Resin composition and molded article

Through a specific proportion of 4-methyl-1-pentene copolymer resin composition, the problem of difficulty in balancing heat resistance and electrical properties in capacitor films is solved, and a smooth film with small surface roughness is realized, improving the quality of capacitors. stability and longevity.

CN115989249BActive Publication Date: 2024-10-18MITSUI CHEMICALS INC
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202180053515.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-30
Publication Date
2024-10-18
Estimated Expiration
2041-08-30

AI Technical Summary

Technical Problem

It is difficult for the existing 4-methyl-1-pentene copolymer to simultaneously meet the requirements for heat resistance, electrical properties and surface roughness in capacitor films, resulting in deterioration of dielectric properties and shortened life.

Method used

Using a specific proportion of 4-methyl-1-pentene copolymer resin composition, by adjusting the mole percentage and molecular structure of the copolymer, a film with small surface roughness and smoothness is prepared to ensure the heat resistance and electrical properties of the film. .

Benefits of technology

The heat resistance and electrical properties of the capacitor film are improved, the problems of deterioration of dielectric properties and shortened life are avoided, and more stable capacitance performance is provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004813724260000121
    Figure GDA0004813724260000121
  • Figure GDA0004813724260000141
    Figure GDA0004813724260000141
  • Figure GDA0004813724260000171
    Figure GDA0004813724260000171
Patent Text Reader

Abstract

The present invention is a resin composition containing a 4-methyl-1-pentene copolymer (A) that meets specific requirements and a 4-methyl-1-pentene copolymer (B) that meets specific requirements. The resin composition of the present invention contains a 4-methyl-1-pentene copolymer, and a film having properties such as heat resistance and a small and smooth surface roughness can be obtained, which can be suitably used for a molded body such as a capacitor film. The surface roughness of the capacitor film of the present invention is small and smooth, thereby eliminating the problems of dielectric property degradation and shortened life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition containing a 4-methyl-1-pentene copolymer and a molded product such as a capacitor film containing the resin composition. Background Art

[0002] 4-methyl-1-pentene polymers are excellent in heat resistance, transparency, electrical properties, etc. compared to polyethylene and polypropylene, and therefore are widely used in various applications. Specifically, capacitor films composed of 4-methyl-1-pentene copolymers are known.

[0003] Patent document 1 records a 4-methyl-1-pentene (co)polymer composition obtained by mixing a 4-methyl-1-pentene (co)polymer and a 4-methyl-1-pentene-α-olefin copolymer in a specific ratio, and records that a hollow molded body formed from the composition has excellent transparency, heat resistance, electrical properties, mechanical properties, uniform stretchability, and dimensional stability.

[0004] Patent Document 2 describes that a capacitor film obtained from a 4-methyl-1-pentene copolymer having specific physical properties has electrical characteristics such as a small capacitance drop rate and stable dielectric loss characteristics when a voltage is applied for a long period of time at high temperature.

[0005] Patent Document 3 describes that a 4-methyl-1-pentene copolymer composition comprising a specific 4-methyl-1-pentene (co)polymer and a 4-methyl-1-pentene copolymer (B) has transparency and rigidity, high impact resistance, and further high heat resistance.

[0006] Patent Document 4 describes that specific 4-methyl-1-pentene polymer particles can reduce rigidity, that is, improve flexibility, without impairing properties such as high stereoregularity and excellent heat resistance.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2013 / 099876

[0010] Patent Document 2: Japanese Patent Application Publication No. 2014-11182

[0011] Patent Document 3: Japanese Patent Application Publication No. 2018-162408

[0012] Patent Document 4: International Publication No. 2019 / 198694 Summary of the invention

[0013] Problems to be solved by the invention

[0014] In order to properly perform the security function, the capacitor film needs to prevent strong adhesion between the films, and the surface roughness must be properly controlled. In addition, if the surface roughness of the capacitor film is large, there are problems such as deterioration of dielectric properties or shortened life.

[0015] The 4-methyl-1-pentene copolymers and the like described in the above patent documents still cannot provide films that satisfy both the properties suitable for capacitor applications (eg, electrical properties, heat resistance, and stretchability) and the requirement for suppressing surface roughness.

[0016] An object of the present invention is to provide a resin composition containing a 4-methyl-1-pentene copolymer, which can obtain a film having properties such as heat resistance and having a small surface roughness and is smooth, and can be suitably used for a molded body such as a capacitor film.

[0017] Methods for solving problems

[0018] The present inventors have conducted intensive studies to solve the above problems and have found that a resin composition containing two specific 4-methyl-1-pentene copolymers at a specific ratio can solve the above problems, thereby completing the present invention.

[0019] The present invention relates to, for example, the following [1] to [7].

[0020] [1] A resin composition comprising a 4-methyl-1-pentene copolymer (A) satisfying the following requirements (Aa) to (Ad) and a 4-methyl-1-pentene copolymer (B) satisfying the following requirements (Ba) to (Bd), and satisfying the following requirements (1) and (2).

[0021] (Aa) The amount (U1) of constituent units derived from 4-methyl-1-pentene is 80.0 to 99.9 mol%, and the total amount (U2) of constituent units derived from at least one selected from linear α-olefins having 2 to 20 carbon atoms is 20.0 to 0.1 mol% (wherein the total of the aforementioned U1 and the aforementioned U2 is set to 100 mol%).

[0022] (Ab) Intrinsic viscosity measured in decalin at 135°C [η] A 0.5~5.0dL / g.

[0023] (Ac) When the copolymer (A) is measured by a cross fractionation chromatograph (CFC) using an infrared spectrophotometer as a detection unit, at least one peak of the eluted component exists in the range of 100 to 140°C.

[0024] (Ad) When the copolymer (A) is measured by the CFC, the molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the eluted component in the range of 100 to 140°C, is 1.0 to 4.5.

[0025] (Ba) The amount (U3) of constituent units derived from 4-methyl-1-pentene is 20.0 to 98.0 mol%, and the total amount (U4) of constituent units derived from at least one selected from linear α-olefins having 2 to 20 carbon atoms is 80.0 to 2.0 mol% (wherein the total of the aforementioned U3 and the aforementioned U4 is set to 100 mol%).

[0026] (Bb) Intrinsic viscosity measured in decalin at 135°C [η] B 2.0~8.0dL / g.

[0027] (Bc) When the copolymer (B) is measured by a cross fractionation chromatograph (CFC) using an infrared spectrophotometer as a detection unit, at least one peak of the eluted component exists in the range of 0°C or higher and lower than 100°C.

[0028] (Bd) When the copolymer (B) is measured by the CFC, the molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the eluted component in the range of 0°C to less than 100°C, is 1.0 to 7.0.

[0029] (1) When the total content of the copolymers (A) and (B) is 100 parts by mass, the content of the copolymer (A) is 5 to 95 parts by mass, and the content of the copolymer (B) is 95 to 5 parts by mass.

[0030] (2) The value (U4-U2) obtained by subtracting U2 (mol %) described in the above requirement (Aa) from U4 (mol %) described in the above requirement (Ba) is 0 mol % or more and 6.5 mol % or less.

[0031] [2] The resin composition described in [1], wherein, when the total content of the copolymer (A) and the copolymer (B) is 100 parts by mass, the content of the copolymer (A) is 5 parts by mass or more and less than 50 parts by mass, and the content of the copolymer (B) is greater than 50 parts by mass and less than 95 parts by mass.

[0032] [3] The resin composition according to [1] or [2], wherein the linear α-olefins in the copolymers (A) and (B) are each independently a linear α-olefin having 10 to 20 carbon atoms.

[0033] [4] A molded article comprising the resin composition according to any one of [1] to [3].

[0034] [5] A film comprising the resin composition according to any one of [1] to [3].

[0035] [6] A film satisfying the following requirements (I) to (III).

[0036] (I) Contains at least two 4-methyl-1-pentene copolymers.

[0037] (II) The surface roughness (Ra) of the film is less than 100 nm.

[0038] (III) The surface roughness (Rz) of the film is less than 500 nm.

[0039] [7] The film according to [5] or [6], which is a capacitor film.

[0040] Effects of the Invention

[0041] The resin composition of the present invention contains a 4-methyl-1-pentene copolymer, and can obtain a film having properties such as heat resistance and a small surface roughness and smoothness, and can be suitably used for a molded body such as a capacitor film. The capacitor film of the present invention has a small surface roughness and is smooth, thereby eliminating the problems of deterioration of dielectric properties and shortened life. DETAILED DESCRIPTION

[0042] Various physical properties are described in the following description, and the details of the measurement conditions of the various physical properties are described in the column of Examples.

[0043] [Resin composition]

[0044] The resin composition of the present invention contains the 4-methyl-1-pentene copolymer (A) and the 4-methyl-1-pentene copolymer (B) described below, and satisfies the following requirements (1) and (2).

[0045] <4-Methyl-1-pentene copolymer (A)>

[0046] The 4-methyl-1-pentene copolymer (A) (hereinafter also referred to as "copolymer (A)") comprises a constituent unit derived from 4-methyl-1-pentene and a constituent unit derived from a linear α-olefin having 2 to 20 carbon atoms, and satisfies the following requirements (Aa) to (Ad). The copolymer (A) preferably further satisfies the following requirement (Ae).

[0047] The copolymer (A) may contain only one type of copolymer or two or more types of copolymers. When the copolymer (A) contains two or more types of copolymers, it is preferred that each copolymer satisfies the above requirements (Aa) to (Ae).

[0048] "Essentials (Aa)"

[0049] In the copolymer (A), the amount of the constituent units derived from 4-methyl-1-pentene (U1) is 80.0 to 99.9 mol%, and the total amount of the constituent units derived from at least one selected from linear α-olefins having 2 to 20 carbon atoms (U2) is 20.0 to 0.1 mol%. U1 is preferably 85.0 to 99.9 mol%, more preferably 90.0 to 99.9 mol%. U2 is preferably 15.0 to 0.1 mol%, more preferably 10.0 to 0.1 mol%. The total of the above U1 and the above U2 is 100 mol%. It should be noted that the 100 mol% means the total of the above U1 and the above U2, and does not mean 100 mol% of all the constituent units constituting the copolymer (A).

[0050] As a straight-chain α-olefin having 2 to 20 carbon atoms, for example, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene can be cited. In this specification, ethylene is included in α-olefins. Among them, from the viewpoint of obtaining a film with a smaller surface roughness and a smoother surface from the resin composition of the present invention, a straight-chain α-olefin having 10 to 20 carbon atoms is preferred, and a straight-chain α-olefin having 10 to 18 carbon atoms is more preferred. Specifically, 1-decene, 1-tetradecene, 1-hexadecene, and 1-octadecene are preferred. For example, as a straight-chain α-olefin having 2 to 20 carbon atoms, 1-hexadecene and 1-octadecene are preferably used in combination.

[0051] The copolymer (A) may have only one type of structural unit derived from a linear α-olefin having 2 to 20 carbon atoms, or may have two or more types.

[0052] To the extent that the purpose of the present invention is not impaired, the copolymer (A) may further have constituent units derived from other polymerizable compounds other than 4-methyl-1-pentene and linear α-olefins having 2 to 20 carbon atoms. Examples of other polymerizable compounds include branched α-olefins having 20 or less carbon atoms other than 4-methyl-1-pentene; vinyl compounds having a cyclic structure such as styrene, vinyl cyclopentene, vinyl cyclohexane, and vinyl norbornane; vinyl esters such as vinyl acetate; unsaturated organic acids such as maleic anhydride or their derivatives; conjugated dienes such as butadiene, isoprene, pentadiene, and 2,3-dimethylbutadiene; 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl Non-conjugated polyenes such as -1,5-heptadiene, 7-methyl-1,6-octadiene, dicyclopentadiene, cyclohexadiene, dicyclooctadiene, methylene norbornene, 5-vinyl norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, and 2-propenyl-2,2-norbornadiene.

[0053] In the copolymer (A), the content of the constituent units derived from other polymerizable compounds is usually 10 mol% or less, preferably 5 mol% or less, more preferably 3 mol% or less in 100 mol% of all constituent units constituting the copolymer (A).

[0054] 《Requirements (Ab)》

[0055] Intrinsic viscosity [η] of copolymer (A) measured in decalin at 135°C A 0.5 to 5.0 dL / g. A It is preferably 0.5 to 4.5 dL / g, more preferably 0.5 to 4.0 dL / g.

[0056] [η] A The copolymer (A) within the above range shows good fluidity during the preparation and molding of the resin composition. In addition, it is considered that the copolymer (A) contributes to improving the stretchability when combined with the 4-methyl-1-pentene copolymer (B).

[0057] 《Requirements (Ac)》

[0058] When the copolymer (A) is measured by a cross-fractionation chromatography device (CFC) using an infrared spectrophotometer as a detection part, at least one peak of the eluted component amount exists in the range of 100 to 140° C. The peak of the eluted component amount preferably exists in the range of 100 to 135° C. It should be noted that the position of the peak of the eluted component amount is determined by the position of the peak top.

[0059] The copolymer (A) preferably has no peak of the amount of eluted components in the range of 0°C or higher and lower than 100°C.

[0060] The copolymer (A) satisfying the requirement (Ac) contains a component having high crystallinity, and the obtained molded product tends to show high heat resistance.

[0061] The content of the components eluted at 135° C. or higher in the total amount of components eluted at 0 to 145° C. of the copolymer (A) is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. The copolymer (A) satisfying this requirement is preferred from the viewpoint of uniform stretchability.

[0062] 《Requirements (Ad)》

[0063] When the copolymer (A) is measured by a cross-fractionation chromatography device (CFC) using an infrared spectrophotometer as a detection unit, the molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the eluted component in the range of 100 to 140° C., is 1.0 to 4.5. The Mw / Mn is preferably 1.5 to 4.5, more preferably 2.0 to 4.5. The average molecular weights are polystyrene-converted values ​​measured by gel permeation chromatography (GPC).

[0064] The resin composition containing the copolymer (A) having Mw / Mn in the above range tends to have a low content of relatively low molecular weight components. Therefore, the transparency of the molded body caused by the oozing out of the low molecular weight components is reduced, and the possibility of the low molecular weight components weakening the crystal structure is reduced. As a result, it is believed that the mechanical properties of the molded body are favorably affected.

[0065] The copolymer (A) having Mw / Mn within the above range can be obtained, for example, using a metallocene catalyst described later.

[0066] 《Requirements (Ae)》

[0067] The melting point (Tm) of the copolymer (A) measured by a differential scanning calorimeter (DSC) is preferably 210 to 260°C, more preferably 220 to 260°C, and further preferably 225 to 260°C.

[0068] The melting point tends to depend on the stereoregularity of the copolymer and the content of the structural unit derived from the linear α-olefin having 2 to 20 carbon atoms. The melting point can be adjusted by using a metallocene catalyst described later and controlling the content of the structural unit.

[0069] The copolymer (A) having a melting point within the above range is preferred from the viewpoint of heat resistance and moldability.

[0070] <4-Methyl-1-pentene copolymer (B)>

[0071] The 4-methyl-1-pentene copolymer (B) (hereinafter also referred to as "copolymer (B)") comprises a constituent unit derived from 4-methyl-1-pentene and a constituent unit derived from a linear α-olefin having 2 to 20 carbon atoms, and satisfies the following requirements (Ba) to (Bd). The copolymer (B) preferably further satisfies the following requirement (Be). The copolymer (B) preferably further satisfies the following requirement (Bf).

[0072] The copolymer (B) may contain only one type of copolymer or two or more types of copolymers. When the copolymer (B) contains two or more types of copolymers, each copolymer preferably satisfies the above requirements (Ba) to (Bf).

[0073] "Essentials (Ba)"

[0074] In the copolymer (B), the amount of the constituent units derived from 4-methyl-1-pentene (U3) is 20.0 to 98.0 mol%, and the total amount of the constituent units derived from at least one selected from linear α-olefins having 2 to 20 carbon atoms (U4) is 80.0 to 2.0 mol%. U3 is preferably 20.0 to 97.0 mol%, more preferably 25.0 to 97.0 mol%. U4 is preferably 80.0 to 3.0 mol%, more preferably 75.0 to 3.0 mol%. The total of the above-mentioned U3 and the above-mentioned U4 is set to 100 mol%. It should be noted that the meaning of 100 mol% is the total of the above-mentioned U3 and the above-mentioned U4, and does not refer to 100 mol% of all the constituent units constituting the copolymer (B).

[0075] As a linear α-olefin having 2 to 20 carbon atoms, for example, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene can be cited. Among them, from the viewpoint that the molded body obtained by the resin composition of the present invention can achieve higher stretching and can maintain high transparency after stretching, it is preferably a linear α-olefin having 10 to 20 carbon atoms, and more preferably a linear α-olefin having 10 to 18 carbon atoms. Specifically, 1-decene, 1-tetradecene, 1-hexadecene, and 1-octadecene are preferred. For example, as a linear α-olefin having 2 to 20 carbon atoms, it is preferred to use 1-hexadecene and 1-octadecene in combination.

[0076] The copolymer (B) may have only one type of structural unit derived from a linear α-olefin having 2 to 20 carbon atoms, or may have two or more types.

[0077] The copolymer (B) may further have a structural unit derived from other polymerizable compounds described in the copolymer (A) within a range not impairing the object of the present invention.

[0078] In the copolymer (B), the content of the constituent units derived from other polymerizable compounds is usually 10 mol% or less, preferably 5 mol% or less, more preferably 3 mol% or less in 100 mol% of all constituent units constituting the copolymer (B).

[0079] 《Requirements (Bb)》

[0080] Intrinsic viscosity [η] of copolymer (B) measured in decalin at 135°C B 2.0 to 8.0 dL / g. B It is preferably 2.5 to 7.5 dL / g, more preferably 2.7 to 7.0 dL / g, further preferably 3.0 to 7.0 dL / g, and particularly preferably 3.5 to 7.0 dL / g.

[0081] [η] B The copolymer (B) within the above range shows good fluidity during the preparation and molding of the resin composition. In addition, it is believed that further combination with the 4-methyl-1-pentene copolymer (A) helps to improve the stretchability. In particular, if [η] B When the content is not less than the above lower limit, the stretchability when formed into a film tends to be more excellent and the rigidity tends to be more excellent.

[0082] 《Requirement (Bc)》

[0083] When the copolymer (B) is measured by a cross-fractionation chromatography device (CFC) using an infrared spectrophotometer as a detection part, at least one peak of the eluted component amount exists in the range of 0° C. to less than 100° C. The peak of the eluted component amount preferably exists in the range of 0 to 80° C. It should be noted that the position of the peak of the eluted component amount is determined by the position of the peak top.

[0084] It is preferred that the copolymer (B) has no peak of the amount of eluted components in the range of 100 to 140°C.

[0085] The copolymer (B) satisfying the requirement (Bc) contains a component having lower crystallinity than the copolymer (A), and the obtained molded product tends to show high flexibility.

[0086] 《Requirements (Bd)》

[0087] When the copolymer (B) is measured by a cross-fractionation chromatography device (CFC) using an infrared spectrophotometer as a detection unit, the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the eluted component in the range of 0°C or more and less than 100°C, i.e., the molecular weight distribution (Mw / Mn) is 1.0 to 7.0. The Mw / Mn is preferably 1.0 to 6.5, more preferably 1.2 to 6.0. The average molecular weights are values ​​calculated in terms of styrene measured by gel permeation chromatography (GPC).

[0088] The resin composition containing the copolymer (B) having Mw / Mn in the above range tends to have a low content of relatively low molecular weight components. Therefore, the transparency of the molded body caused by the oozing out of the low molecular weight components is reduced, and the possibility of the low molecular weight components weakening the crystal structure is reduced. As a result, it is believed that the mechanical properties of the molded body are favorably affected.

[0089] The copolymer (B) having Mw / Mn within the above range can be obtained, for example, using a metallocene catalyst described later.

[0090] "Requirements (Be)"

[0091] When the copolymer (B) is measured by a cross fractionation chromatograph (CFC) using an infrared spectrophotometer as a detection unit, in one embodiment, the number average molecular weight (Mn) of the 0°C elution component is 5,000 or more, or no 0°C elution component exists.

[0092] The copolymer (B) containing the 0°C elution component in the aforementioned CFC contains a component with very low crystallinity (or completely amorphous). The copolymer (B) whose Mn of the 0°C elution component is 5000 or more is generally a high comonomer content with very low crystallinity. Such a polymer has low crystallinity but high molecular weight, and is therefore preferred from the viewpoint that it is not likely to cause a decrease in the transparency of the molded body caused by the bleeding of the low molecular weight component and roller contamination during film molding. Copolymers polymerized using a metallocene catalyst tend to have a larger Mn of the 0°C elution component or to have no 0°C elution component.

[0093] The Mn of the 0°C elution component in the copolymer (B) is preferably 15,000 or more, more preferably 20,000 or more. The upper limit of the Mn is not particularly limited, and may be, for example, 1,000,000. The content ratio of the 0°C elution component in the total elution component amount at 0 to 145°C of the copolymer (B) is not particularly limited, but is preferably 20% by mass or less, and more preferably 10% by mass or less.

[0094] 《Requirements (Bf)》

[0095] The melting point (Tm) of the copolymer (B) measured by differential scanning calorimetry (DSC) is preferably 220°C or less, or no peak indicating the melting point appears in the DSC measurement, more preferably 210°C or less, or no peak indicating the melting point appears in the DSC measurement, and further preferably 100 to 200°C, or no peak indicating the melting point appears in the DSC measurement.

[0096] The copolymer (B) satisfying the requirement (Bf) is preferred from the viewpoint of stretchability.

[0097] <Requirements (1)>

[0098] In the resin composition of the present invention, when the total content of the copolymers (A) and (B) is 100 parts by mass, the content of the copolymer (A) is 5 to 95 parts by mass, and the content of the copolymer (B) is 95 to 5 parts by mass.

[0099] When the content ratio of the copolymer (A) to (B) is within the above range, the obtained molded product tends to have a good balance between rigidity and ductility.

[0100] Furthermore, in the resin composition of the present invention, if the content of the copolymer (B) is greater than the content of the copolymer (A), it is preferred from the perspective of further improving the stretchability. Specifically, when the total content of the copolymer (A) and (B) is set to 100 parts by mass, the content of the copolymer (A) is preferably 5 parts by mass or more and less than 50 parts by mass, more preferably 10 to 40 parts by mass, further preferably 15 to 38 parts by mass, and particularly preferably 15 to 35 parts by mass; the content of the copolymer (B) is preferably greater than 50 parts by mass and less than 95 parts by mass, more preferably 60 to 90 parts by mass, further preferably 62 to 85 parts by mass, and particularly preferably 65 to 85 parts by mass.

[0101] <Requirements (2)>

[0102] In the resin composition of the present invention, the value (U4-U2) obtained by subtracting U2 (mol %) described in the requirement (Aa) from U4 (mol %) described in the requirement (Ba) is 0 mol % or more and 6.5 mol % or less.

[0103] That is, the comonomer content in the copolymer (A) and the copolymer (B) is not different, or the difference is small. By satisfying this requirement, the copolymer (A) and the copolymer (B) in the resin composition have good compatibility, and as a result, the surface roughness during film molding is small, and a smoother film is obtained.

[0104] The aforementioned difference (U4-U2) is preferably greater than 0 mol% and less than 5.5 mol%, more preferably greater than 0 mol% and less than 5.0 mol%, further preferably greater than 0 mol% and less than 4.5 mol%, particularly preferably greater than 0 mol% and less than 4.0 mol%.

[0105] The term "miscibility" in the present invention means the property of uniformly mixing components into one phase. It should be noted that "compatibility" refers to the property of dispersion of the sea phase and the island phase of the sea-island structure, which is different from miscibility.

[0106] The resin composition of the present invention has an intrinsic viscosity [η] measured in decalin at 135°C of usually 2.0 to 8.0 dL / g, preferably 2.5 to 7.0 dL / g, more preferably 2.8 to 6.0 dL / g, further preferably 3.0 to 5.0 dL / g, and particularly preferably 3.3 to 4.5 dL / g. If the intrinsic viscosity [η] is higher than 8.0 dL / g, the moldability tends to be poor, and if the intrinsic viscosity [η] is lower than 2.0 dL / g, the stretchability tends to be poor.

[0107] In the resin composition of the present invention, the content of the comonomer copolymerizable with 4-methyl-1-pentene contained in the resin composition is usually 1.0 to 6.0 mol%, preferably 1.5 to 5.5 mol%, more preferably 2.0 to 5.0 mol%, further preferably 2.5 to 5.0 mol%, particularly preferably 2.5 to 4.7 mol%, and most preferably 2.5 to 4.5 mol%. If the content of the comonomer is higher than 6.0 mol%, the dielectric breakdown strength tends to decrease, and if the content of the comonomer is lower than 1.0 mol%, the elongation tends to deteriorate.

[0108] It should be noted that the total of the above comonomer contents can be calculated as an average value of the contents of the comonomers copolymerized with 4-methyl-1-pentene in the copolymers (A) and (B) in consideration of the mass ratio. For example, the comonomer content of the composition of Example 1 can be calculated by the following formula.

[0109] Comonomer content=(1.4 mol%×35 mass%+4.6 mol%×75 mass%) / (35 mass%+75 mass%)=3.4 mol%.

[0110] When the resin composition of the present invention is measured by a cross-fractionation chromatograph (CFC) using an infrared spectrophotometer as a detection unit, it is preferred that at least one peak of the amount of eluted components exists in the range of 100 to 140°C, and at least one peak of the amount of eluted components exists in the range of 0°C to less than 100°C.

[0111] The melting point (Tm) of the resin composition of the present invention is usually 200 to 260° C., preferably 205 to 250° C., more preferably 210 to 240° C., and further preferably 215 to 230° C. The melting point (Tm) may be measured on the composition before being formed into a molded body, or may be measured on a molded body such as a film obtained only from the resin composition.

[0112] <Total content ratio of copolymer (A) and copolymer (B) in resin composition>

[0113] The total containing ratio of the copolymer (A) and copolymer (B) in the resin composition of the present invention is usually 50 mass % or more, preferably 60 mass % or more, more preferably 70 mass % or more. The upper limit of the containing ratio of copolymer (A) and copolymer (B) can be 100 mass % of resin composition. In the case where the aforementioned resin composition contains other components (for example, other polymer components, additives described later), the aforementioned upper limit is defined by the containing ratio of other components.

[0114] The resin composition of the present invention may contain one or more copolymers (A). In addition, the resin composition of the present invention may contain one or more copolymers (B).

[0115] Copolymer (A) is a relatively low and hard component of intrinsic viscosity [η] compared with copolymer (B), and copolymer (B) is a relatively soft component. It can be considered that the hardness of each polymer is attributed to the content of the comonomer contained in each polymer. The resin composition of the present invention contains these copolymers (A) and copolymer (B), so the molded body obtained by the resin composition maintains the transparency and heat resistance derived from 4-methyl-1-pentene copolymer, and excellent in stretchability. Therefore, the resin composition of the present invention is suitable for manufacturing a capacitor film requiring heat resistance and stretchability.

[0116] <Method for producing copolymers (A) and (B)>

[0117] Copolymer (A) and copolymer (B) can be obtained, for example, by polymerizing 4-methyl-1-pentene, a linear α-olefin having 2 to 20 carbon atoms, and, if necessary, the above-mentioned other polymerizable compound. By carrying out the above-mentioned polymerization in the presence of a metallocene catalyst, copolymers (A) and (B) satisfying the above-mentioned requirements can be suitably obtained.

[0118] Examples of the metallocene catalyst include metallocene catalysts described in International Publication No. 01 / 53369, International Publication No. 01 / 27124, Japanese Patent Application Publication No. 3-193796, Japanese Patent Application Publication No. 02-41303, International Publication No. 06 / 025540, and International Publication No. 2013 / 099876.

[0119] Examples of the metallocene catalyst include a catalyst composed of at least a metallocene compound (a) and a carrier (b).

[0120] 《Metallocene compound (a)》

[0121] The metallocene compound (a) is represented by, for example, the general formula (1) or (2).

[0122] [Chemistry 1]

[0123]

[0124] The meanings of the symbols in the general formula (1) or (2) are as follows.

[0125] R 1 ~R 14 Each is independently a hydrogen atom, a hydrocarbon group, a substituted hydrocarbon group or a silicon-containing group. 1 To R 4 Adjacent substituents may be combined with each other to form a ring. 5 To R 12 Adjacent substituents may be bonded to each other to form a ring.

[0126] Y is a carbon atom or a silicon atom.

[0127] A is a divalent hydrocarbon group having 2 to 20 carbon atoms which may contain an unsaturated bond and / or an aromatic ring. A may have two or more ring structures including the ring formed together with Y.

[0128] M is a metal (transition metal) selected from Group 4 of the periodic table, and examples thereof include titanium, zirconium, and hafnium.

[0129] Q is a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an anionic ligand, or a neutral ligand capable of coordinating with a lone electron pair. When j is 2 or more, each Q may be the same or different.

[0130] j is an integer of 1 to 4, and preferably 2.

[0131] As R 1 ~R 14 The hydrocarbon group in includes, for example, a hydrocarbon group having 1 to 20 carbon atoms, specifically, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, an arylalkyl group having 7 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an alkylaryl group having 7 to 20 carbon atoms.

[0132] R 1 ~R 14The substituted hydrocarbon group (excluding silicon-containing groups) is a group in which a part or all of the hydrogen atoms contained in the aforementioned hydrocarbon group are substituted by functional groups such as halogen atoms (fluorine, chlorine, bromine, iodine), hydroxyl groups and amino groups.

[0133] As R 1 ~R 14 Examples of the silicon-containing group include an alkylsilyl group or an arylsilyl group having 1 to 4 silicon atoms and 3 to 20 carbon atoms. Specific examples thereof include a trimethylsilyl group, a tert-butyldimethylsilyl group, and a triphenylsilyl group.

[0134] R on the fluorene ring 5 To R 12 Adjacent substituents may be bonded to each other to form a ring. Examples of such substituted fluorenyl groups include benzofluorenyl, dibenzofluorenyl, octahydrodibenzofluorenyl, and octamethyloctahydrodibenzofluorenyl.

[0135] R on the fluorene ring 5 To R 12 The substituents are preferably bilaterally symmetrical from the perspective of ease of synthesis, that is, R 5 =R 12 , R 6 =R 11 , R 7 =R 10 , R 8 =R 9 The fluorene ring part is preferably unsubstituted fluorene, 3,6-disubstituted fluorene, 2,7-disubstituted fluorene or 2,3,6,7-tetrasubstituted fluorene. The 3-position, 6-position, 2-position and 7-position of the fluorene ring are respectively connected to R 7 , R 10 , R 6 , R 11 Corresponding.

[0136] R 13 and R 14 Each independently is preferably a hydrogen atom, a hydrocarbon group or a substituted hydrocarbon group.

[0137] In the case of general formula (1), R 13 and R 14 It combines with Y to form a substituted methylene group or a substituted silylene group as a crosslinking portion. Specific examples of the substituted methylene group and the substituted silylene group include, for example, dialkylmethylene groups, dicycloalkylmethylene groups, alkylcycloalkylmethylene groups, alkylarylmethylene groups, diarylmethylene groups, dialkylsilylene groups, dicycloalkylsilylene groups, alkylcycloalkylsilylene groups, alkylarylsilylene groups, diarylsilylene groups, and halogenated groups thereof.

[0138] In the case of general formula (2), Y is combined with the aforementioned divalent hydrocarbon group A to form a cycloalkylene group or a cyclomethylenesilyl group. Specific examples of the cycloalkylene group and the cyclomethylenesilyl group include, for example, a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a cycloheptylene group, a bicyclo[3.3.1]nonylene group, a norbornylene group, an adamantylene group, a tetrahydronaphthylene group, an indanylene group, a cyclodimethylenesilylene group, a cyclotrimethylenesilylene group, a cyclotetramethylenesilylene group, a cyclopentamethylenesilylene group, a cyclohexamethylenesilylene group, and a cycloheptamethylenesilylene group.

[0139] In Q, the halogen atom includes fluorine, chlorine, bromine and iodine; the hydrocarbon group having 1 to 20 carbon atoms includes 1 ~R 14 As anionic ligands, alkoxy groups, aryloxy groups, carboxylate groups, sulfonate groups, etc. can be mentioned; as neutral ligands that can coordinate with lone electron pairs, organic phosphorus compounds such as trimethylphosphine, triethylphosphine, triphenylphosphine, diphenylmethylphosphine, tetrahydrofuran, diethyl ether, diphenylphosphine, etc. can be mentioned. Alkanes, ethers such as 1,2-dimethoxyethane, etc. Preferably, at least one of Q is a halogen atom or an alkyl group having 1 to 20 carbon atoms.

[0140] Specific examples of the metallocene compound (a) include compounds exemplified in International Publication No. 01 / 27124, International Publication No. 2006 / 025540, and International Publication No. 2007 / 308607.

[0141] The metallocene compound (a) is particularly preferably a compound represented by the general formula [A2] described in International Publication No. 2014 / 050817 or the like.

[0142] [Chemistry 2]

[0143]

[0144] In formula [A2], R 1b is a hydrocarbon group, a silicon-containing group or a halogen-containing hydrocarbon group, R 2b ~R 12b The substituents are selected from hydrogen atoms, hydrocarbon groups, silicon-containing groups, halogen atoms and halogen-containing hydrocarbon groups, each of which may be the same or different, and each substituent may be combined with each other to form a ring. M is a transition metal of Group 4 of the periodic table, n is an integer of 1 to 3, Q is synonymous with Q in the above general formula (1) or (2), and j is an integer of 1 to 4.

[0145] As R 1b To R 12bThe hydrocarbon group in the group includes, for example, straight-chain hydrocarbon groups such as straight-chain alkyl and straight-chain alkenyl; branched hydrocarbon groups such as branched alkyl; cyclic saturated hydrocarbon groups such as cycloalkyl, norbornyl, and adamantyl; cyclic unsaturated hydrocarbon groups such as aryl and cycloalkenyl; and groups in which one or more hydrogen atoms possessed by saturated hydrocarbon groups such as aralkyl are replaced by cyclic unsaturated hydrocarbon groups. The number of carbon atoms in the hydrocarbon group is usually 1 to 20, preferably 1 to 15, and more preferably 1 to 10.

[0146] As R 1b To R 12b The silicon-containing group in the formula is, for example, a group represented by the formula -SiR3 (wherein a plurality of Rs are each independently an alkyl group having 1 to 15 carbon atoms or a phenyl group).

[0147] As R 1b To R 12b Examples of the halogen-containing hydrocarbon group include groups in which one or two or more hydrogen atoms possessed by the above hydrocarbon groups such as trifluoromethyl are substituted with halogen atoms.

[0148] As R 2b To R 12b Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0149] As the ring (spiro ring, addition ring) formed by two substituents mutually combining in formula [A2], for example, alicyclic ring and aromatic ring can be mentioned. Specifically, cyclohexane ring, benzene ring, hydrogenated benzene ring and cyclopentene ring can be mentioned, preferably cyclohexane ring, benzene ring and hydrogenated benzene ring. In addition, in such a ring structure, substituents such as alkyl can be further provided on the ring.

[0150] R 1b Particularly preferably, the carbon having a free valence (the carbon bonded to the cyclopentadienyl ring) is a tertiary carbon substituent. 1b , specifically tert-butyl, tert-pentyl, 1-methylcyclohexyl, and 1-adamantyl.

[0151] The fluorene ring portion is not particularly limited as long as it is a structure derived from a known fluorene derivative. From the viewpoint of molecular weight, R 4b and R 5b Preferred is a hydrogen atom.

[0152] R 2b , R 3b , R 6b and R 7b It is preferably a hydrocarbon group having 1 to 20 carbon atoms. 2b With R 3b can combine with each other to form a ring, and R 6b With R 7bThey may also be combined to form a ring. Examples of such substituted fluorenyl groups include benzofluorenyl, dibenzofluorenyl, octahydrodibenzofluorenyl, 1,1,4,4,7,7,10,10-octamethyl-2,3,4,7,8,9,10,12-octahydro-1H-dibenzo[b,h]fluorenyl, 1,1,3,3,6,6,8,8-octamethyl-2,3,6,7,8,10-hexahydro-1H-dicyclopenta[b,h]fluorenyl, and 1',1',3',6',8',8'-hexamethyl-1'H,8'H-dicyclopenta[b,h]fluorenyl.

[0153] R 8b Preferably it is a hydrogen atom. 9b It is preferably an alkyl group having 2 or more carbon atoms. 10b and R 11b A hydrogen atom is also preferred.

[0154] Alternatively, when n=1, R is more preferably 9b With R 10b They are combined to form a ring, and the ring is particularly preferably a 6-membered ring such as a cyclohexane ring. 11b Preferred is a hydrogen atom.

[0155] R 12b An alkyl group is preferred.

[0156] M is a transition metal of Group 4 of the periodic table, such as Ti, Zr or Hf, preferably Zr or Hf, and particularly preferably Zr.

[0157] n is an integer of 1 to 3, preferably 1 or 2, and more preferably 1. When n is the above value, it is preferred from the viewpoint of efficiently obtaining the produced polymer.

[0158] j is an integer of 1 to 4, and preferably 2.

[0159] As the compound represented by the general formula [A2], (8-octamethylfluorene-12'-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride or (8-(2,3,6,7-tetramethylfluorene)-12'-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride is particularly preferred. Here, the above-mentioned octamethylfluorene refers to 1,1,4,4,7,7,10,10-octamethyl-2,3,4,7,8,9,10,12-octahydro-1H-dibenzo[b,h]fluorene.

[0160] 《Carrier (b)》

[0161] The support (b) is preferably in the form of particles, and the metallocene compound (a) is fixed on the surface and inside of the support to form the metallocene catalyst. Such a catalyst is generally called a metallocene-supported catalyst.

[0162] The support (b) contains, as a main component, an organoaluminum compound (b-1), an organoboron compound (b-2), an inorganic compound (b-3), or a complex of two or more selected from these.

[0163] As the organoaluminum compound (b-1), for example, trialkylaluminums such as trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-octylaluminum, dialkylaluminum hydrides such as diisobutylaluminum hydride, tricycloalkylaluminum, and organoaluminumoxy compounds represented by aluminoxanes can be cited. In addition, as the organoaluminum compound (b-1), for example, organoaluminumoxy compounds containing boron atoms, halogen-containing aluminoxanes such as those exemplified in International Publication Nos. 2005 / 066191 and 2007 / 131010, and ionic aluminoxanes such as those exemplified in International Publication No. 2003 / 082879 can also be cited.

[0164] Examples of the organic boron compound (b-2) include trialkylammonium tetraarylborate, trialkylammonium tetra(halogenated aryl)borate, dioctadecylmethylammonium tetra(halogenated aryl)borate, dioctadecylmethylammonium tetra(halogenated aryl)borate, N,N-dialkylanilinium tetra(aryl)borate, and N,N-dialkylanilinium tetra(halogenated aryl)borate.

[0165] As the inorganic compound (b-3), for example, porous oxides, inorganic halides, clay, clay minerals or ion-exchange layered compounds can be cited. As porous oxides, for example, oxides such as SiO2, Al2O3, MgO, ZrO2, TiO2, B2O3, CaO, ZnO, BaO, ThO2, or a complex or mixture containing them can be cited. For example, natural or synthetic zeolites, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-V2O5, SiO2-Cr2O3, SiO2-TiO2-MgO, etc. can be exemplified. As inorganic halides, for example, MgCl2, MgBr2, MnCl2, MnBr2 can be cited. The inorganic halide can be used directly or after being crushed by a ball mill or a vibration mill. Alternatively, an inorganic halide may be used which is dissolved in a solvent such as alcohol and then precipitated into fine particles using a precipitating agent.

[0166] As the support (b), from the viewpoint of high activity and further suppressing the amount of solvent-soluble part, a support containing aluminum atoms is preferred. The content of aluminum atoms in the support (b) is preferably 20% by mass or more, more preferably 20 to 60% by mass, further preferably 30 to 50% by mass, and particularly preferably 35 to 47% by mass.

[0167] As such a carrier (b), solid aluminoxane is suitably used, and for example, solid aluminoxane disclosed in International Publication No. 2010 / 055652, International Publication No. 2013 / 146337, or International Publication No. 2014 / 123212 is particularly suitably used.

[0168] The term "solid" means that the aluminoxane substantially maintains a solid state under a reaction environment in which the solid aluminoxane is used. More specifically, it means that, for example, when the components constituting the olefin polymerization catalyst are brought into contact to prepare the olefin polymerization solid catalyst component, the aluminoxane is in a solid state under a specific temperature and pressure environment in an inert hydrocarbon medium such as hexane or toluene used in the reaction.

[0169] The solid aluminoxane preferably contains an aluminoxane having at least one structural unit selected from the structural unit represented by the following formula (1) and the structural unit represented by the following formula (2), more preferably contains an aluminoxane having a structural unit represented by the following formula (1), and further preferably contains a polymethylaluminoxane composed only of the structural unit represented by the following formula (1).

[0170] [Chemistry 3]

[0171]

[0172] In the formula (1), Me is a methyl group.

[0173] In formula (2), R 1 It is a hydrocarbon group having 2 to 20 carbon atoms, preferably a hydrocarbon group having 2 to 15 carbon atoms, and more preferably a hydrocarbon group having 2 to 10 carbon atoms. Examples of the hydrocarbon group include an alkyl group, a cycloalkyl group, and an aryl group.

[0174] The structure of solid aluminoxane is not necessarily clear, but it is generally estimated that the structural unit represented by formula (1) and / or formula (2) is repeated about 2 to 50 times, but it is not limited to this structure. In addition, the bonding state of its structural units is various, such as linear, cyclic or clustered, and it is estimated that aluminoxane is usually composed of one of them or a mixture thereof. In addition, aluminoxane may be composed only of the structural unit represented by formula (1) or formula (2).

[0175] The solid aluminoxane is preferably solid polymethylaluminoxane, and more preferably solid polymethylaluminoxane consisting only of the structural unit represented by formula (1).

[0176] Solid aluminoxane functions as a catalyst carrier. Therefore, in addition to solid aluminoxane, it is not necessary to use solid inorganic carriers such as silica, alumina, silica-alumina, magnesium chloride, or solid organic carriers such as polystyrene beads as catalyst carriers.

[0177] Solid aluminoxane can be produced by the methods described in, for example, International Publication Nos. 2010 / 055652 and 2014 / 123212.

[0178] 《Organic compound component (c)》

[0179] The metallocene catalyst may further contain an organic compound component (c) as required. The organic compound component (c) is used as required for the purpose of improving polymerization performance and the physical properties of the generated polymer. As the organic compound component (c), the aforementioned organoaluminum compound (b-1) can be used. In addition, for example, alcohols, phenolic compounds, carboxylic acids, phosphorus compounds, amides, polyethers and sulfonates can be cited.

[0180] 《Aggregation Conditions》

[0181] The polymerization of 4-methyl-1-pentene and a linear α-olefin having 2 to 20 carbon atoms for obtaining copolymers (A) and (B) can be carried out in any of liquid phase polymerization methods such as solution polymerization and suspension polymerization or gas phase polymerization methods. In the liquid phase polymerization method, an inactive hydrocarbon solvent can be used, specifically, aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, kerosene, etc.; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, methylcyclohexane, etc.; aromatic hydrocarbons such as benzene, toluene, xylene, etc.; halogenated hydrocarbons such as vinyl chloride, chlorobenzene, dichloromethane, trichloromethane, tetrachloromethane, etc.; a mixed solvent of two or more selected from them. In addition, the olefin containing 4-methyl-1-pentene itself can be used as a polymerization solvent.

[0182] In the olefin polymerization, the method of using each component and the order of adding are arbitrarily selected, and the following methods can be exemplified. Hereinafter, the metallocene compound (a), the support (b) and the organic compound component (c) are also referred to as "components (a) to (c)", respectively.

[0183] (i) A method of adding the components (a) and (b) to a polymerization reactor in an arbitrary order.

[0184] (ii) A method of adding a catalyst component in which the component (a) is supported on the component (b) to a polymerization reactor.

[0185] In each of the above methods (i) to (ii), the component (c) may be further added at an arbitrary stage. In addition, at least two of the catalyst components may be contacted in advance.

[0186] In the solid catalyst component in which component (a) is supported on component (b), olefins such as 4-methyl-1-pentene and 3-methyl-1-pentene may be prepolymerized, and a catalyst component may be further supported on the prepolymerized solid catalyst component.

[0187] When olefin polymerization is performed using a metallocene catalyst, the amount of each component constituting the metallocene catalyst may be as follows: In addition, the content of each component in the metallocene catalyst may be adjusted as follows.

[0188] Component (a) can be used in an amount of usually 10 -10 ~10 -2 mole, preferably 10 -8 ~10 -3 mol. Component (b-1) can be used in an amount such that the molar ratio of aluminum atoms in component (b-1) to all transition metal atoms (M) in component (a) [Al / M] is usually 10 to 10,000, preferably 30 to 2,000, and particularly preferably 150 to 500. Component (b-2) can be used in an amount such that the molar ratio of component (b-2) to all transition metal atoms (M) in component (a) [(b-2) / M] is usually 10 to 10,000, preferably 30 to 2,000, and further preferably 150 to 500. Component (b-3) can be used in an amount such that the molar ratio of component (b-3) to all transition metal atoms (M) in component (a) [(b-3) / M] is usually 10 to 10,000, preferably 30 to 2,000, and further preferably 150 to 500.

[0189] When component (c) is used, when component (b) is component (b-1), it can be used in an amount such that the molar ratio of aluminum atoms in component (b-1) to component (c) [Al / (c)] is usually 0.002 to 500, preferably 0.01 to 60. When component (b) is component (b-2), it can be used in an amount such that the molar ratio of component (b-2) to component (c) [(b-2) / (c)] is usually 0.002 to 500, preferably 0.01 to 60. When component (b) is component (b-3), it can be used in an amount such that the molar ratio of component (b-3) to component (c) [(b-3) / (c)] is usually 0.002 to 500, preferably 0.01 to 60.

[0190] The polymerization temperature is usually -50 to 200°C, preferably 0 to 100°C, and more preferably 20 to 100°C. The polymerization pressure is usually normal pressure to 10 MPa gauge pressure, preferably normal pressure to 5 MPa gauge pressure. The polymerization reaction can be carried out by any method of intermittent, semi-continuous and continuous methods. For the purpose of controlling the molecular weight or polymerization activity of the generated polymer, hydrogen can be added to the polymerization system. The amount of hydrogen added is preferably about 0.001 to 100 NL per 1 kg of olefin.

[0191] As polymerization conditions, multi-step polymerization in which two or more polymerization steps are performed under different reaction conditions may be adopted. For example, by performing polymerization stepwise under two conditions in which the amount of hydrogen used or the ratio of 4-methyl-1-pentene to a linear α-olefin having 2 to 20 carbon atoms is different, a polymer having a desired molecular weight distribution or composition distribution can be obtained.

[0192] For example, the mixture of copolymers (A) and (B) can be produced by a multi-step polymerization method comprising a step (1) in which the 4-methyl-1-pentene copolymer (A) is produced by slurry polymerization, and a step (2) in which the 4-methyl-1-pentene copolymer (B) is produced by slurry polymerization in the presence of the copolymer (A) obtained in the step (1) so that the amount of the copolymer (B) is in the range of 5 to 90 parts by mass based on 100 parts by mass of the total amount of the copolymers (A) and (B).

[0193] The multi-step polymerization method has steps (1) and (2) with different polymerization conditions. It may be a two-step polymerization of steps (1) and (2), or a three-step polymerization including other steps in addition to steps (1) and (2).

[0194] 《Process (1)》

[0195] In step (1), 4-methyl-1-pentene copolymer (A) is produced by slurry polymerization. In step (1), the feed ratio of 4-methyl-1-pentene to the linear α-olefin having 2 to 20 carbon atoms is set so that the amount of the constituent units derived from each is within the above range.

[0196] In step (1), a slurry containing the copolymer (A) is obtained. The slurry concentration, that is, the concentration of the copolymer (A) particles is usually 0.015 to 45% by mass, preferably 0.03 to 35% by mass.

[0197] 《Process (2)》

[0198] In step (2), a 4-methyl-1-pentene copolymer (B) is produced by slurry polymerization in the presence of the copolymer (A) obtained in step (1). In step (2), the feed ratio of 4-methyl-1-pentene to the linear α-olefin having 2 to 20 carbon atoms is set so that the amount of the constituent units derived from each is within the above range.

[0199] In step (2), the copolymer (B) is produced so that the amount of the copolymer (B) is in the range of 5 to 90 parts by mass, based on 100 parts by mass of the total amount of the copolymer (A) obtained in step (1) and the copolymer (B) obtained in step (2).

[0200] In step (2), in one embodiment, 4-methyl-1-pentene and a linear α-olefin having 2 to 20 carbon atoms may be added to a slurry containing the copolymer (A) to perform slurry polymerization of these monomers.

[0201] In step (2), a slurry containing particles containing the copolymer (A) and the copolymer (B) is obtained. The slurry concentration, that is, the particle concentration is usually 3 to 50% by mass, preferably 5 to 40% by mass.

[0202] The multi-step polymerization method uses slurry polymerization. The so-called "slurry polymerization" refers to a polymerization having the following characteristics: the polymer produced by the polymerization is substantially not dissolved in the medium used in the polymerization, but exists in the form of, for example, fine particles dispersed in the medium.

[0203] 《Solid-Liquid Separation Process》

[0204] The particles can be separated and recovered by subjecting the slurry containing the 4-methyl-1-pentene polymer particles containing the copolymers (A) and (B) obtained in step (2) to solid-liquid separation, for example, filtration.

[0205] Post-processing process

[0206] The 4-methyl-1-pentene polymer particles obtained in the above-mentioned multi-step polymerization method, for example, the particles obtained in the above-mentioned solid-liquid separation step, can be subjected to a known post-treatment step such as a catalyst deactivation treatment step, a catalyst residue removal step, a drying step, etc. after being produced by the above-mentioned method, as needed.

[0207] Through the above operation, a mixture of copolymers (A) and (B) can be obtained.

[0208] <Other polymer components>

[0209] The resin composition of the present embodiment may further contain other polymer components other than the copolymers (A) and (B). Examples of other polymer components include α-olefin polymers (E) (excluding the copolymers (A) and (B) above) and elastomers other than these.

[0210] The α-olefin polymer (E) is, for example, a polymer of an α-olefin having 2 to 20 carbon atoms (excluding the above-mentioned copolymers (A) and (B)), and examples thereof include homopolymers or copolymers of an α-olefin having 2 to 20 carbon atoms.

[0211] Examples of the α-olefin having 2 to 20 carbon atoms include linear α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene; and branched α-olefins such as isobutylene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4,4-dimethyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4-ethyl-1-hexene, and 3-ethyl-1-hexene. Among these, α-olefins having 15 or less carbon atoms are preferred, and α-olefins having 10 or less carbon atoms are more preferred.

[0212] The α-olefin polymer (E) may further have a structural unit derived from other polymerizable compounds described in the copolymer (A) within a range not impairing the purpose of the present invention.

[0213] In the α-olefin polymer (E), the content of the constituent units derived from other polymerizable compounds is usually 10 mol% or less, preferably 5 mol% or less, more preferably 3 mol% or less, based on 100 mol% of all the constituent units constituting (E).

[0214] Specific examples of the α-olefin polymer (E) include low-density polyethylene, high-density polyethylene, ethylene-propylene random copolymers, ethylene-1-butene random copolymers, ethylene-propylene-1-butene random copolymers, ethylene-1-hexene random copolymers, ethylene-1-octene random copolymers, ethylene-propylene-ethylidene norbornene random copolymers, ethylene-propylene-1-butene-ethylidene norbornene random copolymers, ethylene-1-butene-1-octene random copolymers and other ethylene copolymers; propylene homopolymers, propylene-1-butene random copolymers, propylene-1-hexene random copolymers, propylene-1-octene random copolymers and other propylene copolymers; 1-butene homopolymers, 1-butene-1-hexene random copolymers, 1-butene-1-octene random copolymers and other butene copolymers; and 4-methyl-1-pentene homopolymers, 4-methyl-1-pentene-1-hexene copolymers and other 4-methyl-1-pentene copolymers. Among them, from the viewpoint of compatibility, 4-methyl-1-pentene homopolymer and 4-methyl-1-pentene copolymer are preferred.

[0215] Intrinsic viscosity [η] of the α-olefin polymer (E) measured in decalin at 135°C E It is usually 0.1 to 10 dL / g, preferably 0.5 to 5 dL / g.

[0216] The melting point (Tm) of the α-olefin polymer (E) measured by differential scanning calorimetry (DSC) is not particularly limited, but is preferably 60° C. or higher, more preferably 70 to 300° C., from the perspective of heat resistance and strength.

[0217] The α-olefin polymer (E) can be produced by a conventionally known method using, for example, a vanadium-based catalyst, a titanium-based catalyst, or a metallocene-based catalyst.

[0218] The resin composition of the present embodiment may contain one or two or more α-olefin polymers (E).

[0219] The content of the α-olefin polymer (E) in the resin composition of the present embodiment is usually 50 parts by mass or less, preferably 40 parts by mass or less, based on 100 parts by mass of the total content of the copolymers (A) and (B).

[0220] In one embodiment, when the resin composition of the present embodiment contains a large amount of 4-methyl-1-pentene homopolymer, the strength of the obtained molded product can be improved, but the tensile property sometimes deteriorates. Therefore, the content ratio of the 4-methyl-1-pentene homopolymer in the resin composition of the present embodiment is preferably 30% by mass or less, more preferably 25% by mass or less, and further preferably 20% by mass or less.

[0221] <Additives>

[0222] The resin composition of the present invention may contain conventionally known additives.

[0223] As additives, for example, auxiliary antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, anti-blocking agents, anti-fogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, fillers, hydrochloric acid absorbents can be cited. The content of the additives is not particularly limited, and is generally 0 to 50 parts by mass, preferably 0 to 10 parts by mass, relative to 100 parts by mass of the polymer components including copolymers (A) and (B).

[0224] The resin composition of the present invention may contain one or more additives.

[0225] [Method for producing resin composition]

[0226] The method for producing the resin composition of the present invention will be described.

[0227] The resin composition of the present invention can be obtained, for example, by mixing the above-mentioned copolymer (A) and copolymer (B) and, if necessary, other polymer components and additives. A mixture of copolymers (A) and (B) can also be obtained by the above-mentioned multi-step polymerization method.

[0228] The components may be mixed by various known methods, for example, a method of mixing the components using a plastomill, a Henschel mixer, a V-blender, a belt blender, a drum, a blender, a kneader-Ruder or the like; a method of further melt-kneading the resulting mixture using a single-screw extruder, a twin-screw extruder, a kneader, a Banbury mixer or the like, and then granulating or pulverizing the resulting molten mixture.

[0229] In the resin composition of the present invention, when measured by cross-fractionation chromatography (CFC) using an infrared spectrophotometer by the detection unit, from the viewpoint of improving the stretchability of the obtained molded product, the amount of eluted components in the range of 135°C or more is preferably 20% by mass or less, more preferably 15% by mass or less, and further preferably 10% by mass or less relative to the total amount of eluted components at 0 to 145°C of the resin composition. The eluted components in the range of 135°C or more usually correspond to 4-methyl-1-pentene homopolymers.

[0230] [Molding body]

[0231] The molded body of the present invention comprises the resin composition of the present invention and can be obtained by known thermoforming methods such as extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, stamping molding, vacuum molding, calendering molding, filament molding, foaming molding, powder coating and the like.

[0232] The molded product of the present invention may be a molded product obtained by further processing a primary molded product obtained by a method such as extrusion molding, injection molding, solution casting, etc., by a method such as blow molding, stretching, etc.

[0233] The molded body of the present invention is preferably a film. In addition to the properties of the conventional 4-methyl-1-pentene copolymer such as heat resistance, mechanical properties, electrical properties (dielectric breakdown strength, etc.), and demolding properties, the film of the present invention has a small surface roughness, is smooth, and has excellent stretchability and flexibility. The film of the present invention comprises the resin composition of the present invention, and can be obtained by, for example, melt molding in the range of 180 to 300°C. The thickness of the film of the present invention is usually 1000 μm or less, preferably 100 μm or less, more preferably 50 μm or less, more preferably 30 μm or less, and particularly preferably 15 μm or less. The lower limit of the thickness of the film of the present invention is not particularly limited, and is usually 1 μm.

[0234] The film surface roughness (Ra) of the film of the present invention is preferably less than 100 nm, more preferably 60 nm or less, and further preferably 40 nm or less. Since the film of the present invention is preferably smoother, the lower limit of the film surface roughness (Ra) is not particularly limited, but is preferably close to 0.

[0235] The film surface roughness (Rz) of the film of the present invention is preferably less than 500 nm, more preferably 400 nm or less, and further preferably 300 nm or less. Since the film of the present invention is preferably smoother, the lower limit of the film surface roughness (Rz) is not particularly limited, but is preferably close to 0.

[0236] The film of the present invention contains at least two types of 4-methyl-1-pentene copolymers such as the above-mentioned 4-methyl-1-pentene copolymer (A) and 4-methyl-1-pentene copolymer (B).

[0237] That is, examples of the film of the present invention include films satisfying the following requirements (I) to (III).

[0238] (I) Contains at least two 4-methyl-1-pentene copolymers.

[0239] (II) The film surface roughness (Ra) is less than 100 nm.

[0240] (III) The film surface roughness (Rz) is less than 500 nm.

[0241] The film of the present invention, for example, in addition to the monolayer film obtained from the resin composition of the present invention, can also be a laminated film having a layer obtained from the resin composition of the present invention. As a method for obtaining a laminated film, for example, there can be cited: a method of laminating other layers on a surface layer film previously obtained by T-die molding or inflation molding by a known lamination method such as extrusion lamination, extrusion coating, etc.; a method of laminating each film by dry lamination after independently molding a plurality of films; a co-extrusion molding method in which a plurality of components are supplied to a multilayer extruder for molding. The aforementioned surface film layer is, for example, a layer obtained from the resin composition of the present invention.

[0242] Examples of uses of the film of the present invention include:

[0243] Stretched films: for example, films for capacitors;

[0244] Semiconductor engineering films: for example, dicing tapes, back grinding tapes, chip bonding films, films for polarizing plates;

[0245] Packaging films: for example, food packaging films, stretch films, cling films, breathable films, shrink films, and easy-to-peel films;

[0246] Diaphragms: for example, battery separators, separators for lithium-ion batteries, electrolyte membranes for fuel cells, and adhesive / bonding material separators;

[0247] Films for electronic components: for example, diffusion films, reflection films, radiation-resistant films, gamma-ray-resistant films, and porous films;

[0248] Release film: for example, release film for flexible printed circuit boards, ACM substrates, rigid-flexible substrates, advanced composite materials, carbon fiber composite curing, glass fiber composite curing, aramid fiber composite curing, nanocomposite curing, filler curing, urethane curing, epoxy curing, semiconductor sealing, polarizing plates, diffusers, prisms, reflectors, fuel cells or various rubber sheets;

[0249] Surface protection films: for example, protective films and masking films for polarizing plates, liquid crystal panels, optical components, lenses, electrical components / electronic products, mobile phones, personal computers or touch panels;

[0250] Building material films: for example, window films for building materials, films for laminated glass, bulletproof materials, films for bulletproof glass, heat insulation sheets, heat insulation films.

[0251] The film of the present invention is preferably a stretched film, for example, preferably a stretched film obtained by forming the resin composition of the present invention into a film or sheet by T-die extrusion molding or the like to obtain a primary molded body, and further uniaxially stretching or biaxially stretching the obtained primary molded body to obtain a stretched film. The stretching ratio in the MD direction and the TD direction can be 1.05 to 20 times independently.

[0252] As the specific use of the stretched film, a capacitor film can be cited. For the capacitor film, sometimes it is necessary to stretch the film and orient the film to increase the strength. By using the resin composition of the present invention, a capacitor film with excellent film processability and high strength can be obtained. In addition, the capacitor film using the resin composition of the present invention has a small surface roughness and excellent smoothness, and has a tendency to maintain transparency even after stretching.

[0253] [Capacitor film]

[0254] The thickness of the capacitor film of the present invention is preferably 1 to 20 μm, more preferably 2 to 15 μm, and even more preferably 2.5 to 10 μm.

[0255] The ratio of the dielectric breakdown strength V(23°C) at 23°C to the dielectric breakdown strength V(120°C) at 120°C of the capacitor film of the present invention, V(120°C) / V(23°C), is preferably 0.50 or more, more preferably 0.55 or more, and further preferably 0.60 or more. In this way, the electrical characteristics are stable when voltage is applied for a long time, and it is useful as a capacitor. The higher the upper limit of the above ratio, the better the electrical characteristics, and in one embodiment, it can be 0.95.

[0256] The dielectric breakdown strength V(120°C) of the capacitor film of the present invention at 120°C is preferably 200 kV / mm or more, more preferably 250 kV / mm or more. The upper limit of the dielectric breakdown strength V(120°C) is not particularly limited, and in one embodiment, may be 700 kV / mm.

[0257] The details of the measurement conditions of the above physical properties are described in the Example column.

[0258] [Method for producing capacitor film]

[0259] The capacitor film of the present invention is obtained by biaxially stretching a film composed of the above-mentioned resin composition. More specifically, the capacitor film is produced by using the above-mentioned resin composition, forming a film by T-die extrusion molding at a temperature of 180 to 300° C., and biaxially stretching the film.

[0260] The stretch ratio is preferably 1.1 to 100 times in terms of area, more preferably 2 to 90 times, further preferably 4 to 80 times, and particularly preferably 10 to 60 times. When the stretch ratio is within the above range, the electrical characteristics required for a film capacitor are easily exhibited.

[0261] The stretching method may be either a sequential biaxial stretching method or a simultaneous biaxial stretching method. From the viewpoint of film formation stability and thickness uniformity, the sequential biaxial stretching method is preferred.

[0262] In the case of the sequential biaxial stretching method, for example, the resin composition is extruded onto a cooling roller by a T-die extrusion molding method to obtain an unstretched film. Next, the unstretched film is stretched (longitudinally stretched) in the film length direction (MD direction) via a preheating roller set to a predetermined stretching temperature. Then, the film is stretched (transversely stretched) in the film width direction (TD direction) while passing through a heating oven set to a predetermined stretching temperature.

[0263] The stretching temperature for longitudinal stretching and transverse stretching is preferably between the glass transition temperature (Tg) and the melting point (Tm) of the polymer such as the 4-methyl-1-pentene copolymer (A) used for stretching. If the stretching is performed at a stretching temperature of 80°C to 210°C, a film showing the desired electrical properties is easily obtained. The above-mentioned stretching temperature is preferably 85°C to 210°C, more preferably 90°C to 210°C, and particularly preferably 90°C to 180°C. The stretching ratio is usually 1.2 to 11.0 times, preferably 1.4 to 9.5 times, and more preferably 2 to 9 times in the length direction of the film and the width direction of the film, respectively, independently.

[0264] In addition, after biaxial stretching, re-stretching may be performed in the film length direction or the film width direction, or in the film length direction and the film width direction. In addition, annealing treatment may be performed after biaxial stretching. The annealing temperature is usually 100 to 230°C, preferably 130 to 220°C.

[0265] Example

[0266] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0267] [Methods for measuring various physical properties]

[0268] <Constitutional unit content in 4-methyl-1-pentene copolymer>

[0269] The amount of constituent units derived from 4-methyl-1-pentene (4-methyl-1-pentene content) and the amount of constituent units derived from α-olefins other than 4-methyl-1-pentene (α-olefin content) were determined by the following apparatus and conditions: 13C-NMR spectrum was calculated.

[0270] The ECP500 NMR device manufactured by JEOL Ltd. was used, with a mixed solvent of o-dichlorobenzene / deuterated benzene (80 / 20 volume %) as the solvent, a sample concentration of 55 mg / 0.6 mL, a measurement temperature of 120°C, an observation nucleus of 13C (125 MHz), a sequence of single pulse proton decoupling, a pulse width of 4.7 μs (45° pulse), a repetition time of 5.5 seconds, an accumulation of more than 10,000 times, and 27.50 ppm as the reference value of the chemical shift for measurement. 13 C-NMR spectrum was used to quantify the composition of 4-methyl-1-pentene and α-olefins.

[0271] <Intrinsic viscosity [η]>

[0272] The intrinsic viscosity [η] is measured using decalin solvent at 135°C. That is, about 20 mg of polymer powder, pellets or resin blocks are dissolved in 15 mL of decalin and the specific viscosity η is measured in an oil bath at 135°C. sp After adding 5 mL of decalin solvent to dilute the decalin solution, the specific viscosity η was measured in the same manner. sp The dilution operation was repeated two more times, and the concentration (C) was extrapolated to η at 0. sp The value of / C was determined as the intrinsic viscosity (see the following formula).

[0273] [η] = lim(η sp / C)(C→0)

[0274] <CFC and molecular weight measurement>

[0275] CFC and molecular weight measurements were performed under the following conditions.

[0276] Device: CFC2 cross-fractionation chromatography (Polymer Char)

[0277] Detector (built-in): IR4 infrared spectrophotometer (Polymer Char)

[0278] Detection wavelength: 3.42μm (2,920cm -1 );fixed

[0279] Sample concentration: 30 mg / 30 mL (diluted with o-dichlorobenzene (ODCB))

[0280] Injection volume: 0.5mL

[0281] Temperature conditions: heating to 145°C at 40°C / min and holding for 30 minutes, cooling to 0°C at 1°C / min and holding for 60 minutes, and then evaluating the dissolution amount in each of the following dissolution zones. The temperature change between zones was set at 40°C / min.

[0282] Dissolution zones: The boundaries of the dissolution zones were set to 0, 5, 10, 15, 20, 25, 30, 35, 50, 70, 90, 95, 100, 102, 104, and 106°C in the range of 0 to 108°C, to every 1°C in the range of 108 to 135°C, and to 135, 140, and 145°C in the range of 135 to 145°C, and the dissolution amount in each zone was evaluated.

[0283] GPC column: Shodex HT-806M × 3 (Showa Denko)

[0284] GPC column temperature: 145°C

[0285] GPC column calibration: monodisperse polystyrene (Tosoh)

[0286] Molecular weight calibration method: Standard calibration method (polystyrene conversion)

[0287] Mobile phase: o-dichlorobenzene (ODCB) with BHT added

[0288] Flow rate: 1.0mL / min

[0289] [Production Examples 1 to 24]

[0290] According to the polymerization method described in Comparative Example 1 (

[0158] ) of International Publication No. 2017 / 150265, the α-olefin is changed to the α-olefin described in Table 1-1 and Table 1-2, and the usage ratio of 4-methyl-1-pentene, α-olefin and hydrogen is changed so that the physical properties of the obtained copolymer become the values ​​of Table 1-1 and Table 1-2, thereby obtaining 4-methyl-1-pentene copolymers (A-1) to (A-12) and (B-1) to (B-12).

[0291] [Table 1-1]

[0292]

[0293] [Table 1-2]

[0294]

[0295] [Example 1]

[0296] [Manufacturing of resin composition]

[0297] 0.1 parts by mass of tris(2,4-di-tert-butylphenyl)phosphate as an auxiliary antioxidant and 0.1 parts by mass of n-octadecyl 3-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate as a heat stabilizer were added to 35 parts by mass of the copolymer (A-1) and 65 parts by mass of the copolymer (B-1) obtained in the above production example.

[0298] Next, the obtained mixture was extruded using a twin-screw extruder BT-30 (screw diameter L / D=46), granulation was carried out under the conditions of a set temperature of 270°C, a resin extrusion amount of 60 g / min and 200 rpm to obtain pellets of the resin composition.

[0299] [Film production]

[0300] The obtained pellets were supplied to a single screw extruder (manufactured by Tanaka Iron Works Co., Ltd.), melt kneaded at a barrel temperature of 270°C, and melt extruded into a film from a T-type slit die at a die temperature of 270°C. Next, the obtained film was air-pressed onto a metal cooling roll controlled at 80°C and pulled at a pulling speed of 0.9 m / min. An unstretched film having a thickness of 200 μm was obtained after cooling and solidification.

[0301] [Stretching of film]

[0302] The obtained unstretched film was preheated by a heated metal roller to raise the film temperature to 160°C, and longitudinally stretched to 3 times between a pair of rollers with a peripheral speed difference, thereby preparing a uniaxially stretched film. Next, the two ends of the uniaxially stretched film in the width direction were gripped with a clamp, introduced into a heating oven, preheated to 160°C, and then transversely stretched to 5 times in the width direction, thereby preparing a biaxially stretched film. Then, the biaxially stretched film was heated to 200°C and annealed. The two ends of the biaxially stretched film thus obtained were cut by a razor using a razor blade, and then wound into a roll, thereby obtaining an evaluation sample.

[0303] The following physical property evaluations were performed using the evaluation samples.

[0304] [Examples 2 to 10, Comparative Examples 1 to 2]

[0305] An unstretched film and a biaxially stretched film were obtained in the same manner as in Example 1 except that the copolymer described in Table 2 was blended as the 4-methyl-1-pentene copolymer and the blending amount was set to the blending amount described in Table 2. Then, an evaluation sample was obtained in the same manner as in Example 1.

[0306] [Examples 11 to 14]

[0307] A 4-methyl-1-pentene copolymer, an unstretched film, and a biaxially stretched film were obtained in the same manner as in Example 3 except that the stretching conditions were changed to those described in Table 2. Then, an evaluation sample was obtained in the same manner as in Example 1.

[0308] The following physical property evaluations were performed using the evaluation samples.

[0309] <Intrinsic viscosity [η]>

[0310] The intrinsic viscosity [η] is measured by the above-mentioned measuring method.

[0311] <Melting point (Tm)>

[0312] In the measurement, the biaxially stretched film obtained above is used as a sample. Using a DSC measuring device (DSC220C) manufactured by Seiko Instruments, the melting point is measured in the following order. First, about 5 mg of the sample is set on an aluminum pan for measurement and sealed. The temperature is raised to 290°C at 100°C / min, and after being kept at 290°C for 5 minutes, the temperature is lowered to -100°C at 10°C / min, and then the temperature is raised from -100°C to 290°C at 10°C / min. In the thermal curve during the second heating, the melting point (Tm) is calculated from the peak vertex of the crystalline melting peak. When multiple peaks are detected, the peak with the highest temperature is taken as the melting point (Tm).

[0313] <Dielectric breakdown strength>

[0314] The dielectric breakdown strength (V / μm) is measured according to ASTM-D149 using a dielectric breakdown tester manufactured by YAMAYO Tester Co., Ltd. For the above-mentioned evaluation samples, a voltage is applied at 23°C and 120°C at a voltage increase rate of 500V / sec, and the dielectric breakdown voltage is measured to obtain the dielectric breakdown strength (V / μm). Next, the ratio V(120°C) / V(23°C) is calculated from the dielectric breakdown strength V(23°C) at 23°C and the dielectric breakdown strength V(120°C) at 120°C.

[0315] <Average thickness>

[0316] The thickness of the evaluation sample was measured at 10 points in the width direction and 10 points in the length direction using a micrometer, and the average value was defined as the thickness of the biaxially stretched film or the unstretched film.

[0317] <Surface roughness Ra>

[0318] The surface roughness of the sample surface was evaluated in the form of a roughness curve using a surface roughness meter manufactured by Tokyo Seimitsu Co., Ltd. A measurement length (l) was extracted in the direction of the average line, the X axis was taken in the direction of the average line of the extracted part, and the Y axis was taken in the direction of the longitudinal magnification. When the roughness curve was expressed by y=f(x), the value obtained by the following formula expressed in nanometers (nm) was taken as Ra. The measurement length was set to 10 mm.

[0319] Ra of less than 100 was evaluated as AA, and Ra of 100 or more was evaluated as BB.

[0320] [Number 1]

[0321]

[0322] <Surface roughness Rz>

[0323] Using a surface roughness meter manufactured by Tokyo Seimitsu Co., Ltd., the state of the concavoconvex surface of the evaluation sample is evaluated in the form of a roughness curve. Only the measurement length is extracted from the roughness curve in the direction of its average line, and the measurement is performed in the direction of the longitudinal magnification from the average line of the extracted part. The average value of the absolute value of the peak elevation (Yp) from the highest peak to the fifth highest peak and the average value of the absolute value of the valley elevation (Yv) from the lowest valley to the fifth lowest valley are calculated as follows, and the value expressed in nanometers (nm) is used as Rz. The measurement length is set to 10 mm.

[0324] The case where Rz was less than 500 was evaluated as AA, and the case where Rz was 500 or more was evaluated as BB.

[0325] [Number 2]

[0326]

[0327] Table 2 shows the evaluation results of the above-mentioned physical properties of each film.

[0328] [Table 2]

[0329]

Claims

1. A resin composition comprising a 4-methyl-1-pentene copolymer (A) satisfying the following requirements (Aa) to (Ad) and a 4-methyl-1-pentene copolymer (B) satisfying the following requirements (Ba) to (Bd), and satisfying the following requirements (1) and (2), wherein the melting point (Tm) of the resin composition is 210 to 240° C., (Aa) The amount U1 of constituent units derived from 4-methyl-1-pentene is 80.0 to 99.9 mol%, and the total amount U2 of constituent units derived from at least one selected from linear α-olefins having 10 to 20 carbon atoms is 20.0 to 0.1 mol%, wherein The total of U1 and U2 is set to 100 mol %; (Ab) Intrinsic viscosity measured in decalin at 135°C [η] A 0.5~5.0dL / g; (Ac) when the copolymer (A) is measured by a cross-fractionation chromatograph (CFC) using an infrared spectrophotometer as a detection unit, at least one peak of the amount of the eluted component is present in the range of 100 to 140° C.; (Ad) when the copolymer (A) is measured by the CFC, the molecular weight distribution Mw / Mn, which is the ratio of the weight average molecular weight Mw to the number average molecular weight Mn of the eluted component in the range of 100 to 140° C., is 1.0 to 4.5, (Ba) the amount U3 of constituent units derived from 4-methyl-1-pentene is 20.0 to 98.0 mol%, and the total amount U4 of constituent units derived from at least one selected from linear α-olefins having 10 to 20 carbon atoms is 80.0 to 2.0 mol%, wherein the total of U3 and U4 is 100 mol%; (Bb) Intrinsic viscosity measured in decalin at 135°C [η] B 2.0~8.0dL / g; (Bc) when the copolymer (B) is measured by a cross-fractionation chromatograph (CFC) using an infrared spectrophotometer as a detection unit, at least one peak of the amount of the eluted component exists in the range of 0° C. to less than 100° C.; (Bd) when the copolymer (B) is measured by the CFC, the molecular weight distribution Mw / Mn, which is the ratio of the weight average molecular weight Mw to the number average molecular weight Mn of the eluted component in the range of 0° C. to less than 100° C., is 1.0 to 7.0, (1) When the total content of the copolymer (A) and (B) is 100 parts by mass, the content of the copolymer (A) is 5 to 95 parts by mass, and the content of the copolymer (B) is 95 to 5 parts by mass; (2) The value (U4-U2) obtained by subtracting U2 (mol %) described in the requirement (Aa) from U4 (mol %) described in the requirement (Ba) is 0 mol % or more and 6.5 mol % or less.

2. The resin composition according to claim 1, wherein when the total content of the copolymer (A) and the copolymer (B) is set to 100 parts by mass, the content of the copolymer (A) is 5 parts by mass or more and less than 50 parts by mass, and the content of the copolymer (B) is greater than 50 parts by mass and less than 95 parts by mass. 3 . A molded body comprising the resin composition according to claim 1 . A film comprising the resin composition according to claim 1 or 2.

5. The film according to claim 4, which satisfies the following requirements (II) to (III), (II) The surface roughness Ra of the film is less than 100 nm; (III) The surface roughness Rz of the film is less than 500 nm. The film according to claim 4 or 5, which is a capacitor film.

Citation Information

Patent Citations

  • Method and catalyst for manufacture of syndiotactic polyolefin

    JP1990041303A

  • Metallocene compound

    JP1991193796A

  • Film for capacitor, metallized film and film capacitor

    JP2014011182A

  • 4-methyl-1-pentene copolymer composition

    JP2018162408A

  • Metallocene compound, process for producing metallocene compound, olefin polymerization catalyst, process for producing polyolefin, and polyolefin

    WO2001027124A1