Polymer membranes and their applications

By controlling the standard deviation of the void volume value on the polymer film, the problems of optical deformation and glare of laminated glass after hot pressing are solved, and the effects of no optical deformation, no glare and good light penetration are achieved. It is suitable for automotive use Preparation of laminated glass.

CN115991919BActive Publication Date: 2024-12-03CHANG CHUN PETROCHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111208116.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-18
Publication Date
2024-12-03
Estimated Expiration
2041-10-18

AI Technical Summary

Technical Problem

Existing laminated glasses are prone to optical deformation and glare problems during the hot pressing process, which affects their visibility and light transmittance, and it is difficult to control the volume of voids and bubble residues.

Method used

Develop a polymer film with a specific standard deviation of void volume value at a specific load area ratio. By adjusting the surface concave and convex structure and material composition of the polymer film, ensuring that the laminated glass is free of optical deformation and glare after thermal pressing. And improve light penetration.

Benefits of technology

The laminated glass has no optical deformation, no glare and good light penetration, and its knocking adhesion and bubble residue test results are improved, which is suitable for the preparation of automotive laminated glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115991919B_ABST
    Figure CN115991919B_ABST
Patent Text Reader

Abstract

The present invention provides a polymer film and a laminated glass using the polymer film. The polymer film has a first surface and a second surface, wherein the standard deviation of the void volume value of the first surface when the load area ratio is 10% is 0.5 cubic micrometers / square micrometer to 2.5 cubic micrometers / square micrometer, and wherein the load area ratio and the void volume are defined according to ISO 25178-2:2012.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer film, and more particularly to a polymer film having a specific standard deviation of void volume (Vv) value at a specific material ratio. The present invention also relates to a laminated glass prepared using the polymer film. Background Art

[0002] Laminated glass is a composite glass material that is formed by sandwiching a polymer film between two glass sheets and tightly combining the glass sheets and the polymer film through heat pressing. Laminated glass is widely used in the automotive and construction industries because of its excellent impact resistance and sound insulation.

[0003] Since the preparation process of laminated glass involves hot pressing between glass sheets and polymer films, in order to prevent air from being trapped between the glass sheets and the polymer films of the laminated glass, patterns are usually pre-embossed on the surface of the polymer film to form patterns (i.e., a concave-convex structure is designed) so that air can be discharged smoothly during the pre-pressing period, thereby preventing bubbles from being generated in the laminated glass. However, the existing laminated glass often has fine filamentary streaks visible to the naked eye under light due to the patterns, causing visual defects of optical distortion, affecting the visibility of the laminated glass, and also affecting the light transmittance of the laminated glass, or prone to refraction and glare, causing discomfort to the viewer's eyes. Summary of the invention

[0004] The inventors have found that the above problem is unexpectedly related to the uniformity of the lines formed on the surface of the polymer film. If the lines on the surface of the polymer film are very uneven, the laminated glass is likely to have thin filamentary stripes visible to the naked eye under light after lamination, causing visual defects of optical deformation, thereby affecting the visibility of the laminated glass and also affecting the light transmittance of the laminated glass. On the contrary, if the lines on the surface of the polymer film are too uniform, the laminated glass is likely to have glare problems after lamination, causing discomfort to the viewer's eyes.

[0005] Based on this, the present invention aims to provide a polymer film, specifically, a polymer film having a specific standard deviation of void volume (Vv) value under a specific load area ratio. After the polymer film of the present invention is heat-pressed with a glass sheet, the laminated glass does not have optical deformation and glare problems, and has an improved light transmittance. The void volume value can be further controlled within a preferred range to further improve the knock adhesion value test and bubble residue test results of the laminated glass. Therefore, the polymer film of the present invention is particularly suitable for use in the preparation of automotive laminated glass.

[0006] Specifically, an object of the present invention is to provide a polymer film, wherein the polymer film has a first surface and a second surface, and the standard deviation of the void volume (Vv) value of the first surface when the load area ratio is 10% is 0.5 cubic micrometers / square micrometer (μm 3 / μm 2 ) to 2.5 cubic microns / square microns, and the definitions of the loading area ratio and the void volume are based on ISO 25178-2:2012.

[0007] In some embodiments of the present invention, the Vv value of the first surface of the polymer at a loading area ratio of 10% is 2 cubic micrometers / square micrometer to 35 cubic micrometers / square micrometer.

[0008] In some embodiments of the present invention, the first surface of the polymer has a surface roughness Rz value of 15 μm to 55 μm, wherein the Rz value is measured according to JIS B 0601 (1994).

[0009] In some embodiments of the present invention, the standard deviation of the Vv value of the second surface of the polymer at a loading area ratio of 10% is 0.5 cubic micrometers / square micrometer to 2.5 cubic micrometers / square micrometer.

[0010] In some embodiments of the present invention, the Vv value of the second surface of the polymer at a loading area ratio of 10% is 2 cubic micrometers / square micrometer to 35 cubic micrometers / square micrometer.

[0011] In some embodiments of the present invention, the second surface of the polymer has an Rz value of 15 μm to 55 μm, wherein the Rz value is measured according to JIS B 0601 (1994).

[0012] In some embodiments of the present invention, the polymer film comprises polyvinylacetal, and the polyvinylacetal can be selected from the following group: poly(vinyl formal), poly(vinyl acetal), poly(vinyl butyral), poly(vinyl valeral), poly(vinyl hexanal), and combinations thereof. In a preferred embodiment of the present invention, the polyvinyl acetal is poly(vinyl butyral).

[0013] In some embodiments of the present invention, the polymer film has a thickness of 0.1 mm to 2.5 mm.

[0014] Another object of the present invention is to provide a laminated glass, comprising a first glass sheet, a second glass sheet, and an intermediate film between the first glass sheet and the second glass sheet, wherein the intermediate film is provided by the polymer film as described above.

[0015] In order to make the above-mentioned objectives, technical features and advantages of the present invention more obvious and easy to understand, some specific implementation schemes are described in detail below. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a test sampling schematic diagram of the “standard deviation of void volume (Vv) value” of the present invention. DETAILED DESCRIPTION

[0017] Some specific embodiments according to the present invention will be described in detail below; however, without departing from the spirit of the present invention, the present invention can also be practiced in a variety of different forms of solutions, and the protection scope of the present invention should not be limited to the specific embodiments.

[0018] Unless otherwise stated, the terms “a”, “an”, “the” and similar terms used in the specification and claims should be understood to include both the singular and the plural.

[0019] Unless otherwise specified, the terms “first”, “second” and the like used in the specification and the claims are merely used to distinguish the described elements or components and have no special meanings and are not used to represent a sequence.

[0020] Unless otherwise specified, in this specification and claims, the term "load area ratio" is defined in accordance with ISO 25178-2: 2012. The load area curve is a function curve of the surface height to the area of ​​the area it covers, and the load area ratio refers to the area above a specified height.

[0021] Unless otherwise specified, in this specification and claims, the term "void volume (Vv)" is defined in accordance with ISO 25178-2: 2012. Void volume (Vv) refers to the volume of voids per unit area at a specific load area ratio.

[0022] In this specification and claims, the term "standard deviation of void volume (Vv) values" is calculated as follows: Figure 1 As shown, on a 30 cm × 30 cm polymer film, 3 cm × 3 cm test samples were cut at four corners 1 cm away from the two edges and at the center to obtain five test samples, and the Vv values ​​of the five test samples were measured, and the standard deviation of the void volume value was calculated based on the five Vv values.

[0023] Unless otherwise specified, in this specification and claims, the term "surface roughness Rz value" refers to the ten-point average roughness of a surface and is measured according to JIS B 0601 (1994).

[0024] The utility of the present invention compared with the prior art is to provide a polymer film having a specific Vv value standard deviation at a specific load area ratio, and to provide a laminated glass having no optical distortion and glare problems and good light transmittance by using the polymer film. The laminated glass is particularly suitable for application in the automotive industry. The following is a detailed description of the polymer film of the present invention and its related applications.

[0025] 1. Polymer film

[0026] 1.1. Composition of polymer films

[0027] The polymer film of the present invention comprises polyvinyl acetal as an essential component, and may further comprise other optional components, such as a plasticizer or other existing additives, as required. In some embodiments of the present invention, the polymer film comprises polyvinyl acetal and a plasticizer, or the polymer film is substantially composed of polyvinyl acetal and a plasticizer, or the polymer film is composed of polyvinyl acetal and a plasticizer.

[0028] The polymer film of the present invention may be a single-layer film consisting of a single layer, or a multi-layer film consisting of multiple layers, as long as the polymer film as a whole meets the specified Vv value standard deviation conditions. In the scheme where the polymer film is a multi-layer film, the materials of each layer of the polymer film may be the same or different, and each layer may play the same or different functional layer, and the functional layer may provide one or more of the following functions: sound insulation function, heat insulation function, reflection function, anti-reflection function, refraction function, anti-refraction function, light splitting function, and light reduction function.

[0029] 1.1.1. Polyvinyl acetal

[0030] Examples of polyvinyl acetals include, but are not limited to, poly(vinyl formal), poly(vinyl acetal), poly(vinyl butyral), poly(vinyl valeral), and poly(vinyl hexane acetal). Each of the aforementioned polyvinyl acetals may be used alone or in combination. In a preferred embodiment of the present invention, the polyvinyl acetal is poly(vinyl butyral). In the following examples, the polymer film is composed of poly(vinyl butyral) and a plasticizer.

[0031] The molecular weight of the polyvinyl acetal is not particularly limited. In some embodiments of the present invention, the number average molecular weight (Mn) of the polyvinyl acetal may be 90,000 to 125,000, more specifically 105,000 to 120,000, such as 90,000, 90,500, 91,000, 91,500, 92,000, 92,500, 93,000, 93,500, 94,000, 94,500, 95,000, 95,500, 96,000. , 96,500, 97,000, 97,500, 98,000, 98,500, 99,000, 99,500, 100,000, 100,500, 101,000, 101,500, 102,000, 102,500, 103,000, 103,500, 104,000, 104,500, 105,000, 105,500, 106,000, 106,500, 1 07,000、107,500、108,000、108,500、109,000、109,500、110,000、110,500、111,000、111,500、112,000、112,500、113,000、113,500、114,000、114,500、115,000、115,500、116,000、116,500、117 ,000, 117,500, 118,000, 118,500, 119,000, 119,500, 120,000, 120,500, 121,000, 121,500, 122,000, 122,500, 123,000, 123,500, 124,000, 124,500, or 125,000, or within the range formed by any two of the above values, but the invention is not limited thereto.

[0032] In some embodiments of the present invention, the polyvinyl acetal may have an acetal content (i.e., degree of acetalization) of 74% to 84% by weight, based on the total weight of hydroxyl groups, acetal groups, and acetyl groups of the polyvinyl acetal, such as 74%, 74.5%, 75%, 75.5%, 76%, 76.5%, 77%, 77.5%, 78%, 78.5%, 79%, 79.5%, 80%, 80.5%, 81%, 81.5%, 82%, 82.5%, 83%, 83.5%, or 84% by weight, or a degree of acetalization within a range formed by any two of the foregoing values. The polyvinyl acetal may have an acetyl content (i.e., degree of acetylation) of 0.1 wt % to 3.0 wt %, based on the total weight of the hydroxyl group, acetal group, and acetyl group of the polyvinyl acetal, for example, 0.1 wt %, 0.2 wt %, 0.3 wt %, 0.4 wt %, 0.5 wt %, 0.6 wt %, 0.7 wt %, 0.8 wt %, 0.9 wt %, 1.0 wt %, 1.1 wt %, 1.2 wt %, 1.3 wt %, 1.4 wt %, 1.5 wt %, 1.6 wt %, 1.7 wt %, 1.8 wt %, 1.9 wt %, 2.0 wt %, 2.1 wt %, 2.2 wt %, 2.3 wt %, 2.4 wt %, 2.5 wt %, 2.6 wt %, 2.7 wt %, 2.8 wt %, 2.9 wt %, or 3.0 wt %, or a degree of acetylation within a range consisting of any two of the foregoing values.

[0033] In a preferred embodiment of the present invention, based on the total weight of the hydroxyl group, acetal group and acetyl group of the polyvinyl acetal, the hydroxyl content of the polyvinyl acetal is preferably 16% to 23% by weight, more preferably 18% to 21% by weight, such as 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, or 23% by weight, or within the range formed by any two of the above values. When the hydroxyl content of the polyvinyl acetal is within the specified range, the polyvinyl acetal has better compatibility with the plasticizer. If the hydroxyl content of the polyvinyl acetal is higher than the specified range, the plasticizer is prone to seepage. If the hydroxyl content of the polyvinyl acetal is lower than the specified range, the pummel adhesion of the laminated glass obtained is poor and does not meet the specifications.

[0034] 1.1.2. Plasticizer

[0035] Herein, plasticizer refers to a chemical substance that can change the plasticity of thermoplastic resin, and may also be referred to as plasticizer. Examples of plasticizers include, but are not limited to, esters of polyacids or polyols, such as triethylene glycol bis(2-ethylhexanoate), tetraethylene glycol bis(2-ethylhexanoate), triethylene glycol bis(2-ethylbutyrate), tetraethylene glycol bis(2-ethylbutyrate), triethylene glycol diheptanoate, tetraethylene glycol diheptanoate, dihexyl adipate, dioctyl adipate, cyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, bis[2-(2-butoxyethoxy)ethyl adipate], polymeric adipate (polymeric adipate), dipropylene glycol dibenzoate, tripropylene glycol dibenzoate, polypropylene glycol dibenzoate, isodecyl benzoate, 2-ethylhexyl benzoate, propylene glycol dibenzoate, diisononyl phthalate, dibutoxyethyl terephthalate, castor oil, methyl ricinoleate, soybean oil, epoxidized soybean oil, and combinations thereof.

[0036] The consumption of plasticizer has no particular restrictions, as long as the pre-plasticizing effect can be provided. Generally speaking, the consumption of plasticizer can be controlled at 30 to 60 weight parts with 100 weight parts of polyvinyl acetal, for example 30 weight parts, 31 weight parts, 32 weight parts, 33 weight parts, 34 weight parts, 35 weight parts, 36 weight parts, 37 weight parts, 38 weight parts, 39 weight parts, 40 weight parts, 41 weight parts, 42 weight parts, 43 weight parts, 44 weight parts, 45 weight parts, 46 weight parts, 47 weight parts, 48 ​​weight parts, 49 weight parts, 50 weight parts, 51 weight parts, 52 weight parts, 53 weight parts, 54 weight parts, 55 weight parts, 56 weight parts, 57 weight parts, 58 weight parts, 59 weight parts, or 60 weight parts, or in the scope consisting of any two numerical values.

[0037] 1.1.3. Other existing additives

[0038] Existing additives may include any substance that can adaptably improve the processability of the polymer film during the manufacturing process, or impart specific functions to the polymer film. Examples of existing additives include, but are not limited to, dyes, pigments, stabilizers, antioxidants, flame retardants, infrared absorbers, infrared blockers, ultraviolet absorbers, ultraviolet stabilizers, lubricants, dispersants, surfactants, chelating agents, coupling agents, adhesives, and adhesion control agents. The aforementioned additives can be used alone or in combination. For example, the polymer film may contain a dye or a pigment to form a colored polymer film, or contain an ultraviolet absorber or an infrared absorber to form a polymer film with anti-ultraviolet function or a polymer film with anti-infrared function.

[0039] 1.2. Properties of polymer films

[0040] 1.2.1. Void volume (Vv)

[0041] The concavoconvex structure of the surface of a polymer film can be presented by measuring the three-dimensional image of the surface morphology. ISO 25178-2:2012 is a measurement specification for evaluating surface morphology, which discloses a parameter related to surface morphology, namely, void volume (Vv). Vv is defined as the void volume per unit area at a specified load area ratio, and can be calculated from an area load area curve, wherein the Y axis of the area load area curve represents the surface height, and the X axis represents the load area ratio. When the load area ratio of the X axis is 0%, the surface height of the Y axis is the maximum value, and when the load area ratio of the X axis is 100%, the surface height of the Y axis is 0. For example, the Vv value at a load area ratio of 10% represents the void volume size covered below the horizontal cutting plane set at the Y axis surface height corresponding to the load area ratio of 10% on the X axis. Therefore, when the load area ratio is 0%, the Vv value is the maximum value, and when the load area ratio is 100%, the Vv value is 0. For relevant descriptions of the Vv parameter, please refer to ISO25178-2:2012, the full text of which is incorporated herein for reference.

[0042] In the process of preparing laminated glass, in order to allow air to be discharged smoothly without remaining between the polymer film and the glass sheet, the surface of the polymer film needs to be formed with textures (i.e., specific concave-convex structures) to facilitate exhaust. However, studies have found that when the standard deviation of the Vv value on the surface of the polymer film is too large, there will be fine filamentary stripes in the middle of the laminated glass after the hot pressing process that are visible to the naked eye under light, which will cause optical deformation visual defects to the viewer, affecting the visibility of the laminated glass and even the light transmittance of the laminated glass. On the other hand, if the standard deviation of the Vv value on the surface of the polymer film is too small, the laminated glass will have glare problems, causing discomfort to the viewer's eyes.

[0043] In view of this, one technical feature of the present invention is to control the standard deviation of the Vv value of the polymer film within a specific range to avoid the optical deformation and glare problems of the laminated glass. Specifically, the standard deviation of the Vv value of the first surface of the polymer film of the present invention when the load area rate is 10% is 0.5 cubic micrometers / square micrometer to 2.5 cubic micrometers / square micrometer, such as 0.5 cubic micrometers / square micrometer, 0.6 cubic micrometers / square micrometer, 0.7 cubic micrometers / square micrometer, 0.8 cubic micrometers / square micrometer, 0.9 cubic micrometers / square micrometer, 1.0 cubic micrometers / square micrometer, 1.1 cubic micrometers / square micrometer, 1.2 cubic micrometers / square micrometer, 1.3 cubic micrometers / square micrometer, 1.4 cubic micrometers / square micrometer, 1.6 cubic micrometers / square micrometer, 1.7 cubic micrometers / square micrometer, 1.8 cubic micrometers / square micrometer, 1.9 cubic micrometers / square micrometer, 2.0 cubic micrometers / square micrometer, 2.1 cubic micrometers / square micrometer, 2.2 cubic micrometers / square micrometer, 2.3 cubic micrometers / square micrometer, 2.4 cubic micrometers / square micrometer, 2.5 cubic micrometers / square micrometer, 2.6 cubic micrometers / square micrometer, 2.7 cubic micrometers / square micrometer, 2.8 cubic micrometers / square micrometer, 2.9 cubic micrometers / square micrometer, 3.0 cubic micrometers / square micrometer, 3.1 cubic micrometers / square micrometer, 3.2 cubic micrometers / square micrometer, 3.3 cubic micrometers / square micrometer, 3.4 cubic micrometers / square micrometer, 3.5 cubic micrometers / square micrometer, 3.6 cubic micrometers / square micrometer, micrometers, 1.4 cubic micrometers / square micrometer, 1.5 cubic micrometers / square micrometer, 1.6 cubic micrometers / square micrometer, 1.7 cubic micrometers / square micrometer, 1.8 cubic micrometers / square micrometer, 1.9 cubic micrometers / square micrometer, 2.0 cubic micrometers / square micrometer, 2.1 cubic micrometers / square micrometer, 2.2 cubic micrometers / square micrometer, 2.3 cubic micrometers / square micrometer, 2.4 cubic micrometers / square micrometer, or 2.5 cubic micrometers / square micrometer, or within a range consisting of any two of the above values.

[0044] In addition, the smaller the Vv value is, the shallower the grooves on the surface of the polymer film are, which makes it difficult for the air between the polymer film and the glass sheet to be completely discharged and difficult to fully bond. In view of this, in order to make the laminated glass free of bubbles and edge debonding defects, the first surface of the polymer film of the present invention preferably has a Vv value within a specific range.In some embodiments of the present invention, the Vv value of the first surface of the polymer membrane at a loading area rate of 10% is 2 cubic microns / square microns to 35 cubic microns / square microns, for example, 2 cubic microns / square microns, 2.5 cubic microns / square microns, 3 cubic microns / square microns, 3.5 cubic microns / square microns, 4 cubic microns / square microns, 4.5 cubic microns / square microns, 5 cubic microns / square microns, 5.5 cubic microns / square microns, 6 cubic microns / square microns, 6.5 cubic microns / square microns, 7 cubic microns / square microns, 7.5 cubic microns / square microns, 8 cubic microns / square microns, 8.5 cubic microns / square microns, 9 cubic microns / square microns, 10 cubic microns / square microns, 11 cubic microns / square microns, 12 cubic microns / square microns, 13 cubic microns / square microns, 14 cubic microns / square microns, 15 cubic microns / square microns, 16 cubic microns / square microns, 17 cubic microns / square microns, 18 cubic microns / square microns, 19 cubic microns / square microns, 20 cubic microns / square microns, 21 cubic microns / square microns, 23 cubic microns / square microns, 24 cubic microns / square microns, 25 cubic microns / square microns, 26 cubic microns / square microns, 27 cubic microns / square microns, 28 cubic microns / square microns, 29 cubic microns / square microns, 30 cubic microns / square microns, 31 cubic microns / square microns, 33 cubic microns / square microns, 34 cubic microns / square microns, 35 cubic microns / square microns 15 cubic microns / square microns, 16 cubic microns / square microns, 16.5 cubic microns / square microns, 17 cubic microns / square microns, 17.5 cubic microns / square microns, 18 cubic microns / square microns, 19 cubic microns / square microns, 20 cubic microns / square microns, 21 cubic microns / square microns, 22 cubic microns / square microns, 23 cubic microns / square microns, 24 cubic microns / square microns, 25 cubic microns / square microns, 26 cubic microns / square microns, 27 cubic microns / square microns, 28 cubic microns / square microns, 29 cubic microns / square microns, 30 cubic microns / square microns, 31 cubic microns / square microns, 32 cubic microns / square microns, 33 cubic microns / square microns, 34 cubic microns / square microns, 35 cubic microns / square microns, 36 cubic microns / square microns, 37 cubic microns / square microns, 38 cubic microns / square microns, 39 cubic microns / square microns, 40 cubic microns / square microns, 41 cubic microns / square microns, 42 cubic microns / square microns, 43 cubic microns / square microns, 44 cubic microns / square microns m / sq. micron, 18.5 m3 / sq. micron, 19 m3 / sq. micron, 19.5 m3 / sq. micron, 20 m3 / sq. micron, 20.5 m3 / sq. micron, 21 m3 / sq. micron, 21.5 m3 / sq. micron, 22 m3 / sq. micron, 22.5 m3 / sq. micron, 23 m3 / sq. micron, 23.5 m3 / sq. micron, 24 m3 / sq. micron, 24.5 m3 / sq. micron, 25 m3 / sq. micron, 25.5 m3 / sq. micron, 26 m3 / sq. micron, 26.5 m3 / sq. micron, 27 m3 / sq. micron m / square micron, 27.5 cubic microns / square micron, 28 cubic microns / square micron, 28.5 cubic microns / square micron, 29 cubic microns / square micron, 29.5 cubic microns / square micron, 30 cubic microns / square micron, 30.5 cubic microns / square micron, 31 cubic microns / square micron, 31.5 cubic microns / square micron, 32 cubic microns / square micron, 32.5 cubic microns / square micron, 33 cubic microns / square micron, 33.5 cubic microns / square micron, 34 cubic microns / square micron, 34.5 cubic microns / square micron, or 35 cubic microns / square micron, or in a range consisting of any two of the above values.

[0045] In a preferred embodiment of the present invention, the standard deviation of the Vv value of the second surface of the polymer film when the load area rate is 10% is also 0.5 cubic microns / square microns to 2.5 cubic microns / square microns. In addition, the Vv value of the second surface of the polymer when the load area rate is 10% can be 2 cubic microns / square microns to 35 cubic microns / square microns. The specific numerical examples of the Vv value of the second surface can refer to the relevant description of the first surface, and will not be repeated here.

[0046] 1.2.2.Rz value

[0047] In some embodiments of the present invention, the first surface of the polymer film has an Rz value of 15 to 55 μm, for example, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, or 55 μm, or within a range consisting of any two of the above values. The Rz value is measured according to JIS B 0601 (1994).

[0048] In a preferred embodiment of the present invention, the second surface of the polymer film also preferably has an Rz value of 15 μm to 55 μm. For specific numerical examples of the Rz value of the second surface, reference may be made to the relevant description of the first surface.

[0049] 1.2.3. Glass transition temperature (Tg)

[0050] In some embodiments of the present invention, the glass transition temperature (Tg) of the polymer film can be controlled at 10°C to 22°C, for example, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, or 22°C, or within a range consisting of any two of the above values. If the Tg of the polymer film is higher than the specified range, the polymer film is relatively hard, and it may not be easy to form the desired texture when mechanical embossing is performed. If the Tg of the polymer film is lower than the specified range, the polymer film is relatively soft, and the polymer film may be easily broken when mechanical embossing is performed. In a preferred embodiment of the present invention, the Tg of the polymer film is 12°C to 15°C.

[0051] 1.2.4.Thickness

[0052] Under the condition of meeting the specified Vv value standard deviation, the thickness of the polymer film of the present invention can be adjusted according to actual needs. Generally speaking, the thickness of the polymer film can be 0.1 mm to 2.5 mm, such as 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm, 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, 0.55 mm, 0.6 mm, 0.65 mm, 0.7 mm, 0.75 mm, 0.8 mm, 0.85 mm, 0.9 mm, 0.95 mm, 1.0 mm, 1.05 mm, 1.1 mm, 1.15 mm, 1.2 mm, 1.25 mm In some embodiments, the polymer film has a thickness of 0.1 mm, 0.2 mm, 0.3 mm, 0.76 mm, or 1.52 mm. In some embodiments, the polymer film has a thickness of 0.1 mm, 0.2 mm, 0.3 mm, 0.76 mm, or 1.52 mm.

[0053] The polymer film of the present invention is not limited to the film with uniform thickness as described above. The polymer film of the present invention may also be a wedge-shaped film with different thicknesses at both ends, which is usually used to prepare a head-up display (HUD) for a car. Therefore, in this article, a wedge-shaped film with different thicknesses at both ends is also referred to as a "HUD film". In some embodiments of the present invention, the thickness of the thin end of the HUD film may be 0.5 to 1 mm, for example, 0.5 mm, 0.55 mm, 0.6 mm, 0.65 mm, 0.7 mm, 0.75 mm, 0.8 mm, 0.85 mm, 0.9 mm, 0.95 mm, or 1 mm, or within a range consisting of any two of the above values. In some embodiments of the present invention, the thickness of the thick end of the HUD film may be 1.2 mm to 1.7 mm, such as 1.2 mm, 1.25 mm, 1.3 mm, 1.35 mm, 1.4 mm, 1.45 mm, 1.5 mm, 1.55 mm, 1.6 mm, 1.65 mm, or 1.7 mm, or within a range consisting of any two of the above values. In the following embodiment, the thickness of the thin end of the HUD film is 0.76 mm and the thickness of the thick end is 1.45 mm, and the width of the HUD film is 1210 mm.

[0054] 1.3. Preparation of polymer membranes

[0055] The preparation method of the polymer film of the present invention is not particularly limited. For example, polyvinyl acetal and selected components (such as plasticizers) can be mixed and kneaded to obtain a polymer film composition, and then the polymer film composition is formed into a film using an existing film preparation method, and mechanical embossing is performed to facilitate providing the desired Vv value standard deviation, Vv value, and Rz value on the surface of the polymer film. Examples of the film preparation method include but are not limited to calendaring, casting, extrusion tentering, direct extrusion, and extrusion blow molding.

[0056] In some embodiments of the present invention, the polymer film is prepared in the following manner, but the present invention is not limited thereto: a resin-state polyvinyl acetal and a plasticizer are mixed at a temperature of 100° C. to 150° C. and a rotation speed of 10 rpm to 50 rpm using a mixer, and kneaded for 5 minutes to 30 minutes to obtain a polymer film composition. After the polymer film composition is cooled to room temperature, the polymer film composition is placed in an extruder to extrude into a film. The above film-forming steps are repeated as needed and the composition of the polymer film composition is adjusted to provide films with different functions, and each film can be laminated to form a polymer film with a multilayer structure.

[0057] The polymer film can then be preheated and mechanically embossed to provide the desired Vv value standard deviation, Vv value, and Rz value, wherein the angles of the upper and lower embossing wheels can be adjusted to make the extruded polymer film into a wedge shape to produce a HUD film. Mechanical embossing refers to the use of rollers to create patterns on the surface of a formed polymer film. The methods of mechanical embossing include, but are not limited to, the embossing wheel method and the calendering wheel method, among which the embossing wheel method is preferred. There is no special restriction on the pattern style of mechanical embossing, for example, including diamond, linear, serrated, square, conical, circular, approximately circular, and irregular shapes. The aforementioned pattern styles can be used alone or in combination.

[0058] The preheating and mechanical embossing conditions are adaptively adjusted according to the composition of the polymer film used. Generally speaking, the preheating wheel temperature can be 45°C to 82°C, specifically 58°C to 75°C, and more specifically 60°C to 75°C. The embossing wheel temperature can be 80°C to 150°C, specifically 90°C to 140°C, and more specifically 110°C to 130°C. The embossing wheel torque can be 0.3N·m (Newton.m) to 1.8N·m, specifically 0.75N·m to 1.55N·m, and more specifically 0.8N·m to 1.5N·m. The embossing wheel pressure can be 2kg / cm 2 (kg / cm2) to 50kg / cm 2 , specifically 10kg / cm 2 Up to 40kg / cm 2 , more specifically 15kg / cm 2 Up to 25kg / cm 2 .

[0059] Regarding the Vv properties of polymer films, the study found that the Vv value and the standard deviation of the Vv value can be adjusted by the torque of the pressing wheel or the temperature of the preheating wheel. The greater the torque of the pressing wheel, the greater the standard deviation of the Vv value of the polymer film, and the greater the Vv value. The higher the temperature of the preheating wheel, the smaller the standard deviation of the Vv value of the polymer film.

[0060] 2. Laminated glass

[0061] The polymer film of the present invention can be used to prepare laminated glass. Therefore, the present invention also provides a laminated glass, which comprises a first glass sheet, a second glass sheet, and an intermediate film located between the first glass sheet and the second glass sheet, wherein the intermediate film is provided by the polymer film as described above.

[0062] The first glass sheet and the second glass sheet may be the same or different, and may be any glass sheet commonly used to prepare laminated glass, such as float glass, tempered glass, wired glass, or ordinary flat glass, but the present invention is not limited thereto. In the following embodiments, float glass is used as the first glass sheet and the second glass sheet.

[0063] The laminated glass of the present invention can be prepared by the existing laminated glass preparation method in the relevant technical field. For example, the laminated glass can be prepared as follows: a polymer film is sandwiched between two glass sheets to obtain a laminate, the laminate is placed in a vacuum bag and evacuated at a temperature of 20°C to 30°C (vacuum degree> 500 mmHg) for at least 10 minutes, then the vacuum bag containing the laminate is placed in a heating furnace, and the temperature is slowly increased from 60°C to 130°C. After at least 30 minutes, the vacuum bag is taken out of the heating furnace to complete pre-pressing. Then, the pre-pressed laminate is placed in an autoclave and hot-pressed under high temperature and high pressure conditions for 100 minutes to 150 minutes to obtain laminated glass. Generally speaking, the high temperature and high pressure conditions can be a pressure of 10 bar to 15 bar and a temperature of 100°C to 150°C.

[0064] 3. Example

[0065] 3.1. Description of measurement method

[0066] The present invention is further illustrated by the following specific embodiments, wherein the measuring instruments and methods used are as follows:

[0067] [Measurement of Molecular Weight of Polyvinyl Acetal]

[0068] The molecular weight distribution of polyvinyl acetal was measured by gel permeation chromatography (GPC), wherein polyvinyl acetal was dissolved in tetrahydrofuran (THF), GPC analysis was performed under the following conditions, and the molecular weight was calculated as the ratio of the area corresponding to the polystyrene standard (Waters PS STD).

[0069] Device: Waters 1515 PUMP system

[0070] Detector: Waters 2414 RI

[0071] Elution conditions: 1.0 mL / min, THF

[0072] Column: Waters Styragel HR5 THF, Waters Styragel HR4 THF, Waters StyragelHR3 THF, Waters Styragel HR1 THF

[0073] [Measurement of acetalization degree of polyvinyl acetal]

[0074] The acetalization degree of polyvinyl acetal is measured in accordance with JIS K6728.

[0075] [Measurement of degree of acetylation of polyvinyl acetal]

[0076] The degree of acetylation of polyvinyl acetal is measured in accordance with JIS K6728.

[0077] [Measurement of hydroxyl content of polyvinyl acetal]

[0078] The hydroxyl content of polyvinyl acetal is measured according to JIS K6728.

[0079] [Measurement of glass transition temperature (Tg)]

[0080] The Tg of the polymer film was measured in a nitrogen atmosphere using a differential scanning calorimeter (model: TA DSC 25, purchased from TA Instruments). First, 7 mg of the polymer film was taken as a sample and placed on the sample stage of the differential scanning calorimeter, and the temperature was raised to 150°C at a heating rate of 10°C / min and then maintained at this temperature for 5 minutes. Then, the sample was equilibrated at -50°C and maintained at this temperature for 5 minutes, and then the temperature was raised to 100°C at a heating rate of 10°C / min to obtain a temperature versus heat flow curve (X axis is temperature, Y axis is heat flow), and the temperature corresponding to the midpoint of the glass transition was recorded as Tg.

[0081] [Bubble Residual Test]

[0082] The laminated glass was cut into 30 cm x 30 cm test samples. The test samples were placed vertically in an oven at 120°C for 14 days, and the test samples were observed with the naked eye to see if there were any bubbles remaining, wherein the bubbles refer to bubbles that exist between the glass and the polymer film at the edge of the laminated glass and are not in contact with the outside air. The evaluation criteria are as follows: if there are no bubbles remaining in the test sample, it is recorded as "◎", indicating that the bubble test result is excellent; if there are bubbles with a diameter of less than 0.5 mm remaining in the test sample and the number of bubbles is one, it is recorded as "○", indicating that the bubble test result is good; and if there are bubbles with a diameter of less than 0.5 mm remaining in the test sample and the number of bubbles is more than two, or there are bubbles with a diameter of more than 0.5 mm remaining in the test sample, it is recorded as "×", indicating that the bubble test result is not good.

[0083] [Measurement of void volume (Vv) and calculation of Vv value standard deviation]

[0084] First, the polymer film was cut into 3 cm × 3 cm test samples. At a temperature of 24 ± 3 ° C and a relative humidity of 63 ± 3%, the void volume (Vv) value of the polymer film at a loading area ratio of 10% was measured using a laser scanning confocal microscope (model: LEXT OLS5000-SAF, purchased from Olympus) according to the specification of ISO 25178-2:2012. The measurement conditions of the Vv value are as follows: the light source has a wavelength of 405 nm, the objective lens magnification is 100 times (MPLAPON-100xLEXT), the optical zoom is 50 times, the image area is 1500 μm × 1500 μm, the resolution is 1024 pixels × 1024 pixels, the operating condition is set to auto tilt removal, and no filter is used. In the obtained load area curve, the core void volume (Vvc) value at a load area ratio of 10% to 80% and the trough void volume (Vvv) value at a load area ratio of 80% can be obtained. The void volume (Vv) value is the sum of the trough void volume (Vvv) value and the core void volume (Vvc) value. The unit of the void volume (Vv) value is cubic micrometer / square micrometer. In the attached examples, the Vv value is obtained by averaging five Vv values. The sampling method is as follows Figure 1 As shown, a 30 cm × 30 cm polymer film is taken, and 3 cm × 3 cm test samples are cut from the four corners of the polymer film 1 cm away from the edge, and a 3 cm × 3 cm test sample is cut from the center of the polymer film to obtain a total of five test samples.

[0085] In addition, the standard deviation of the five Vv values ​​is calculated to obtain the standard deviation of the Vv value.

[0086] [Measurement of surface roughness Rz value]

[0087] The surface roughness Rz value of the polymer film was measured using a roughness tester (model: SE300, purchased from Kosaka Laboratory Ltd.) according to JIS B 0601 (1994). First, the polymer film was cut into a size of 8 cm × 30 cm as a test sample. The measurement conditions were set as follows: the vertical magnification was set to automatic, the horizontal magnification was set to 25 mm / λc, the cut-off distance was set to 2.5 mm (i.e., calculated every 2.5 mm), the evaluation length was seven times the cut-off distance, and the reference length was set to 17.5 mm, and the measurement direction was the machine direction.

[0088] [Evaluation of optical distortion]

[0089] First, prepare a 30 cm × 30 cm laminated glass as a test sample, and prepare a projector, a sample holder, and a white screen. Place the projector, sample holder, and white screen in a dark room, with the sample holder placed between the projector and the white screen. The distance between the projector and the sample holder and the distance between the sample holder and the white screen are both 1.5 meters. Place the test sample on the sample holder, and adjust the angle so that the test sample is tilted 15 degrees toward the projector relative to the axis vertical to the ground. Turn on the projector light source so that the light passes through the test sample and is projected onto the white screen. Observe whether there is a significant difference in brightness (i.e., continuous light and dark stripes) on the white screen. If not, it means that there are no filamentary stripes (light ripples) in the laminated glass, and record it as "no"; if yes, it means that there are filamentary stripes (light ripples) in the laminated glass, and record it as "yes".

[0090] [Light transmittance measurement]

[0091] The light transmittance of laminated glass is analyzed according to ASTM D1003. First, two flat glass sheets of 6 cm in length × 6 cm in width × 3 mm in thickness are taken, washed with water and blown dry. The two glass sheets are placed side by side, and the light transmittance of the two glass sheets is measured using a haze meter (model: NDH2000 Haze meter, purchased from Nippon Denshoku). Next, a polymer film is placed between the two glass sheets and heated by a hot press at 150°C and 2 kg / cm 2 Up to 3kg / cm 2 The laminated glass was obtained by hot pressing for 2 to 3 minutes under pressure, and then the surface of the glass was cleaned with alcohol. After that, the light transmittance of the laminated glass was measured using a haze meter.

[0092] [Glare evaluation]

[0093] After cutting the polymer film into 50 cm × 50 cm test samples, place the test samples on a 60 cm × 60 cm × 2 mm thick glass sheet. Place an incandescent lamp 30 cm below the glass sheet. Let 10 testers look directly at the film with their naked eyes 100 cm above the test sample and record whether the testers' eyes feel uncomfortable. The evaluation criteria are as follows: if the number of testers who feel uncomfortable in the eyes is 0 to 3, it means that the glare evaluation is good and is recorded as "A"; if the number of testers who feel uncomfortable in the eyes is 4 to 6, it means that the glare evaluation is ordinary and is recorded as "B"; if the number of testers who feel uncomfortable in the eyes is 7 to 10, it means that the glare evaluation is poor and is recorded as "C".

[0094] [Pummel adhesion test]

[0095] Three sheets of 30 cm × 15 cm laminated glass were prepared and placed at -20°C for 2 hours. Next, the laminated glass was placed on an automatic tapping machine for tapping adhesion test at a temperature of 20°C to 25°C, and tapped with a one-pound hammer starting from the end of the laminated glass and continuously tapped in the horizontal direction at intervals of about 12.7 mm to the center of the laminated glass. The tapped laminated glass is placed at room temperature for 30 minutes and then compared with a standard test piece. The laminated glass is evaluated according to the exposure degree of the polymer film of the tapped laminated glass, and the evaluation result is expressed as a numerical value from 0 to 9, wherein a numerical value of 0 indicates that the exposure degree of the polymer film is greater than 90%, a numerical value of 1 indicates that the exposure degree of the polymer film is less than 90% and greater than 80%, a numerical value of 2 indicates that the exposure degree of the polymer film is less than 80% and greater than 70%, a numerical value of 3 indicates that the exposure degree of the polymer film is less than 70% and greater than 60%, a numerical value of 4 indicates that the exposure degree of the polymer film is less than 60% and greater than 50%, a numerical value of 5 indicates that the exposure degree of the polymer film is less than 50% and greater than 40%, a numerical value of 6 indicates that the exposure degree of the polymer film is less than 40% and greater than 30%, a numerical value of 7 indicates that the exposure degree of the polymer film is less than 30% and greater than 20%, a numerical value of 8 indicates that the exposure degree of the polymer film is less than 20% and greater than 10%, and a numerical value of 9 indicates that the exposure degree of the polymer film is less than 10%. If the value is greater than 6, it means that the adhesion is too high, the glass is not easy to break and it is easy to cause injuries, so it is not suitable for automotive laminated glass. If the value is less than 4, it means that the adhesion is too poor, the glass is easy to break and spray out, and it is not suitable for automotive laminated glass. If the value is between 4 and 6, it means that the adhesion is moderate and it is suitable for automotive laminated glass.

[0096] 3.2. Preparation and property measurement of polymer films

[0097] First, 100 parts by weight of poly(vinyl butyral) (PVB, purchased from Changchun Petrochemical Co., Ltd.) and 40 parts by weight of a plasticizer (triethylene glycol bis(2-ethylhexanoate)) were mixed to obtain a mixture, which was kneaded at 120° C. at a rotation speed of 35 rpm for 15 minutes using a mixer, and then cooled to room temperature to obtain a polymer film composition. Next, the polymer film composition was placed in an extruder and extruded into a polymer film.

[0098] According to the parameter conditions shown in Table 1-1 and Table 1-2, the two surfaces of the polymer film were preheated and mechanically embossed to obtain the polymer films of Examples 1 to 11 and Comparative Examples 1 to 9. In addition to the parameter conditions shown in Table 1-1 and Table 1-2, the line speed of the polymer film passing between the embossing wheels was 18m / min. The molecular weight, acetal degree, acetylation degree and hydroxyl content ratio of the PVB used in Examples 1 to 11 and Comparative Examples 1 to 9 were measured according to the method described above, and the results are recorded in Table 2-1 to Table 2-2. In addition, the thickness, Tg, Vv, Vv standard deviation, and Rz of the polymer films of Examples 1 to 11 and Comparative Examples 1 to 9 were measured according to the measurement method described above, and the results are recorded in Table 2-3 to Table 2-4.

[0099] Table 1-1: Mechanical embossing parameters of polymer films of Examples 1 to 11

[0100]

[0101]

[0102] Table 1-2: Mechanical embossing parameter conditions of polymer films of Comparative Examples 1 to 9

[0103]

[0104] Table 2-1: Properties of PVB of Examples 1 to 11

[0105]

[0106]

[0107] Table 2-2: Properties of PVB of Comparative Examples 1 to 9

[0108]

[0109] Table 2-3: Properties of polymer films of Examples 1 to 11

[0110]

[0111]

[0112] Table 2-4: Properties of polymer films of Comparative Examples 1 to 9

[0113]

[0114] 3.3. Preparation and property evaluation of laminated glass

[0115] The polymer films of Examples 1 to 11 and Comparative Examples 1 to 9 were used to prepare laminated glass. First, two clean transparent float glass sheets (length 300 mm, width 300 mm, thickness 2 to 2.2 mm) were prepared. Then, the polymer films of Examples 1 to 11 and Comparative Examples 1 to 9 were sandwiched between the two transparent float glass sheets to obtain a laminate. The laminate was evacuated by a vacuum bag method to perform pre-compression. The operation of the vacuum bag method is as follows: the laminate was placed in a vacuum bag and evacuated at a temperature of 20° C. to 30° C. (vacuum degree> 500 mmHg) for at least 10 minutes. Then, the vacuum bag containing the laminate was placed in a heating furnace, first maintained at a temperature of 20° C. to 30° C. for 10 to 20 minutes, then heated to 60° C. to 130° C. and maintained for 15 to 45 minutes. After that, the vacuum bag was taken out of the heating furnace and cooled at room temperature. After cooling, the vacuum was released and the laminate was taken out. The pre-pressed laminate was placed in an autoclave for hot pressing at a pressure of 13 bar and a temperature of 135° C. for 120 minutes, and then cooled to room temperature to obtain a laminated glass.

[0116] According to the above methods, the laminated glasses of Examples 1 to 11 and Comparative Examples 1 to 9 were subjected to optical deformation evaluation, light transmittance measurement, glare evaluation, knock adhesion value test, and bubble residue test, and the results are recorded in Table 3-1 and Table 3-2.

[0117] Table 3-1: Properties of laminated glass of Examples 1 to 11

[0118]

[0119]

[0120] Table 3-2: Properties of laminated glasses of Comparative Examples 1 to 9

[0121]

[0122] As shown in Table 3-1, the laminated glass made from the polymer film of the present invention obtains satisfactory results in the optical distortion evaluation, glare evaluation, knock adhesion value test and bubble residue test and has a light transmittance of at least 87%. Examples 1 to 11 show that when the standard deviation of the Vv value on the surface of the polymer film is within the specified range, the laminated glass obtained has the advantages of optical distortion, no glare, and good transmittance. In particular, Examples 1 to 10 further show that when the standard deviation of the Vv value on the surface of the polymer film is within the specified range, and the Vv value and Rz value are both within the preferred range, the laminated glass obtained has the advantages of no optical distortion, no glare, and good transmittance, and has a suitable knock adhesion value and no bubble residue.

[0123] In contrast, as shown in Table 3-2, the laminated glass made from the polymer film not belonging to the present invention cannot simultaneously possess the advantages of no optical distortion, no glare, and good transmittance. Specifically, the comparison of Examples 1 to 9 shows that if the standard deviation of the Vv value on the surface of the polymer film is not within the specified range, even if the Vv value and the Rz value are within the preferred range, the laminated glass cannot simultaneously possess the advantages of no optical distortion, no glare, and good transmittance.

[0124] The above embodiments are only used to illustrate the principle and efficacy of the present invention and to describe the technical features of the present invention, and are not intended to limit the scope of protection of the present invention. Any changes or arrangements that can be easily completed by any person skilled in the art without violating the technical principle and spirit of the present invention are within the scope of the present invention.

Claims

1. A polymer film, characterized in that The polymer film has a first surface and a second surface, wherein the standard deviation of the void volume (Vv) value of the first surface when the material ratio is 10% is 0.5 cubic micrometers / square micrometers (μm 3 / μm 2 ) to 2.5 cubic microns / square microns, and wherein the load area ratio and the void volume are defined according to ISO 25178-2:2012, wherein the polymer film comprises polyvinylacetal.

2. The polymer film according to claim 1, characterized in that The void volume value of the first surface when the loading area ratio is 10% is 2 cubic micrometers / square micrometer to 35 cubic micrometers / square micrometer.

3. The polymer film according to claim 1, characterized in that The first surface has a surface roughness Rz value of 15 μm to 55 μm, the Rz value being measured in accordance with JIS B 0601 (1994).

4. The polymer film according to claim 1, characterized in that The standard deviation of the void volume value of the second surface at a loading area ratio of 10% is 0.5 cubic micrometers / square micrometer to 2.5 cubic micrometers / square micrometer.

5. The polymer film according to claim 4, characterized in that The void volume value of the second surface when the loading area ratio is 10% is 2 cubic micrometers / square micrometer to 35 cubic micrometers / square micrometer.

6. The polymer film according to claim 4, characterized in that The second surface has a surface roughness Rz value of 15 μm to 55 μm, the Rz value being measured in accordance with JIS B 0601 (1994).

7. The polymer film according to claim 1, characterized in that The polyvinyl acetal is poly(vinyl butyral).

8. The polymer film according to any one of claims 1 to 6, characterized in that It has a thickness of 0.1 mm to 2.5 mm.

9. A laminated glass, characterized in that: The invention comprises a first glass sheet, a second glass sheet, and an intermediate film located between the first glass sheet and the second glass sheet, wherein the intermediate film is provided by the polymer film according to any one of claims 1 to 8.