich imine groups. The lone pair electrons on the imine group are used to make the nitrogen atom act as a coordinating atom to coordinate with the empty d orbital of the Zn atom, so that it can combine with Zn(NO3)2 fully and evenly. After pyrolysis, a two-dimensional layered porous carbon material is obtained.
[0017] Preferably, the covalent organic framework COF is generated by microwave heating of the composite solution stirring method and dehydration condensation by Schiff base reaction, specifically:
[0018] Under microwave heating, small molecule compounds containing aldehyde groups and small molecule compounds containing amino groups are selected as ligand materials through solution stirring method, and imine-rich COF is generated through Schiff base reaction.
[0019] Preferably, the amount of amino group to aldehyde group in the small molecule compound containing aldehyde group and the small molecule compound containing amino group is 1:1.
[0020] Preferably, the microwave heating conditions of the first microwave heating composite solution stirring method are: microwave treatment time is 1-2 hours, and microwave heating temperature is 60-80°C.
[0021] Preferably, the conditions for the second microwave heating are: microwave heating time is 2-3h, and microwave heating temperature is 40-60°C.
[0022] Preferably, the solid precipitate B is placed in a Joule heating device for pore formation and carbon layer stripping to obtain a solid material C. Specifically, the burnt brown solid precipitate B is placed in a graphite paper, placed in a Joule heating device, first evacuated to a vacuum environment, then argon is introduced, and in a flowing argon atmosphere, the temperature is rapidly raised to 1200-1500° C., and heated for 30-50 seconds to obtain a solid material C;
[0023] The target two-dimensional layered porous carbon material is prepared by high-temperature pyrolysis of material C. Specifically, the solid material C is placed in a quartz porcelain boat, put into a tubular furnace, and in a flowing argon atmosphere, the heating rate is selected to be 2-5°C / min. After the temperature is raised to 800-1000°C, it is heated for 2-3h to perform pore formation and carbon layer peeling treatment, and the COF organic carbon is further graphitized to prepare the target two-dimensional layered porous carbon material.
[0024] Preferably, the suspension A is subjected to microwave heating for a second time and then dried to obtain a brown solid precipitate B, and the drying conditions are as follows: drying in a drying oven at 100° C. for 10-12 hours to completely evaporate the solvent to obtain a brown solid precipitate B.
[0025] According to the first aspect of the embodiments of the present application, the above-mentioned two-dimensional layered porous carbon material or the two-dimensional layered porous carbon material obtained by the above-mentioned preparation method is used in lithium battery negative electrode materials.
[0026] Beneficial effects of this application:
[0027] 1. This application innovatively adopts a microwave method and a composite stirring method to prepare a two-dimensional layered porous carbon material using Schiff base COF as a precursor. The material morphology shows an ultra-thin two-dimensional structure; it has high conductivity and a continuous electron transmission path, and the rich porous structure can fully infiltrate and accommodate the electrolyte, thereby providing a larger electrode / electrolyte two-phase interface for the charge transfer reaction. These advantages can effectively improve the cycle performance and rate performance of lithium-ion batteries.
[0028] 2. The two-dimensional layered porous carbon material prepared in the present application is rich in nitrogen atom doping, which provides more active sites for the embedding of lithium ions in the subsequent charging and discharging process; at the same time, the nitrogen element in the two-dimensional porous carbon appears in four chemical components, namely pyridine nitrogen, pyrrole nitrogen, Zn-N bond and graphitic nitrogen; among which the existence of Zn-N bond changes the existence form of N element, and can also significantly improve the electrochemical performance of lithium-ion batteries.
[0029] 3. The preparation method of the present application utilizes microwave heating multiple times to accelerate the movement of molecules between ligands, thereby accelerating the reaction and shortening the time required for the entire synthesis process; no harsh conditions such as vacuum and pressurization are required, and the required COF material can be quickly generated through the Schiff base reaction by simply stirring the solution under microwave heating. The whole process saves time and effort, is simple and efficient.
[0030] 4. In the preparation method of the present application, the solid precipitate B obtained by mixing COF with melamine and zinc nitrate is subjected to Joule heating, which is conducive to the rapid decomposition of zinc nitrate. Due to the rapid decomposition and evaporation of zinc nitrate in a short time, the sites originally anchored on COF will have cavities, and due to the release of gas during the decomposition process, the original morphology is destroyed, and COF is stripped into ultra-thin carbon sheets. In this process, no pore-forming agent or carbon layer stripping agent is added, but it plays a pore-forming role, and the large amount of gas released by rapid decomposition in a short time plays the role of stripping the carbon layer. Finally, the material C is pyrolyzed at high temperature to prepare the target two-dimensional layered porous carbon material, and Zn(NO3)2 is completely decomposed by high temperature, and the COF organic carbon is further graphitized while forming pores and stripping the carbon layer, making it more conductive. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0032] Figure 1 Scanning electron microscopy of the two-dimensional layered porous carbon material prepared in this embodiment Figure 1 ;
[0033] Figure 2Scanning electron microscopy of the two-dimensional layered porous carbon material prepared in this embodiment Figure 2 ;
[0034] Figure 3 Scanning electron microscopy of the two-dimensional layered porous carbon material prepared in this embodiment Figure 3 ;
[0035] Figure 4 Scanning electron microscopy of the two-dimensional layered porous carbon material prepared in this embodiment Figure 4 ;
[0036] Figure 5 Transmission electron microscopy of the two-dimensional layered porous carbon material prepared in the present application example Figure 1 ;
[0037] Figure 6 Transmission electron microscopy of the two-dimensional layered porous carbon material prepared in the present application example Figure 2 ;
[0038] Figure 7 High-resolution XPS spectrum of nitrogen in the two-dimensional layered porous carbon material prepared in the embodiment of the present application;
[0039] Figure 8 This is a high-resolution XPS spectrum of zinc in the two-dimensional layered porous carbon material prepared in the embodiment of the present application;
[0040] Fig. 9 The two-dimensional layered porous carbon material and the material without Zn-N bond prepared in the present application example are used as the negative electrode material of lithium battery respectively. -1 Comparison of cycling performance at current density of;
[0041] Fig.10 When the two-dimensional layered porous carbon material prepared in the present embodiment is used as the negative electrode of lithium battery, at 0.5Ag -1 Cyclic performance diagram at current density of ;
[0042] Fig.11 This is a rate performance diagram at different current densities when the two-dimensional layered porous carbon material prepared in the embodiment of the present application is used as a lithium battery negative electrode. DETAILED DESCRIPTION
[0043] In order to make the technical solutions and advantages in the embodiments of the present application more clearly understood, the exemplary embodiments of the present application are further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than an exhaustive list of all the embodiments. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict.
[0044] An embodiment of the present application provides a two-dimensional layered porous carbon material having an extremely thin two-dimensional layered structure; the pores of the porous carbon material are unevenly distributed between the layers and present an irregular network; the two-dimensional layered porous carbon material is doped with rich nitrogen atoms; the nitrogen atoms exist in the form of pyridine nitrogen, pyrrole nitrogen, Zn-N bonds and graphitic nitrogen.
[0045] like Figures 1 to 6 As shown, the material morphology shows an extremely thin two-dimensional layered porous carbon structure; the rich porous structure can fully infiltrate and accommodate the electrolyte, thereby providing a larger electrode / electrolyte two-phase interface for the charge transfer reaction. These advantages can effectively improve the cycle performance and rate performance of lithium-ion batteries.
[0046] like Figures 7 and 8 As shown, through the X-ray photoelectron spectroscopy (XPS) analysis of the two-dimensional porous carbon material, it can be seen that the XPS high-resolution spectrum of zinc element shows that the content of residual zinc element is very small, only about 0.5at.%, and Zn2p 3 / 2 The peak appears at 1022 eV, indicating that the zinc element exists in the form of Zn 0 , instead of Zn 2+ , indicating that the decomposition process of zinc nitrate is complete and thorough. The XPS high-resolution energy spectrum of nitrogen element shows that the nitrogen element in the two-dimensional porous carbon appears four chemical components: pyridinic nitrogen, pyrrolic nitrogen, Zn-N bond and graphitic nitrogen. Among them, the Zn-N bond can be attributed to the vaporized residual zinc element changing the chemical environment of the nitrogen element in the two-dimensional porous carbon material. In addition, the residual zinc atoms can also improve the electrochemical performance of lithium-ion batteries. In other words, the two-dimensional layered porous carbon material prepared in this application is rich in nitrogen atom doping, which provides more active sites for the embedding of lithium ions in the subsequent charging and discharging process; at the same time, the nitrogen element in the two-dimensional porous carbon appears four chemical components, namely pyridinic nitrogen, pyrrolic nitrogen, Zn-N bond and graphitic nitrogen.
[0047] like Fig. 9 As shown in the figure, it can be seen that the two-dimensional porous carbon material prepared in the embodiment of the present application contains a Zn-N bond material at a current density of 0.2A. -1 After 145 cycles, the specific capacity can reach 542 mAh g -1 However, the material without Zn-N bond has a specific capacity of only 312 mAh g -1 This is because the existence of the Zn-N bond changes the existence form of the N element and can also significantly improve the electrochemical performance of lithium-ion batteries.
[0048] The embodiment of the present application provides a method for preparing a two-dimensional layered porous carbon material, which is used to prepare the above-mentioned two-dimensional layered porous carbon material; the method comprises the following steps:
[0049] (1) For the first time, microwave heating of composite solution stirring method and Schiff base reaction dehydration condensation were used to generate covalent organic framework COF; this step is based on Schiff base reaction to prepare covalent organic framework, and the whole reaction process uses microwave heating process to accelerate the movement of ligand molecules, and only needs to stir for 1-2 hours to complete the Schiff base reaction process. Compared with many covalent organic framework preparation methods that require vacuum and long-term heating, it is time-saving and labor-saving and simpler. Different COF ligands can also be selected for synthesis according to needs, and the selection of ligands includes but is not limited to: p-phenylenediamine, m-phenylenediamine, o-phenylenediamine, terephthalaldehyde, m-phthalaldehyde, o-phthalaldehyde, trimesic acid, 1,3,5-tris(4-aminophenyl)benzene. It is worth noting that the amount of amino and aldehyde groups in the small molecule compound containing aldehyde group and the small molecule compound containing amino group is 1:1.
[0050] (2) stirring and mixing the acetonitrile solution of COF, the aqueous solution of melamine and zinc nitrate hexahydrate at room temperature to obtain a suspension A;
[0051] (3) The suspension A is subjected to microwave heating for a second time and then dried to obtain a brown solid precipitate B. In the implementation, the mixture of COF, melamine and zinc nitrate is treated by microwave heating to accelerate the molecular motion, thereby making the three mixed more uniformly and ensuring the uniformity of the morphology obtained subsequently.
[0052] (4) placing the solid precipitate B in a Joule heating device for pore formation and carbon layer stripping to obtain a solid material C;
[0053] (5) Material C is pyrolyzed at high temperature to prepare the target two-dimensional layered porous carbon material.
[0054] In the embodiment of the present application, when preparing a two-dimensional layered porous carbon material, the Joule heating method is first used to decompose and evaporate the zinc nitrate particles in a short time, thereby playing the role of a pore-forming agent and a carbon layer stripping agent. Then, when preparing a two-dimensional layered porous carbon material, a high-temperature pyrolysis method is used to form pores and strip the carbon layer. There is no need to use hard templates such as mesoporous silica and zeolite molecular sieves to form pores, so in the subsequent process, acid washing, alkali washing, centrifugal drying and other processes are eliminated, which reduces costs and greatly simplifies the operating steps, making the entire operation process simpler and easier, and reducing harm to the environment.
[0055] In the process of preparing the two-dimensional layered carbon material in the embodiment of the present application, the characteristics of the Schiff base COF with interlayer stacking structure and rich imine groups are fully utilized to ensure that the coordination process with metal atoms is uniform and sufficient. The stacking structure is destroyed in the subsequent pyrolysis process to obtain an ultra-thin two-dimensional porous carbon material.
[0056] The preparation method provided in the embodiment of the present application adopts a microwave heating composite solution stirring method and utilizes a Schiff base reaction dehydration condensation to generate a covalent organic framework COF, specifically:
[0057] Under microwave heating, small molecule compounds containing aldehyde groups and small molecule compounds containing amino groups are selected as ligand materials through solution stirring method, and imine-rich COF is generated through Schiff base reaction.
[0058] The preparation method provided in the examples of the present application adopts the microwave heating conditions of the first microwave heating composite solution stirring method as follows: the microwave treatment time is 1-2 hours and the microwave heating temperature is 60-80°C.
[0059] In the preparation method provided in the examples of the present application, the conditions for the second microwave heating are: the microwave heating time is 2-3h, and the microwave heating temperature is 40-60°C.
[0060] The preparation method provided in the embodiment of the present application is to place the solid precipitate B in a Joule heating device for pore formation and carbon layer stripping to obtain a solid material C. Specifically, the burnt brown solid precipitate B is placed in a graphite paper, placed in a Joule heating device, first evacuated to a vacuum environment, then argon gas is introduced, and in a flowing argon atmosphere, the temperature is quickly raised to 1200-1500° C., and heated for 30-50 seconds to obtain a solid material C;
[0061] The target two-dimensional layered porous carbon material is prepared by high-temperature pyrolysis of material C. Specifically, the solid material C is placed in a quartz porcelain boat, put into a tubular furnace, and in a flowing argon atmosphere, the heating rate is selected to be 2-5°C / min. After the temperature is raised to 800-1000°C, it is heated for 2-3h to perform pore formation and carbon layer peeling treatment, and the COF organic carbon is further graphitized to prepare the target two-dimensional layered porous carbon material.
[0062] In the preparation method provided in the embodiment of the present application, the suspension A is subjected to microwave heating for a second time and then dried to obtain a brown solid precipitate B. The drying conditions are as follows: drying in a drying oven at 100°C for 10-12 hours to completely evaporate the solvent to obtain a brown solid precipitate B.
[0063] As an embodiment of the present application, a method for preparing a two-dimensional layered porous carbon material is provided with the following specific steps:
[0064] S1: 700-750 mg of terephthalaldehyde and 550-600 mg of p-phenylenediamine were mixed in 80-100 ml of anhydrous ethanol, ultrasonically dispersed for 5-15 minutes, and then 3-5 ml of glacial acetic acid were added, and ultrasonically dispersed again for 5-15 minutes, and then placed in a microwave heating device and stirred the solution for 1-2 hours and 60-80°C. After the reaction was completed, the resulting suspension was centrifuged twice with alcohol and water to obtain a yellow precipitate, which was then placed in a drying oven and dried at 60°C-80°C for 10-12 hours to obtain COF.
[0065] S2: 0.6-1.0 g of the COF material prepared in step S1 is dissolved in 30-50 ml of acetonitrile solution, and then 0.3-0.5 g of melamine and 1.2-2.0 g of zinc nitrate hexahydrate are dissolved in 20-30 ml of deionized water and stirred evenly, and then the aqueous solution containing melamine and zinc nitrate hexahydrate is poured into the acetonitrile solution containing COF to obtain a suspension containing the above three materials. The suspension is stirred at room temperature for 1-2 hours.
[0066] S3: Place the stirred solution in a microwave heating device, set the time to 2-3 hours, and set the temperature to 40-60° C. After the end, place the mixed suspension in a drying oven, and dry it at 100° C. for 10-12 hours to completely evaporate the solvent to obtain a brown solid precipitate B.
[0067] S4: Place the above-mentioned burnt brown solid precipitate B in graphite paper, put it into a Joule heating device, first evacuate it to a vacuum environment, then introduce argon gas, and quickly heat it to 1200-1500°C in a flowing argon atmosphere for 30-50 seconds to obtain an incompletely carbonized COF material C. This step is to allow the Zn(NO3)2 particles to decompose quickly, acting as a pore-forming agent and a carbon layer stripping agent.
[0068] S5: Place the COF material C that has not been completely carbonized after Joule heating in a quartz boat, put it into a tube furnace, and heat it to 800-1000°C for 2-3h in a flowing argon atmosphere. The heating rate is 2-5°C / min. This step is to allow Zn(NO3)2 to decompose completely as a pore-forming agent and a stripping agent for the carbon layer, and further graphitize the COF organic carbon to make it more conductive. After the high-temperature pyrolysis is completed, a two-dimensional layered porous carbon material can be obtained.
[0069] The embodiments of the present application provide the application of the above-mentioned two-dimensional layered porous carbon material or the two-dimensional layered porous carbon material obtained according to the above-mentioned preparation method in lithium battery negative electrode materials.
[0070] like Figure 10 to Figure 11 As shown, the electrochemical performance test of the two-dimensional layered porous carbon material prepared in this application was carried out.
[0071] like Fig.10 As shown, when the two-dimensional layered porous carbon material prepared in the embodiment of the present application is used as the negative electrode material of the lithium ion battery, at 0.5A g -1 At a current density of 1.547 W, after 300 consecutive cycles, the specific capacity can still reach 515.9 mAh g -1 The higher specific capacity indicates that the two-dimensional layered porous carbon material can provide sufficient lithium storage active sites.
[0072] like Fig.11 As shown, when the two-dimensional layered porous carbon material prepared in the embodiment of the present application is used as the negative electrode material of the lithium ion battery, the current density is 0.1A g -1 ,0.3Ag -1 ,0.5Ag -1 ,1.0Ag -1 ,3.0Ag -1 ,5.0A g -1 When the reversible specific capacity can reach 701mAh g -1 ,494mAh g -1 ,434mAh g -1 ,343mAh g -1 ,247mAh g -1 , 191mAh g -1 When the current density returns to 0.3Ag -1 When the specific capacity is 443 mAh g -1 , indicating that the material has good reversibility and the unique two-dimensional layered porous structure accelerates the transmission of electrons and lithium ions.
[0073] Based on the above, the two-dimensional layered porous carbon material prepared in the present application, when used as the negative electrode material of a lithium-ion battery, gives full play to the advantages of the material having a rich pore structure and a large specific surface area, promotes the uniform deposition of lithium ions to avoid the appearance of lithium dendrites, and at the same time buffers the large volume changes during the charge and discharge process, thereby improving the cycle performance and rate performance of the lithium-ion battery. Although the preferred embodiments of the present application have been described, once the technicians in this field know the basic creative concepts, they can make additional changes and modifications to these embodiments. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present application.
[0074] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.
Claims
1. A two-dimensional layered porous carbon material, It is characterized in that It has an extremely thin two-dimensional layered structure; the pores of the porous carbon material are unevenly distributed between the sheets and sheets, presenting an irregular network; the two-dimensional layered porous carbon material is doped with abundant nitrogen atoms; the nitrogen atoms exist in the form of pyridinic nitrogen, pyrrolic nitrogen, Zn-N bonds and graphitic nitrogen; The method for preparing the two-dimensional layered porous carbon material comprises the following steps: For the first time, the microwave heating composite solution stirring method and the Schiff base reaction were used to generate the covalent organic framework COF by dehydration condensation; specifically, under microwave heating, the solution stirring method was used to select small molecule compounds containing aldehyde groups and small molecule compounds containing amino groups as ligand materials, and the imine-rich COF was generated by the Schiff base reaction; the microwave heating conditions of the microwave heating composite solution stirring method for the first time were: the microwave treatment time was 1-2 hours, and the microwave heating temperature was 60-80°C; The acetonitrile solution of COF and the aqueous solution of melamine and zinc nitrate hexahydrate were mixed uniformly by stirring at room temperature to obtain a suspension A; The suspension A is subjected to microwave heating for the second time and dried to obtain a brown solid precipitate B; the conditions for the second microwave heating are: microwave heating time is 2-3h, and microwave heating temperature is 40-60°C; The solid precipitate B is placed in a Joule heating device for pore formation and carbon layer stripping to obtain a solid material C; in a flowing argon atmosphere, the temperature is rapidly raised to 1200-1500° C. and heated for 30-50 seconds to obtain a solid material C; Material C is pyrolyzed at high temperature to prepare the target two-dimensional layered porous carbon material.
2. A method for preparing a two-dimensional layered porous carbon material, It is characterized in that Used to prepare the two-dimensional layered porous carbon material according to claim 1; comprising the following steps: For the first time, microwave heating composite solution stirring method and Schiff base reaction dehydration condensation were used to generate covalent organic framework COF; specifically, under microwave heating, small molecule compounds containing aldehyde groups and small molecule compounds containing amino groups were selected as ligand materials through solution stirring method, and imine-rich COF was generated through Schiff base reaction; The microwave heating conditions of the first microwave heating composite solution stirring method are as follows: microwave treatment time is 1-2 hours, microwave heating temperature is 60-80°C; The acetonitrile solution of COF and the aqueous solution of melamine and zinc nitrate hexahydrate were mixed uniformly by stirring at room temperature to obtain a suspension A; The suspension A is subjected to microwave heating for the second time and dried to obtain a brown solid precipitate B; the conditions for the second microwave heating are: microwave heating time is 2-3h, and microwave heating temperature is 40-60°C; The solid precipitate B is placed in a Joule heating device for pore formation and carbon layer stripping to obtain a solid material C; specifically, in a flowing argon atmosphere, the temperature is rapidly raised to 1200-1500° C. and heated for 30-50 seconds to obtain the solid material C; Material C is pyrolyzed at high temperature to prepare the target two-dimensional layered porous carbon material.
3. The preparation method according to claim 2, It is characterized in that The amount of amino groups and aldehyde groups in the small molecule compound containing aldehyde groups and the small molecule compound containing amino groups is 1:
1.
4. The preparation method according to claim 2, It is characterized in that The solid precipitate B is placed in a Joule heating device for pore formation and carbon layer stripping to obtain a solid material C. Specifically, the burnt brown solid precipitate B is placed in a graphite paper, placed in a Joule heating device, first evacuated to a vacuum environment, and then argon gas is introduced; The target two-dimensional layered porous carbon material is prepared by high-temperature pyrolysis of material C. Specifically, the solid material C is placed in a quartz porcelain boat, put into a tubular furnace, and in a flowing argon atmosphere, the heating rate is selected to be 2-5°C / min. After the temperature is raised to 800-1000°C, it is heated for 2-3h to perform pore formation and carbon layer peeling treatment, and the COF organic carbon is further graphitized to prepare the target two-dimensional layered porous carbon material.
5. The preparation method according to claim 2, It is characterized in that The suspension A is subjected to microwave heating for the second time and dried to obtain a brown solid precipitate B. The drying conditions are as follows: drying in a drying oven at 100° C. for 10-12 hours to completely evaporate the solvent to obtain a brown solid precipitate B.
6. Use of the two-dimensional layered porous carbon material according to claim 1 or the two-dimensional layered porous carbon material obtained by the preparation method according to any one of claims 2 to 5 in lithium battery negative electrode materials.
Citation Information
Patent Citations
Zinc-based negative electrode material preparation method
CN110534729A
Method for preparing porous carbon nanosheet through pyrolysis of two-dimensional covalent organic framework
CN113845107A