A positive electrode precursor for sodium ion battery and its preparation method and application

By covering the nickel-ferromanganese ternary precursor shell on the core of the nickel-cobalt-manganese ternary precursor and using specific complexing agents, the uneven distribution and morphology of the Ni-Fe-Mn precursor in sodium ion batteries is solved. The poor problem improves the electrochemical stability and cycling performance of the battery.

CN115991506BActive Publication Date: 2024-11-12GUANGDONG JIANA ENERGY TECH CO LTD +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211650064.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-11-12
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The existing Ni-Fe-Mn layered hydroxide precursors have problems such as uneven element distribution, poor spherical shape, poor morphology, low tap density and poor circulation performance in sodium ion batteries, resulting in poor electrochemical performance. .

Method used

The nickel-cobalt-manganese ternary precursor is used as the core, and the outer surface is coated with the nickel-ferromanganese ternary precursor shell. A specific complexing agent is used to adjust the precipitation speed, achieve uniform co-precipitation, and improve spherical shape and tap density.

Benefits of technology

It achieves uniform element distribution, uniform particle size distribution, high spherical shape and high tap density, improves the electrochemical stability and cyclic performance of the positive electrode material of sodium ion battery and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115991506B_ABST
    Figure CN115991506B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of sodium ion batteries, and more specifically, to a positive electrode precursor for sodium ion batteries, and a preparation method and application thereof. The positive electrode precursor for sodium ion batteries has a core-shell structure, the core of the core-shell structure is a nickel-cobalt-manganese ternary precursor, and the shell of the core-shell structure is a nickel-iron-manganese ternary precursor; the specific surface area of ​​the positive electrode precursor for sodium ion batteries is greater than 9m 2 / g; the tap density of the positive electrode precursor for the sodium ion battery> 1.5g / cm 3 The complexing agent used in the process of forming the nickel-iron-manganese ternary precursor includes at least one of monoethanolamine, diethanolamine, triethanolamine, trisodium nitrilotriacetate, ethylenediaminetetraacetate, diethylenetriaminepentaacetic acid and its salts. The positive electrode precursor for sodium ion battery has the advantages of uniform element distribution, no segregation, uniform particle size distribution, good sphericity, clear primary particle morphology, high tap density, good electrochemical stability and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a positive electrode precursor for a sodium ion battery, and a preparation method and application thereof. Background Art

[0002] In the past decade, sodium-ion batteries have received a lot of attention from the academic and commercial circles. There are more than 20 companies engaged in sodium-ion battery research in the world. Chinese companies such as Sino-Science Sodium Battery are in a leading position in the industrialization of sodium-ion batteries. At present, the industrialization of sodium-ion batteries is still in its early stages, but sodium-ion batteries have the potential to be rapidly promoted.

[0003] The positive electrode material requires the use of sodium ion active materials. The mainstream positive electrode materials of sodium ion batteries include transition metal oxides, polyanionic compounds, Prussian blue compounds and liquid sodium, etc. Such materials need to have good electrochemical properties, safety, chemical stability and thermal stability, so as to have a high theoretical specific capacity and battery cycle life.

[0004] Transition metal oxides are currently the most popular positive electrode materials, such as sodium iron phosphate, sodium iron manganate, sodium titanate manganate, etc. These positive electrode materials have a higher discharge specific capacity in theory, but poor cycle performance. However, their shortcomings can be improved by introducing active or inert elements for doping or substitution. In lithium-ion batteries, elements such as copper and iron that cannot be used as positive electrode materials perform well in sodium-ion batteries. At present, the transition metal oxide system performs best. The copper-based oxide battery used by Sino-Science Sodium performs well, with an energy density of 145Wh / kg; the nickel layered oxide battery of the British company FARADION has a mass energy density of 150Wh / kg to 160Wh / kg, far exceeding other sodium-ion battery systems.

[0005] The coprecipitation method has the advantages of uniform product, easy to control morphology, low cost and low energy consumption. For example, the production of nickel, cobalt and manganese, a ternary material for lithium-ion batteries, is currently mainly carried out by using ammonia as a complexing agent to control the crystallization coprecipitation method under a protective atmosphere to obtain the hydroxide precursor of nickel, cobalt and manganese. However, the ternary material nickel, cobalt and manganese for lithium-ion batteries does not involve iron. The K of Fe(OH)2 at room temperature sp 8.0×10 -16 (much lower than Ni(OH)2 and Mn(OH)2), its precipitation pH is low, and it is easy to precipitate before other metals (Ni, Mn), and under alkaline environmental conditions, Fe 2+ , Fe 3+ It does not complex with ammonia water and cannot co-precipitate with Ni and Mn. It can only generate hydroxide precipitation, which leads to uneven distribution of co-precipitated materials (uneven distribution of Fe elements), which directly affects the electrochemical performance. 2+During the coprecipitation reaction, it is easily oxidized to Fe 3+ , Fe(OH)3 K sp 4.0×10 -38 , easier with OH - Combined precipitation forms new crystal nuclei, causing segregation, affecting the uniform distribution of Fe elements, and leading to uneven particle size distribution. In addition, since Ni-Fe-Mn is not uniformly co-precipitated, the sphericity of the precursor particles is poor and it is easy to be amorphous. The tap density of the precursor is low, and it is easy to become compacted during drying, which makes screening difficult.

[0006] Therefore, the current co-precipitation preparation process of Ni-Fe-Mn hydroxide precursor needs to be optimized and improved.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The first object of the present invention is to provide a positive electrode precursor for a sodium ion battery, by using a nickel-cobalt-manganese ternary precursor with high sphericity as the core, and using a specific type of complexing agent that can complex nickel ions, ferrous ions and manganese ions in the process of forming the shell of the nickel-iron-manganese ternary precursor, the precipitation rate difference in each metal ion reaction system is alleviated, and uniform coprecipitation is achieved; since the growth of the precursor is inherited, the nickel ions, ferrous ions and manganese ions will continue to attach to the growth site on the core and continue to grow to the target particle size. Therefore, the positive electrode precursor for a sodium ion battery provided by the present invention has uniform element distribution, no segregation, uniform particle size distribution, good sphericity, and high tap density.

[0009] The second object of the present invention is to provide a method for preparing a positive electrode precursor for a sodium ion battery, by first preparing a nickel-cobalt-manganese ternary precursor core, then coating the surface of the nickel-cobalt-manganese ternary precursor core with a nickel-iron-manganese ternary precursor shell, and using a specific type of complexing agent, the sphericity of the positive electrode precursor for a sodium ion battery can be effectively improved, the morphology can be improved, the tapping can be improved, and the elements can be evenly distributed without segregation.

[0010] The third object of the present invention is to provide a positive electrode plate.

[0011] A fourth object of the present invention is to provide a sodium ion battery.

[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0013] In a first aspect, the present invention provides a positive electrode precursor for a sodium ion battery, wherein the positive electrode precursor for a sodium ion battery has a core-shell structure, wherein the core of the core-shell structure is a nickel-cobalt-manganese ternary precursor, and the shell of the core-shell structure is a nickel-iron-manganese ternary precursor.

[0014] The primary particles of both the core and the shell in the core-shell structure are lamellar in shape, and the secondary particles are spherical in shape.

[0015] Among them, the chemical formula of the nickel-cobalt-manganese ternary precursor is Ni x Co y Mn z (OH)2, where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1.

[0016] Among them, the ratios of nickel, cobalt, and manganese elements in the nickel-cobalt-manganese ternary precursor can be any arbitrary and conventional ratios. x includes, but is not limited to, any point value among 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or the range value between any two of them; y includes, but is not limited to, any point value among 0.01, 0.05, 0.1, 0.2, 0.3 or the range value between any two of them; z includes, but is not limited to, any point value among 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or the range value between any two of them.

[0017] The chemical formula of the nickel-iron-manganese ternary precursor is Ni a Fe b Mn c (OH)2, where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1.

[0018] Among them, the ratios of nickel, iron, and manganese elements in the nickel-iron-manganese ternary precursor can be any arbitrary and conventional ratios. a includes, but is not limited to, any point value among 0.1, 0.2, 0.3, 0.4, 0.5 or the range value between any two of them; b includes, but is not limited to, any point value among 0.1, 0.2, 0.3, 0.4, 0.5 or the range value between any two of them; c includes, but is not limited to, any point value among 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or the range value between any two of them.

[0019] The specific surface area of the cathode precursor for sodium-ion batteries > 9 m 2 / g; including, but not limited to, 9.1 m 2 / g, 9.2 m 2 / g, 9.3 m 2 / g, 9.5 m 2 / g, 9.8 m 2 / g, 10 m 2 / g, 10.5 m 2 / g, 11 m 2 / g, 11.5 m2 / g, 12m 2 / g, 12.5m 2 / g, 13m 2 / g, 13.5m 2 / g, 14m 2 / g, 15m 2 / g, or a range of values ​​between them.

[0020] Among them, the specific surface area of ​​the precursor will affect the sintering activity of the back-end material, and then affect the capacity of the positive electrode material.

[0021] The tap density of the positive electrode precursor for sodium ion battery is>1.5g / cm 3 ; Including but not limited to 1.53g / cm 3 , 1.55g / cm 3 , 1.60g / cm 3 , 1.65g / cm 3 , 1.70g / cm 3 , 1.75g / cm 3 , 1.80g / cm 3 , 1.90g / cm 3 Any point value in or any range of values ​​between them.

[0022] The positive electrode precursor for sodium ion batteries prepared by the present invention has high tap density, and can avoid compaction during the drying process, which makes it difficult to sieve.

[0023] Moreover, tap density is the key to increasing capacity. The greater the tap density of a material, the more material can be packed into the battery under the same volume, and the greater the specific energy.

[0024] The complexing agent used in the process of forming the nickel-iron-manganese ternary precursor includes at least one of monoethanolamine, diethanolamine, triethanolamine, trisodium nitrilotriacetate, ethylenediaminetetraacetate, diethylenetriaminepentaacetic acid and their salt compounds.

[0025] In some specific embodiments of the present invention, the nickel-iron-manganese ternary precursor is formed by a co-precipitation method.

[0026] Among them, monoethanolamine is 2-hydroxyethylamine, also known as ethanolamine, and its chemical formula is C2H7NO.

[0027] Diethanolamine (DEA), also known as 2,2'-dihydroxydiethylamine, has a chemical formula of C4H 11 NO2.

[0028] Triethanolamine, also known as tri(2-hydroxyethyl)amine, can be regarded as a trihydroxyl substitute of triethylamine. Its chemical formula is C6H 15NO3.

[0029] Among them, the chemical formula of trisodium nitrilotriacetate is C6H8NNa3O7.

[0030] In some specific embodiments of the present invention, the EDTA salt includes disodium EDTA and / or tetrasodium EDTA.

[0031] In some specific embodiments of the present invention, the diethylenetriaminepentaacetic acid and its salt compounds include diethylenetriaminepentaacetic acid (DTPA, whose chemical formula is C 14 H 23 N3O 10 ) and / or diethylenetriamine pentaacetic acid pentasodium (DTPA-5Na, whose chemical formula is C 14 H 18 N3Na5O 10 ).

[0032] The primary particles of the nickel-cobalt-manganese ternary precursor are in the form of flakes, and the secondary particles are in the form of spheres (primary particles aggregate to form secondary particles).

[0033] The primary particles of the nickel-iron-manganese ternary precursor are in the form of flakes, and the secondary particles are in the form of spheres (primary particles aggregate to form secondary particles).

[0034] The present invention provides a positive electrode precursor for a sodium ion battery, aiming to solve the problems of uneven element distribution, poor sphericity, poor morphology, low tap density, low positive electrode material capacity and poor cycle performance existing in the Ni-Fe-Mn layered hydroxide precursor in the prior art.

[0035] like Figure 1 The cross-sectional structure diagram of the positive electrode precursor for sodium ion battery provided by the present invention is shown. The positive electrode precursor for sodium ion battery provided by the present invention has a core-shell structure, see Figure 1 The present invention uses a nickel-cobalt-manganese ternary precursor with high sphericity as the core (referred to as the NCM precursor core), covers the outer surface of the core with a nickel-iron-manganese ternary precursor to form a shell (referred to as the NFM precursor shell), and adds a specific type of complexing agent that can complex nickel ions, ferrous ions and manganese ions during the formation of the shell NFM, which can alleviate the precipitation rate difference of each metal ion in the reaction system, achieve uniform coprecipitation, make the elements evenly distributed and non-segregated, and avoid the generation of new nuclei to cause uneven particle size distribution. At the same time, since the growth of the precursor is inherited, the nickel ions, ferrous ions and manganese ions will continue to attach to the growth sites on the core and continue to grow to the target particle size, effectively improving the sphericity of the positive electrode precursor for sodium ion batteries, improving its morphology, and improving the tapping.

[0036] Therefore, the positive electrode precursor for sodium ion batteries provided by the present invention has the advantages of uniform element distribution, no segregation, uniform particle size distribution, good sphericity, clear primary particle morphology, high tap density, good electrochemical stability and cycle performance, etc., which can increase the life of sodium ion batteries and is suitable for mass production and application.

[0037] Preferably, the D50 particle size of the inner core is 1-5 μm, including but not limited to any point value of 2 μm, 3 μm, 4 μm or a range value between any two of them.

[0038] Preferably, the D50 particle size of the positive electrode precursor for a sodium ion battery is 4 to 15 μm, including but not limited to any point value of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, and 14 μm, or a range value between any two of them.

[0039] In some specific embodiments of the present invention, the chemical formula Ni x Co y Mn z In (OH)2, 0.1≤x≤0.98, 0.01≤y≤0.2, 0.01≤z≤0.9.

[0040] In some specific embodiments of the present invention, the chemical formula Ni a Fe b Mn c In (OH)2, 0.1≤a≤0.4, 0.1≤b≤0.4, 0.2≤c≤0.8.

[0041] In a second aspect, the present invention provides a method for preparing a positive electrode precursor for a sodium ion battery as described above, comprising the following steps:

[0042] A nickel-cobalt-manganese ternary mixed salt solution, a precipitant solution and a first complexing agent solution are added to the first base solution to carry out a first coprecipitation reaction to form a nickel-cobalt-manganese ternary precursor core and obtain a nickel-cobalt-manganese ternary precursor crystal core slurry.

[0043] Wherein, the first complexing agent solution includes at least one of ammonia water (ammonia water solution), ammonium sulfate solution, ammonium chloride solution and ammonium nitrate solution.

[0044] The nickel-cobalt-manganese ternary precursor crystal core slurry is evenly mixed with the precipitant solution and the second complexing agent solution to obtain a second base liquid, and then a nickel-iron-manganese ternary mixed salt solution, the precipitant solution and the second complexing agent solution are added thereto to carry out a second coprecipitation reaction to form a nickel-iron-manganese ternary precursor shell, and the nickel-iron-manganese ternary precursor shell is coated on the outer surface of the nickel-cobalt-manganese ternary precursor core. After the second coprecipitation reaction is completed, solid-liquid separation, screening and demagnetization are carried out in sequence to obtain the positive electrode precursor for the sodium ion battery.

[0045] The second complexing agent solution includes at least one of a monoethanolamine solution, a diethanolamine solution, a triethanolamine solution, a trisodium nitrilotriacetate solution, an ethylenediaminetetraacetate solution, a diethylenetriaminepentaacetic acid solution and a salt solution thereof.

[0046] The present invention first prepares a nickel-cobalt-manganese ternary precursor core with high sphericity, then covers the outer surface of the nickel-cobalt-manganese ternary precursor core with a nickel-iron-manganese ternary precursor shell, and uses a specific type of second complexing agent in the process of forming the nickel-iron-manganese ternary precursor shell, so that the sphericity of the positive electrode precursor for a sodium ion battery is effectively improved, the morphology is improved, the tapping is improved, and the elements are evenly distributed without segregation, and the particle size distribution is even.

[0047] In some specific embodiments of the present invention, the D50 particle size of the crystal nuclei (solid particles) in the nickel-cobalt-manganese ternary precursor crystal nucleus slurry is 1 to 5 μm. That is, the first coprecipitation reaction can be carried out until the D50 particle size of the crystal nuclei (solid particles) in the nickel-cobalt-manganese ternary precursor crystal nucleus slurry is 1 to 5 μm.

[0048] It is understandable that the end of the reaction can also be determined based on the reaction time of the first coprecipitation reaction.

[0049] Preferably, the molar concentration of the first complexing agent solution is 4-10 mol / L, including but not limited to any one of 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or a range between any two of them.

[0050] Preferably, the total molar concentration of metal ions in the nickel-cobalt-manganese ternary mixed salt solution is 1 to 2.5 mol / L, including but not limited to any one of 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, 2.3 mol / L or a range between any two of them.

[0051] Preferably, the molar concentration of the second complexing agent solution is 1-10 mol / L, including but not limited to any one of 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or a range between any two of them.

[0052] Preferably, the total molar concentration of metal ions in the nickel-iron-manganese ternary mixed salt solution is 1 to 3 mol / L, including but not limited to any one of 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, 2.3 mol / L, 2.5 mol / L, 2.8 mol / L or a range between any two of them.

[0053] In some specific embodiments of the present invention, the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese ternary mixed salt solution is 10-98 (including but not limited to any one of 20, 30, 40, 50, 60, 70, 80, 90 or a range between any two of them): 1-20 (including but not limited to any one of 3, 5, 8, 10, 12, 15, 18 or a range between any two of them): 1-90 (including but not limited to any one of 5, 10, 20, 30, 40, 50, 60, 70, 80 or a range between any two of them).

[0054] In some specific embodiments of the present invention, the molar ratio of nickel, iron and manganese in the nickel-iron-manganese ternary mixed salt solution is 10-40 (including but not limited to any one of 15, 20, 25, 30, 35 or any range between two): 10-40 (including but not limited to any one of 15, 20, 25, 30, 35 or any range between two): 20-80 (including but not limited to any one of 30, 40, 50, 60, 70 or any range between two). Among them, the iron element mainly exists in the form of ferrous ions. That is, the iron source used to prepare the nickel-iron-manganese ternary mixed salt solution is a ferrous salt, such as ferrous sulfate, ferrous nitrate, ferrous chloride, etc., but not limited thereto.

[0055] Preferably, the precipitant solution comprises sodium hydroxide solution and / or potassium hydroxide solution.

[0056] Preferably, the molar concentration of the precipitant solution used in the first coprecipitation reaction is 7-12 mol / L; including but not limited to any one of 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L or a range between any two of them.

[0057] Preferably, the molar concentration of the precipitant solution used in the second coprecipitation reaction is 2-8 mol / L, including but not limited to any one of 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, 6 mol / L, 7 mol / L or a range between any two of them.

[0058] Preferably, the pH value of the first base solution is 10.8-12.5, including but not limited to any one of 11.0, 11.3, 11.5, 12, 12.3 or a range between any two of them.

[0059] The mass concentration of ammonium ions in the first base solution is 1 to 5 g / L, including but not limited to any point value of 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L or a range value between any two of them.

[0060] In some specific embodiments of the present invention, the first base solution is mainly prepared by mixing a first complexing agent solution, a precipitant solution and water.

[0061] Preferably, the pH of the second base solution is 9.5-11, including but not limited to any one of 9.8, 10.0, 10.3, 10.5, 10.8 or a range between any two of them.

[0062] The molar concentration of the second complexing agent in the second base solution is 0.1-1 mol / L, including but not limited to any one of 0.3 mol / L, 0.5 mol / L, 0.8 mol / L or a range between any two of them.

[0063] In some specific embodiments of the present invention, water is also added during the process of uniformly mixing the nickel-cobalt-manganese ternary precursor crystal core slurry with the precipitant solution, the second complexing agent solution and water.

[0064] Preferably, during the first coprecipitation reaction, the temperature of the mixed material is 35-60°C, including but not limited to any point value of 40°C, 45°C, 50°C, 55°C, 58°C or a range value between any two of them.

[0065] In some specific embodiments of the present invention, the temperature of the first base liquid is 35-60°C, including but not limited to any point value of 40°C, 45°C, 50°C, 55°C, 58°C or a range value between any two of them.

[0066] During the first coprecipitation reaction, the pH of the mixed material is 10.5-12.5, including but not limited to any one of 11.0, 11.3, 11.5, 11.8, 12.0, 12.3 or a range between any two of them.

[0067] Preferably, during the first coprecipitation reaction, the mass concentration of ammonium ions in the mixed material is 1 to 5 g / L, including but not limited to any one of 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L or a range between any two of them.

[0068] Preferably, the first coprecipitation reaction time is 5 to 60 hours, including but not limited to any one of 10 hours, 20 hours, 30 hours, 40 hours, and 50 hours, or a range between any two of them.

[0069] In some specific embodiments of the present invention, during the first coprecipitation reaction, the mixed material is stirred at a speed of 150 to 350 r / min, wherein the speed includes but is not limited to any one of 200 r / min, 250 r / min, and 300 r / min or a range between any two of the above.

[0070] Preferably, during the second coprecipitation reaction, the temperature of the mixed material is 40-50°C, including but not limited to any one of 42°C, 45°C, 48°C or a range between any two of them.

[0071] In some specific embodiments of the present invention, the temperature of the second base liquid is 40-50°C, including but not limited to any point value of 42°C, 45°C, 48°C or a range value between any two of them.

[0072] During the second coprecipitation reaction, the pH of the mixed material is 9.5-11, including but not limited to any one of 9.8, 10.0, 10.3, 10.5, 10.8 or a range between any two of them.

[0073] Preferably, during the second coprecipitation reaction, the molar concentration of the complexing agent in the mixed material is 0.1-1.0 mol / L; including but not limited to any one of 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or a range between any two of them.

[0074] Preferably, the second coprecipitation reaction time is 10 to 100 h, including but not limited to any one of 20 h, 30 h, 40 h, 50 h, 60 h, 70 h, 80 h, 90 h or a range between any two of them.

[0075] In some specific embodiments of the present invention, during the second coprecipitation reaction, the mixed material is stirred at a speed of 100 to 200 r / min, wherein the speed includes but is not limited to any one of 120 r / min, 150 r / min, and 180 r / min or a range between any two of them.

[0076] In some specific embodiments of the present invention, the first coprecipitation reaction and the second coprecipitation reaction are both carried out under an inert gas atmosphere. Preferably, the inert gas atmosphere is a bubbling method to introduce an inert gas into the first base liquid and the second base liquid, respectively, and the inert gas is selected from at least one of nitrogen, helium and argon, and the amount of the inert gas introduced is 1 to 5 m 3 / h, including but not limited to 2m 3 / h、3m 3 / h、4m 3 / h, or the range between any two of them.

[0077] In some specific embodiments of the present invention, after the solid-liquid separation and before the screening, the steps of washing and drying are also included.

[0078] In a third aspect, the present invention provides a positive electrode plate, which is mainly prepared from the positive electrode precursor for a sodium ion battery as described above, or the positive electrode precursor for a sodium ion battery prepared by the preparation method of the positive electrode precursor for a sodium ion battery as described above.

[0079] In a fourth aspect, the present invention provides a sodium ion battery comprising the positive electrode plate as described above.

[0080] The sodium ion battery has excellent electrochemical performance, good electrochemical stability, good cycle performance and long service life.

[0081] Compared with the prior art, the present invention has the following beneficial effects:

[0082] The positive electrode precursor for a sodium ion battery provided by the present invention has the advantages of uniform element distribution, no segregation, uniform particle size distribution, good sphericity, clear primary particle morphology, high tap density, good electrochemical stability and cycle performance, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0084] Figure 1 A schematic cross-sectional structure diagram of a positive electrode precursor for a sodium ion battery provided by the present invention;

[0085] Figure 2 This is a SEM image of the nickel-cobalt-manganese ternary precursor core obtained in step (1) of Example 1 provided by the present invention;

[0086] Figure 3 This is a SEM image of the positive electrode precursor for a sodium ion battery prepared in step (2) of Example 1 provided by the present invention;

[0087] Figure 4 This is a SEM image of the nickel-cobalt-manganese ternary precursor core obtained in step (1) of Example 2 provided by the present invention;

[0088] Figure 5 This is a SEM image of the positive electrode precursor for a sodium ion battery prepared in step (2) of Example 2 provided by the present invention;

[0089] Figure 6 This is a SEM image of the positive electrode precursor for a sodium ion battery prepared in Comparative Example 1 provided by the present invention. DETAILED DESCRIPTION

[0090] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0091] Example 1

[0092] The method for preparing a positive electrode precursor for a sodium ion battery provided in this embodiment comprises the following steps:

[0093] (1) Prepare a mixed sulfate solution of nickel ions, cobalt ions, and manganese ions (i.e., a nickel-cobalt-manganese ternary mixed salt solution, i.e., a nickel-cobalt-manganese sulfate mixed solution), wherein the molar ratio of nickel, cobalt, and manganese is 8:1:1, and the sum of the concentrations of nickel ions, cobalt ions, and manganese ions (i.e., the total molar concentration of metal ions) is 1.5 mol / L. The three materials of the nickel-cobalt-manganese sulfate mixed solution, the 10 mol / L NaOH solution, and the 5 mol / L ammonia solution are respectively transported to a reactor having a first base liquid by a metering pump in a certain ratio (molar ratio 1:2:0.1), wherein the temperature of the first base liquid is 50°C, the pH is 11.8, and the ammonium radical concentration is 1.5 g / L. Under the protection of a nitrogen atmosphere, the temperature of the first coprecipitation reaction is controlled at 50°C, the pH of the reaction process is controlled at 11.4, the ammonium radical concentration is 1.5 g / L, and the stirring speed is 250 rpm, and the first coprecipitation reaction is carried out to form a nickel-cobalt-manganese ternary precursor core. After the reaction was continued for 50 hours, the feeding was stopped to obtain a nickel-cobalt-manganese ternary precursor crystal core slurry, wherein the particle size of the crystal core was D50=3.596 μm.

[0094] (2) Prepare a mixed sulfate solution of nickel ion, ferrous ion and manganese ion (i.e., a nickel-iron-manganese ternary mixed salt solution, i.e., a nickel-iron-manganese sulfate mixed solution), wherein the molar ratio of nickel element, iron element and manganese element is 30:35:35, and the sum of the concentrations of nickel ion, ferrous ion and manganese ion (i.e., the total molar concentration of metal ions) is 2.0 mol / L. The nickel-iron-manganese sulfate mixed solution, 8 mol / L NaOH (precipitant) solution and 3 mol / L disodium ethylenediaminetetraacetic acid solution are respectively transported to a reactor containing a second base liquid by a metering pump in a certain ratio (molar ratio of 1:2:0.12), wherein the second base liquid is obtained by uniformly mixing the nickel-cobalt-manganese ternary precursor crystal core slurry (500 L) obtained in step (1) with the precipitant solution, the second complexing agent solution and pure water, the temperature of the second base liquid is 50° C., the pH is 10.5, and the concentration of the second complexing agent in the second base liquid is 0.1 mol / L. Under the protection of nitrogen atmosphere, the temperature of the second coprecipitation reaction was controlled at 48°C, the pH of the reaction process was controlled at 10.0, the concentration of the complexing agent was 0.15 mol / L, the stirring speed was 150 rpm, and the second coprecipitation reaction was carried out to form a nickel-iron-manganese ternary precursor shell and coat it on the surface of the nickel-cobalt-manganese ternary precursor core. After 60 hours of continuous feeding, the feeding was stopped, and the qualified precursor slurry in the reactor was transported to a centrifuge for filtration, and then washed, dried, screened, demagnetized and packaged in sequence to obtain a positive electrode precursor for sodium ion batteries with a core-shell structure. The core of the core-shell structure is the nickel-cobalt-manganese ternary precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)2, the outer shell is a nickel-iron-manganese ternary precursor Ni 0.3 Fe 0.35Mn 0.35 (OH)2.

[0095] Among them, the particle size D50 of the positive electrode precursor for sodium ion batteries is 9.64 μm, and the tap density is 1.72 g / cm 3 , with a specific surface area of ​​9.56m 2 / g, the microscopic secondary particles are spherical particles, and the macroscopic morphology is black powder.

[0096] like Figure 1 Shown is a schematic diagram of the cross-sectional structure of the positive electrode precursor for a sodium ion battery provided by the present invention.

[0097] The SEM image of the nickel-cobalt-manganese ternary precursor core obtained in step (1) of this embodiment 1 is as follows: Figure 2 As shown, the SEM image of the positive electrode precursor for sodium ion battery prepared in step (2) of this embodiment 1 is as follows Figure 3 shown.

[0098] Example 2

[0099] The method for preparing a positive electrode precursor for a sodium ion battery provided in this embodiment comprises the following steps:

[0100] (1) Prepare a mixed sulfate solution of nickel ions, cobalt ions, and manganese ions (i.e., a nickel-cobalt-manganese ternary mixed salt solution, i.e., a nickel-cobalt-manganese sulfate mixed solution), wherein the molar ratio of nickel, cobalt, and manganese is 8:1:1, and the sum of the concentrations of nickel ions, cobalt ions, and manganese ions (i.e., the total molar concentration of metal ions) is 2.0 mol / L. The three materials of the nickel-cobalt-manganese sulfate mixed solution, the 10 mol / L NaOH solution, and the 5 mol / L ammonia solution are respectively transported to a reactor having a first base liquid by a metering pump in a certain ratio (molar ratio 1:2:0.1), wherein the temperature of the first base liquid is 50°C, the pH is 11.8, and the ammonium concentration is 1.5 g / L. Under the protection of a nitrogen atmosphere, the temperature of the first coprecipitation reaction is controlled at 55°C, the pH of the reaction process is controlled at 10.8, the ammonium concentration is 1.8 g / L, and the stirring speed is 250 rpm, and the first coprecipitation reaction is carried out to form a nickel-cobalt-manganese ternary precursor core. After the reaction was continued for 14 hours, the feeding was stopped to obtain a nickel-cobalt-manganese ternary precursor crystal core slurry, wherein the particle size of the crystal core was D50=2.583 μm.

[0101] (2) Prepare a mixed sulfate solution of nickel ion, ferrous ion and manganese ion (i.e., a nickel-iron-manganese ternary mixed salt solution, i.e., a nickel-iron-manganese sulfate mixed solution), wherein the molar ratio of nickel element, iron element and manganese element is 30:35:35, and the sum of the concentrations of nickel ion, ferrous ion and manganese ion (i.e., the total molar concentration of metal ions) is 2.0 mol / L. The nickel-iron-manganese sulfate mixed solution, 5 mol / L NaOH (precipitant) solution and 2 mol / L diethylenetriamine pentaacetic acid pentasodium solution are respectively transported to a reactor containing a second base liquid by a metering pump in a certain ratio (molar ratio of 1:2:0.2), wherein the second base liquid is obtained by uniformly mixing the nickel-cobalt-manganese ternary precursor crystal core slurry (1000 L) obtained in step (1) with the precipitant solution, the second complexing agent solution and pure water, the temperature of the second base liquid is 40° C., the pH is 10.5, and the concentration of the second complexing agent in the second base liquid is 0.3 mol / L. Under the protection of nitrogen atmosphere, the temperature of the second coprecipitation reaction was controlled at 40°C, the pH of the reaction process was controlled at 10.5, the concentration of the complexing agent was 0.2 mol / L, the stirring speed was 200 rpm, and the second coprecipitation reaction was carried out to form a nickel-iron-manganese ternary precursor shell and coat it on the surface of the nickel-cobalt-manganese ternary precursor core. After continuous feeding for 45 hours, the feeding was stopped, and the qualified precursor slurry in the reactor was transported to a centrifuge for filtration, and then washed, dried, screened, demagnetized and packaged in sequence to obtain a positive electrode precursor for sodium ion batteries with a core-shell structure. The core of the core-shell structure is the nickel-cobalt-manganese ternary precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)2, the outer shell is a nickel-iron-manganese ternary precursor Ni 0.3 Fe 0.35 Mn 0.35 (OH)2.

[0102] Among them, the particle size D50 of the positive electrode precursor for sodium ion batteries is 6.355 μm, and the tap density is 1.53 g / cm 3 , with a specific surface area of ​​12.39m 2 / g, the microscopic secondary particles are spherical particles, and the macroscopic morphology is black powder.

[0103] The SEM image of the nickel-cobalt-manganese ternary precursor core obtained in step (1) of this embodiment 2 is as follows: Figure 4 As shown, the SEM image of the positive electrode precursor for sodium ion battery prepared in step (2) of this embodiment 2 is as follows Figure 5 shown.

[0104] Example 3

[0105] The method for preparing a positive electrode precursor for a sodium ion battery provided in this embodiment comprises the following steps:

[0106] (1) is basically the same as (1) of Example 2, except that the molar ratio of nickel element, cobalt element and manganese element in the nickel cobalt manganese sulfate mixed solution is replaced with 55:5:40.

[0107] (2) is basically the same as (2) of Example 2, except that the molar ratio of nickel element, iron element and manganese element in the nickel-iron-manganese sulfate mixed solution is replaced with 10:30:60.

[0108] The positive electrode precursor for sodium ion battery with core-shell structure prepared in this embodiment has a core of nickel-cobalt-manganese ternary precursor Ni 0.55 Co 0.05 Mn 0.4 (OH)2, the outer shell is a nickel-iron-manganese ternary precursor Ni 0.1 Fe 0.3 Mn 0.6 (OH)2.

[0109] Among them, the particle size D50 of the positive electrode precursor for sodium ion batteries is 6.804 μm, and the tap density is 1.65 g / cm 3 , with a specific surface area of ​​13.68m 2 / g, the microscopic secondary particles are spherical particles, and the macroscopic morphology is black powder.

[0110] Example 4

[0111] The method for preparing a positive electrode precursor for a sodium ion battery provided in this embodiment comprises the following steps:

[0112] (1) Prepare a nitrate mixed solution of nickel ions, cobalt ions, and manganese ions (i.e., a nickel-cobalt-manganese ternary mixed salt solution, i.e., a nickel-cobalt-manganese nitrate mixed solution), wherein the molar ratio of nickel, cobalt, and manganese is 8:1:1, and the sum of the concentrations of nickel ions, cobalt ions, and manganese ions (i.e., the total molar concentration of metal ions) is 1.0 mol / L. The three materials of the nickel-cobalt-manganese nitrate mixed solution, 8 mol / L KOH solution, and 8 mol / L ammonia solution are respectively delivered to a reactor having a first base liquid by a metering pump in a certain ratio (molar ratio 1:2:0.24), wherein the temperature of the first base liquid is 40°C, the pH is 12, and the ammonium radical concentration is 3 g / L. Under the protection of a nitrogen atmosphere, the temperature of the first coprecipitation reaction is controlled at 40°C, the pH of the reaction process is controlled at 11.8, the ammonium radical concentration is 3 g / L, and the stirring speed is 250 rpm, and the first coprecipitation reaction is carried out to form a nickel-cobalt-manganese ternary precursor core. After the reaction was continued for 32 hours, the feeding was stopped to obtain a nickel-cobalt-manganese ternary precursor crystal core slurry, wherein the particle size of the crystal core was D50=1.453 μm.

[0113] (2) Prepare a nitrate mixed solution of nickel ion, ferrous ion and manganese ion (i.e., nickel-iron-manganese ternary mixed salt solution, i.e., nickel-iron-manganese nitrate mixed solution), wherein the molar ratio of nickel element, iron element and manganese element is 30:35:35, and the sum of the concentrations of nickel ion, ferrous ion and manganese ion (i.e., the total molar concentration of metal ions) is 3.0 mol / L. The nickel-iron-manganese nitrate mixed solution, 5 mol / L KOH solution and 5 mol / L trisodium nitrilotriacetate solution are respectively transported to a reactor containing a second base liquid by a metering pump in a certain ratio (molar ratio of 1:2:0.69), wherein the second base liquid is obtained by uniformly mixing the nickel-cobalt-manganese ternary precursor crystal core slurry (1000 L) obtained in step (1) with a precipitant solution, a second complexing agent solution and pure water, wherein the temperature of the second base liquid is 45° C., the pH is 10, and the concentration of the second complexing agent in the second base liquid is 0.8 mol / L. Under the protection of nitrogen atmosphere, the temperature of the second coprecipitation reaction was controlled at 45°C, the pH of the reaction process was controlled at 10, the concentration of the complexing agent was 0.8 mol / L, the stirring speed was 200 rpm, and the second coprecipitation reaction was carried out to form a nickel-iron-manganese ternary precursor shell and coat it on the surface of the nickel-cobalt-manganese ternary precursor core. After continuous feeding for 50 hours, the feeding was stopped, and the qualified precursor slurry in the reactor was transported to a centrifuge for filtration, and then washed, dried, screened, demagnetized and packaged in sequence to obtain a positive electrode precursor for sodium ion batteries with a core-shell structure. The core of the core-shell structure is the nickel-cobalt-manganese ternary precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)2, the outer shell is a nickel-iron-manganese ternary precursor Ni 0.3 Fe 0.35 Mn 0.35 (OH)2.

[0114] Among them, the particle size D50 of the positive electrode precursor for sodium ion batteries is 4.024 μm, and the tap density is 1.59 g / cm 3 , the specific surface area is 15.56m 2 / g, the microscopic secondary particles are spherical particles, and the macroscopic morphology is black powder.

[0115] Comparative Example 1

[0116] The preparation method of the positive electrode precursor for a sodium ion battery provided in this comparative example comprises the following steps:

[0117] A mixed sulfate solution of nickel ion, ferrous ion and manganese ion (i.e., a ternary mixed salt solution of nickel, iron and manganese, i.e., a mixed solution of nickel, iron and manganese sulfate) was prepared, wherein the molar ratio of nickel, iron and manganese was 30:35:35, and the sum of the concentrations of nickel ion, ferrous ion and manganese ion (i.e., the total molar concentration of metal ions) was 2.0 mol / L. The three materials of the mixed solution of nickel, iron and manganese sulfate, 5 mol / L NaOH solution and 2 mol / L ammonia solution were respectively transported to a reactor with a bottom liquid through a metering pump in a certain ratio (molar ratio 1:2:0.32), wherein the bottom liquid was a mixed solution of pure water, NaOH solution and complexing agent solution, the temperature of the bottom liquid was 40°C, the pH was 10.5, and the concentration of the complexing agent was 0.3 mol / L. Under the protection of a nitrogen atmosphere, the temperature of the coprecipitation reaction was controlled at 45°C, the pH of the reaction process was controlled at 10.5, the concentration of the complexing agent was 0.3 mol / L, and the stirring speed was 200 rpm. After continuous feeding for 45 hours, the feeding is stopped, and the qualified precursor slurry in the reactor is transported to a centrifuge for filtration, and then washed, dried, sieved, demagnetized and packaged in sequence to obtain a positive electrode precursor for a sodium ion battery.

[0118] Among them, the particle size D50 of the positive electrode precursor for sodium ion batteries is 6.355 μm, and the tap density is 1.09 g / cm 3 , with a specific surface area of ​​19.18m 2 / g, the microscopic secondary particles are amorphous particles, and the macroscopic morphology is black powder.

[0119] The SEM image of the positive electrode precursor for sodium ion battery prepared in this comparative example 1 is as follows: Figure 6 shown.

[0120] Comparative Example 2

[0121] The preparation method of the positive electrode precursor for a sodium ion battery provided in this comparative example is basically the same as that in Example 2, except that in step (2), the second complexing agent is replaced by ammonia water of equimolar concentration.

[0122] The particle size D50 of the positive electrode precursor for sodium ion battery prepared in this comparative example is 6.262 μm, and the tap density is 0.89 g / cm 3 , the specific surface area is 24.78m 2 / g, the microscopic secondary particles are amorphous particles, and the macroscopic morphology is black powder.

[0123] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A positive electrode precursor for sodium ion batteries, It is characterized in that The positive electrode precursor for a sodium ion battery has a core-shell structure, the core of the core-shell structure is a nickel-cobalt-manganese ternary precursor, and the shell of the core-shell structure is a nickel-iron-manganese ternary precursor; Among them, the chemical formula of the nickel-cobalt-manganese ternary precursor is Ni x Co y Mn z (OH) 2 , where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1; The chemical formula of the nickel-iron-manganese ternary precursor is Ni a Fe b Mn c (OH) 2 , where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1; The specific surface area of ​​the positive electrode precursor for sodium ion battery is>9m 2 / g; The tap density of the positive electrode precursor for sodium ion battery is>1.5g / cm 3 ; The complexing agent used in the process of forming the nickel-iron-manganese ternary precursor includes at least one of monoethanolamine, diethanolamine, triethanolamine, trisodium nitrilotriacetate, diethylenetriaminepentaacetic acid and salts thereof.

2. The positive electrode precursor for sodium ion battery according to claim 1, It is characterized in that The D50 particle size of the core is 1 to 5 μm; And / or, the D50 particle size of the positive electrode precursor for the sodium ion battery is 4 to 15 μm.

3. The method for preparing a positive electrode precursor for a sodium ion battery according to claim 1 or 2, It is characterized in that The steps include: Adding a nickel-cobalt-manganese ternary mixed salt solution, a precipitant solution and a first complexing agent solution into a first base solution to perform a first coprecipitation reaction to form a nickel-cobalt-manganese ternary precursor core, thereby obtaining a nickel-cobalt-manganese ternary precursor crystal core slurry; The nickel-cobalt-manganese ternary precursor crystal core slurry is uniformly mixed with the precipitant solution and the second complexing agent solution to obtain a second base solution, and then a nickel-iron-manganese ternary mixed salt solution, the precipitant solution and the second complexing agent solution are added thereto to perform a second coprecipitation reaction to form a nickel-iron-manganese ternary precursor shell and coat the surface of the nickel-cobalt-manganese ternary precursor core, and then solid-liquid separation, screening and demagnetization are sequentially performed to obtain the positive electrode precursor for a sodium ion battery; Wherein, the first complexing agent solution includes at least one of ammonia water, ammonium sulfate solution, ammonium chloride solution and ammonium nitrate solution; The second complexing agent solution includes at least one of a monoethanolamine solution, a diethanolamine solution, a triethanolamine solution, a trisodium nitrilotriacetate solution, a diethylenetriaminepentaacetic acid solution and a salt solution thereof.

4. The method for preparing a positive electrode precursor for a sodium ion battery according to claim 3, It is characterized in that At least one of the following conditions is met: (1) The molar concentration of the first complexing agent solution is 4 to 10 mol / L; (2) the total molar concentration of metal ions in the nickel-cobalt-manganese ternary mixed salt solution is 1 to 2.5 mol / L; (3) the molar concentration of the second complexing agent solution is 1 to 10 mol / L; (4) The total molar concentration of metal ions in the nickel-iron-manganese ternary mixed salt solution is 1 to 3 mol / L.

5. The method for preparing a positive electrode precursor for a sodium ion battery according to claim 3, It is characterized in that At least one of the following conditions is met: (1) The precipitant solution comprises sodium hydroxide solution and / or potassium hydroxide solution; (2) the molar concentration of the precipitant solution used in the first coprecipitation reaction is 7 to 12 mol / L; (3) The molar concentration of the precipitant solution used in the second coprecipitation reaction is 2 to 8 mol / L.

6. The method for preparing a positive electrode precursor for a sodium ion battery according to claim 3, It is characterized in that The pH of the first base solution is 10.8-12.5, and the mass concentration of ammonium ions in the first base solution is 1-5 g / L; And / or, the pH of the second base solution is 9.5-11, and the molar concentration of the second complexing agent in the second base solution is 0.1-1 mol / L.

7. The method for preparing a positive electrode precursor for a sodium ion battery according to claim 3, It is characterized in that At least one of the following conditions is met: (1) During the first coprecipitation reaction, the temperature of the mixed material is 35 to 60° C., and the pH of the mixed material is 10.5 to 12.5; (2) During the first coprecipitation reaction, the mass concentration of ammonium ions in the mixed material is 1 to 5 g / L; (3) The first coprecipitation reaction time is 5 to 60 hours.

8. The method for preparing a positive electrode precursor for a sodium ion battery according to claim 3, It is characterized in that At least one of the following conditions is met: (1) During the second coprecipitation reaction, the temperature of the mixed material is 40 to 50° C., and the pH of the mixed material is 9.5 to 11; (2) During the second coprecipitation reaction, the molar concentration of the complexing agent in the mixed material is 0.1 to 1.0 mol / L; (3) The second coprecipitation reaction time is 10 to 100 hours.

9. A positive electrode sheet, It is characterized in that The positive electrode precursor for a sodium ion battery is mainly prepared from the positive electrode precursor for a sodium ion battery as claimed in claim 1 or 2, or the positive electrode precursor for a sodium ion battery prepared by the preparation method of the positive electrode precursor for a sodium ion battery as claimed in any one of claims 3 to 8.

10. A sodium ion battery, It is characterized in that Comprising the positive electrode sheet as described in claim 9.

Citation Information

Patent Citations

  • Layered oxide positive electrode material, preparation method thereof and sodium ion battery

    CN115148978A

  • Layered sodium ion positive electrode material and preparation method and application thereof

    CN115394979A

  • Positive electrode active material and its preparation method, sodium ion battery and apparatus containing the sodium ion battery

    US20210336262A1