A method for preparing and purifying calcium sulfate in nitric acid solution

By adding a decalcifying agent and a precipitation-promoting agent to the nitric acid solution, the problem of difficulty in removing Ca2+ from solutions with high nitric acid content by freezing is solved, efficient calcium sulfate purification is achieved, and high-purity calcium sulfate and low impurity content are obtained. Calcium sulfate finished product.

CN116002740BActive Publication Date: 2024-10-18GUIZHOU BATIAN ECOTYPIC ENG CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211739065.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-18
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

When dealing with high nitric acid content and multi-metal ions, the existing freezing method is difficult to effectively remove Ca2+ from the nitrate phosphate rock decomposition solution, and it is difficult to obtain high-purity calcium sulfate by-products.

Method used

Add a decalcifying agent (such as concentrated sulfuric acid) and a sedimentation-promoting agent (such as a mixed solution of polyacrylamide, sodium polyacrylate, carboxymethylcellulose, and polyethyleneimine) to the nitric acid solution containing calcium ions. After incubation at 80°C, the mixture is cooled and filtered to obtain insoluble matter, which is then dried and washed to obtain purified calcium sulfate.

Benefits of technology

The sedimentation speed and removal rate of calcium ions are improved, reaching a Ca2+ removal rate of more than 98%. The obtained calcium sulfate is of high purity, with a total impurity content of less than 0.5% and trace amounts of other metal elements remaining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004032838780000071
    Figure BDA0004032838780000071
Patent Text Reader

Abstract

The present invention discloses a method for preparing and purifying calcium sulfate in a nitric acid solution, and relates to the technical field of phosphate ore processing; the method for preparing and purifying calcium sulfate in a nitric acid solution described in the present application comprises the following steps: adding a decalcifying agent and a precipitation promoting agent to a nitric acid solution containing calcium ions, keeping the temperature at 60 to 80°C for 10 to 15 minutes, cooling the temperature to 5 to 10°C after the insulation is completed, filtering to obtain insoluble matter; and post-treating the insoluble matter to obtain purified calcium sulfate. The method for preparing and purifying calcium sulfate in a nitric acid solution described in the present application improves the precipitation of calcium ions by adding a precipitation promoting agent, and reduces the acidity of calcium sulfate by crushing and washing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phosphate ore processing, and in particular to a method for preparing and purifying calcium sulfate in a nitric acid solution. Background Art

[0002] As early as the 1930s, the process of using nitric acid to decompose phosphate rock was studied and a theoretical phase diagram was established. Phosphate rock-nitric acid decomposition liquid is currently mainly used to make nitrophosphate fertilizer. However, since it contains a large amount of calcium ions, it greatly affects the water solubility of nitrophosphate fertilizer products, so calcium removal is necessary. The more calcium ions are removed, the higher the water solubility of the product P2O5.

[0003] At present, the methods for processing phosphate rock-nitric acid decomposition liquid in the world can be summarized as carbonization method, mixed acid method, sulfate method and freezing method according to different calcium removal methods; the principle of calcium removal by freezing method is that when the temperature of phosphate rock-nitric acid decomposition liquid is lowered, the solution will form a suspension containing Ca(NO3)2·4H2O crystals, and the purpose of calcium removal is achieved through solid-liquid separation.

[0004] Although most of the Ca in the solution can be removed by freezing, 2+ However, when the nitric acid content in the solution is high and the content of other metal ions is high, the freezing method cannot effectively remove Ca 2+ , the frozen decalcification liquid needs to be further processed. At present, there is no better process to deal with the decalcification liquid. When the nitric acid content in the solution is high and the content of other metal ions is high, it can better remove Ca 2+ , and a by-product with higher purity of calcium sulfate can be obtained.

[0005] Calcium sulfate has excellent physical, chemical and mechanical properties such as high temperature resistance, acid and alkali resistance, chemical corrosion resistance, good electrical insulation, high strength, good toughness and compatibility, and easy surface treatment. As a new functional material, it is widely used in the manufacturing of plastics, rubber, adhesives, friction materials, coatings, paints, thermal insulation materials, lightweight building materials and other products.

[0006] Therefore, we propose a method for preparing and purifying calcium sulfate in nitric acid solution. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for preparing and purifying calcium sulfate in a nitric acid solution, comprising the following steps:

[0008] A method for preparing and purifying calcium sulfate in a nitric acid solution comprises the following steps:

[0009] A decalcifying agent and a precipitation promoting agent are added to a nitric acid solution containing calcium ions, and the solution is kept warm at 60-80°C for 10-15 minutes. After the warming is completed, the solution is cooled to 5-10°C and filtered to obtain an insoluble substance. The insoluble substance is post-treated to obtain purified calcium sulfate.

[0010] Preferably, the nitric acid solution containing calcium ions is prepared according to the following steps:

[0011] S1, acid hydrolysis separation: add phosphate concentrate and nitric acid with a mass concentration of 62% into the acid hydrolysis tank, the acid-ore ratio of nitric acid to phosphate concentrate is 1.05-1.1:1, the acid hydrolysis temperature is 60-65°C, the residence time is 1.5-2.0 hours, and after the reaction is completed, the acid hydrolyzate is pumped into a filter press for filtration and washing, and the discharged acid hydrolyzate is sent to frozen crystallization for decalcification;

[0012] S2, freezing separation: the discharged acid hydrolysis liquid is pumped into a crystallizer, cooled to -5°C to -8°C under stirring to obtain a frozen crystal slurry, and calcium nitrate crystals [Ca(NO3)2·4H2O] in the frozen crystal slurry are precipitated; the frozen crystal slurry is sent to a double drum filter for filtration to obtain a filter cake and an acid hydrolysis filtrate, the filter cake is washed with a nitric acid solution with a mass concentration of 62% and water in turn, and the washed acid obtained by washing is returned to the acid hydrolysis separation process for use; the acid hydrolysis filtrate obtained in this step is a nitric acid solution containing calcium ions.

[0013] Preferably, the calcium ion content in the nitric acid solution is 10-70 g / L, and the weight content of nitric acid in the nitric acid solution is 10-200 g / L. The specific weight content of calcium ions in the nitric acid solution is 10g / L, 20g / L, 30g / L, 40g / L, 50g / L, 60g / L or 70g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable; the specific weight content of nitric acid in the nitric acid solution is 10-200g / L, which can be 10g / L, 11g / L, 12g / L, 13g / L, 20g / L, 20g / L, 25g / L, 29g / L, 30g / L, 40g / L, 50g / L, 56g / L, 60g / L, 70g / L, 80g / L, 90g / L, 100g / L, 120g / L, 130g / L, 180g / L or 200g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0014] Preferably, the decalcifying agent is concentrated sulfuric acid, and the molar amount of the concentrated sulfuric acid is 1.1 to 1.5 times the molar amount of calcium ions. The specific molar amount of concentrated sulfuric acid is the molar amount of calcium ions, which can be 1.1, 1.2, 1.3, 1.4 or 1.5, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0015] Preferably, the precipitation promoting agent is a mixed solution composed of polyacrylamide, sodium polyacrylate, carboxymethyl cellulose and polyethylene imine.

[0016] More preferably, 1L of the precipitation-promoting agent includes the following raw materials by weight:

[0017] Polyacrylamide 0.2-0.3g, sodium polyacrylate 0.2-0.3g, carboxymethyl cellulose 0.2-0.3g, polyethylene imine 0.1-0.2g. Specifically, 1L of the sedimentation promoter includes the following weights of raw materials: polyacrylamide 0.2g, sodium polyacrylate 0.2g, carboxymethyl cellulose 0.2g, polyethylene imine 0.1g, and the balance is water; or 1L of the sedimentation promoter includes the following weights of raw materials: polyacrylamide 0.3g, sodium polyacrylate 0.3g, carboxymethyl cellulose 0.3g, polyethylene imine 0.2g, and the balance is water; or 1L of the sedimentation promoter includes the following weights of raw materials: polyacrylamide 0.25g, sodium polyacrylate 0.25g, carboxymethyl cellulose 0.25g, polyethylene imine 0.15g, and the balance is water; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable. The sedimentation promoter selected in the present application has good flocculation properties, can reduce the friction resistance between liquids, and accelerate the sedimentation of calcium sulfate by the decalcifying agent.

[0018] More preferably, every 1m 3 The nitric acid solution uses 0.5 to 0.6 L of the precipitation promoter. 3 The nitric acid solution using the precipitation promoter can be 0.5L or 0.6L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Preferably, the insoluble matter is post-treated, including: the insoluble matter is post-treated, including: first drying the insoluble matter at 90-100° C., crushing it through a 50-100 mesh sieve to obtain a dried matter after drying, then washing it with alcohol 2-3 times, and drying it at 70-80° C. to obtain purified calcium sulfate.

[0020] More preferably, the alcohol is industrial alcohol, wherein the weight of the industrial alcohol is 3 to 5 times that of the dry matter, and the specific weight of the industrial alcohol and the weight of the dry matter can be 3 times, 4 times or 5 times, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0021] The beneficial effects of this application are:

[0022] 1. The addition of decalcification agent and precipitation promoter can increase the sedimentation rate and total sedimentation weight of calcium ions; after adding decalcification agent and precipitation promoter at the same time, the Ca 2+ The removal rate reaches over 98%.

[0023] 2. The calcium sulfate obtained by post-processing the insoluble matter has high purity, a total amount of impurities <0.5%, and only trace amounts of other metal elements remain. DETAILED DESCRIPTION

[0024] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0025] As used herein, "and / or" includes the term of any and all combinations of one or more associated listed items. The terms used herein are only used to describe specific embodiments and are not intended to limit the present invention. As used herein, the singular forms "a", "an", "an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise. It is further understood that "including", when used in this specification, specifies the stated features, integers, steps, operations, elements and / or compositions, but does not exclude the existence or addition of one or more other features, integers, steps, operations, elements, compositions and / or combinations thereof.

[0026] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. It is further understood that terms, such as defined in commonly used dictionaries, are interpreted in accordance with their meanings in the context of the relevant art and are not in an idealized or overly formal sense unless explicitly so defined herein.

[0027] The exemplary invention described herein may appropriately lack any one or more element limitations that are not specifically disclosed herein. Therefore, the terms "comprise", "include", "contain", etc. should be understood broadly and non-restrictively. In addition, the terminology used herein is used as a description, not a limitation, and it is unintentional to use these terminology expressions that do not include any equivalent characteristics, but only describe some of their characteristics, but various modifications are possible within the scope of the present invention according to the rights. Therefore, although the present invention has been specifically disclosed by preferred embodiments and optional features, the modifications disclosed herein to embody the changes of the present invention may be recorded by those skilled in the art, and such modifications and changes will be considered to be within the scope of the present invention.

[0028] The raw materials or reagents used in the embodiments of the present invention and the comparative examples are all purchased from mainstream manufacturers in the market. The manufacturer is not specified or the concentration is not specified. They are all analytically pure raw materials or reagents that can be routinely obtained. As long as the expected effect can be achieved, there is no particular restriction. The reaction flask and rotary evaporator and other instruments and equipment used in the present embodiment are all purchased from major manufacturers in the market. As long as the expected effect can be achieved, there is no particular restriction. If specific techniques or conditions are not specified in the present embodiment, the techniques or conditions described in the literature in this area or according to the product specification are carried out.

[0029] In the present invention, the nitric acid solution containing calcium ions comes from the acid hydrolysis separation and freezing separation process of phosphate concentrate; the specific process is:

[0030] Acid hydrolysis separation: The acid hydrolysis of phosphate concentrate utilizes the existing nitric acid phosphate fertilizer device. Phosphate concentrate and nitric acid (and washing acid) with a mass concentration of 62% are added into the acid hydrolysis tank. The acid-ore ratio (weight) of nitric acid to phosphate concentrate is 1.05-1.1:1. The acid hydrolysis temperature is 60-65°C and the residence time is 1.5-2 hours. After the reaction is completed, the acid hydrolyzate is pumped into a filter press for filtration and washing. The discharged filter cake is used to produce soil conditioner. The discharged acid hydrolyzate is sent for freezing crystallization and decalcification.

[0031] Freeze separation: pump the acid hydrolysis liquid into a crystallizer and cool it to -5°C under stirring to obtain a frozen crystal slurry, so that calcium nitrate crystals [Ca(NO3)2·4H2O] in the frozen crystal slurry are precipitated; send the frozen crystal slurry to a double drum filter for filtration to obtain a filter cake and an acid hydrolysis filtrate, and wash the filter cake with a nitric acid solution with a mass concentration of 62% and water in turn, and return the washed acid (the mass concentration of nitric acid is 30-45%) obtained by washing to the acid hydrolysis separation process for use.

[0032] After freezing separation, the calcium content in the acid hydrolysis filtrate is largely removed, and the decalcification rate is between 70% and 80%. The acid hydrolysis filtrate still has a high residual Ca 2+ The acid hydrolysis filtrate obtained at this time is a nitric acid solution containing calcium ions. 2+ The content is 10-70g / L, the nitric acid content is 10g / L-200g / L, and the other metal content is 1mg / L-10mg / L.

[0033] Therefore, if the nitric acid solution containing calcium ions is not removed, 2+ As well as other metals, it will affect the normal progress of the subsequent neutralization and slag removal process.

[0034] Example 1

[0035] A method for preparing and purifying calcium sulfate using the above nitric acid solution comprises the following steps:

[0036] Concentrated sulfuric acid and a precipitation promoter are added to a nitric acid solution containing calcium ions, and the solution is kept warm at 60°C for 10 minutes. After the keeping warm is completed, the solution is cooled to 5°C and filtered to obtain an insoluble substance and a filtrate. The insoluble substance is dried (dried at 90-100°C, with a moisture content of ≤10%), crushed and sieved through a 50-100 mesh sieve after drying, and then washed twice with industrial alcohol 3 times the weight of the dried substance, and dried (dried at 70-80°C, with a moisture content of ≤1%) to obtain a purified calcium sulfate product.

[0037] The feed ratio is: the molar amount of concentrated sulfuric acid is 1.1 times the molar amount of calcium ions; 3 The nitric acid solution uses 0.5L of the precipitation-promoting agent;

[0038] 1L of sedimentation accelerator includes the following raw materials by weight:

[0039] Polyacrylamide 0.2g, sodium polyacrylate 0.2g, carboxymethyl cellulose 0.2g, polyethyleneimine 0.1g, the balance is water;

[0040] Example 2

[0041] A method for preparing and purifying calcium sulfate using the above nitric acid solution comprises the following steps:

[0042] Concentrated sulfuric acid and a precipitation promoter are added to a nitric acid solution containing calcium ions, and the solution is kept warm at 80°C for 15 minutes. After the keeping warm is completed, the solution is cooled to 10°C and filtered to obtain an insoluble substance and a filtrate. The insoluble substance is dried (dried at 90-100°C, with a moisture content of ≤10%), crushed and sieved through a 50-100 mesh sieve after drying, and then washed three times with industrial alcohol 5 times the weight of the dried substance, and dried (dried at 70-80°C, with a moisture content of ≤1%) to obtain a purified calcium sulfate product.

[0043] The feed ratio is: the molar amount of concentrated sulfuric acid is 1.5 times the molar amount of calcium ions; 3 The nitric acid solution uses 0.6L of the precipitation-promoting agent;

[0044] 1L of sedimentation accelerator includes the following raw materials by weight:

[0045] Polyacrylamide 0.3g, sodium polyacrylate 0.3g, carboxymethyl cellulose 0.3g, polyethyleneimine 0.2g, and the balance is water;

[0046] Example 3

[0047] A method for preparing and purifying calcium sulfate using the above nitric acid solution comprises the following steps:

[0048] Concentrated sulfuric acid and a precipitation promoter are added to a nitric acid solution containing calcium ions, and the solution is kept warm at 70°C for 13 minutes. After the keeping warm is completed, the solution is cooled to 8°C and filtered to obtain an insoluble substance and a filtrate. The insoluble substance is dried (dried at 90-100°C, with a moisture content of ≤10%), crushed and sieved through a 50-100 mesh sieve after drying, and then washed twice with industrial alcohol 4 times the weight of the dried substance, and dried (dried at 70-80°C, with a moisture content of ≤1%) to obtain a purified calcium sulfate product.

[0049] The feed ratio is: the molar amount of concentrated sulfuric acid is 1.3 times the molar amount of calcium ions; 3 The nitric acid solution uses 0.55L of the precipitation-promoting agent;

[0050] 1L of sedimentation accelerator includes the following raw materials by weight:

[0051] Polyacrylamide 0.25g, sodium polyacrylate 0.25g, carboxymethyl cellulose 0.25g, polyethyleneimine 0.15g, and the balance is water;

[0052] Comparative Example 1

[0053] The concentrated sulfuric acid in Example 1 was not added, and the other conditions were the same as those in Example 1;

[0054] Comparative Example 2

[0055] The precipitation-promoting agent in Example 1 was not added, and the other conditions were the same as those in Example 1;

[0056] Comparative Example 3

[0057] The precipitation promoting agent and concentrated sulfuric acid in Example 1 were not added, and the other conditions were the same as those in Example 1;

[0058] In the embodiment, the nitric acid solution used is 1L, Ca 2+ When the content is 0.5 g / L, the nitric acid content is 150 g / L, and the other metal content is 8 mg / L, the purity and content of the calcium sulfate products obtained in Examples 1 to 3 and Comparative Examples 1 to 3, as well as the impurity content in the filtrate are investigated. The corresponding results are summarized in the following Table 1.

[0059] Table 1

[0060]

[0061]

[0062] From Table 1, it can be seen that the method described in Example 1 to Example 3 obtains a finished calcium sulfate product, and the theoretical yield reaches 95.59-99.51%, and the impurity content is only 0.15-0.31%, with high purity; while in Comparative Example 1, when only a precipitation promoting agent is added, the precipitation promoting agent is directly dissolved in the decalcification solution, and the nitric acid solution is subjected to heat preservation and cooling, and no precipitation is produced; while in Comparative Example 2, only concentrated sulfuric acid is added to obtain a finished calcium sulfate product, and the theoretical yield reaches 73.04%, and the impurity content is 3.5%, and about 30% of calcium remains in the filtrate, which cannot be recovered. Comparative Example 3 is a blank control, and no precipitation promoting agent and concentrated sulfuric acid are added, and no precipitation is produced after heat preservation and cooling.

[0063] In the specific experimental process, it was found that in Examples 1 to 3, after cooling, filtration was performed at a relatively fast speed, and the filter cake could be drained in generally 15 minutes; while in Comparative Example 2, under the same vacuum pressure and device conditions, the filtration speed was slow, and the filter cake could not be drained. The obtained insoluble matter (wet filter cake) was dried before the next step of operation was performed;

[0064] The above embodiments and specific scheme descriptions do not limit the patent protection scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing and purifying calcium sulfate in a nitric acid solution, characterized in that: The steps include: Adding a decalcifying agent and a precipitation promoting agent to a nitric acid solution containing calcium ions, keeping the solution at 60-80°C for 10-15 minutes, cooling the solution to 5-10°C after the solution is kept warm, filtering the solution to obtain an insoluble substance; post-treating the insoluble substance to obtain purified calcium sulfate; The decalcifying agent is concentrated sulfuric acid, and the molar amount of the concentrated sulfuric acid is 1.1 to 1.5 times the molar amount of calcium ions; The precipitation promoting agent is a mixed solution composed of polyacrylamide, sodium polyacrylate, carboxymethyl cellulose and polyethylene imine; 1L of sedimentation accelerator includes the following raw materials by weight: Polyacrylamide 0.2~0.3g, sodium polyacrylate 0.2~0.3g, carboxymethyl cellulose 0.2~0.3g, polyethyleneimine 0.1~0.2g; Every 1m 3 The nitric acid solution containing calcium ions uses 0.5-0.6 L of the precipitation-promoting agent; The nitric acid solution containing calcium ions is prepared according to the following steps: S1, acid hydrolysis separation: add phosphate concentrate and nitric acid solution with a mass concentration of 62% into the acid hydrolysis tank, the acid-ore ratio of nitric acid to phosphate concentrate is 1.05-1.1:1, the acid hydrolysis temperature is 60-65°C, the residence time is 1.5-2.0 hours, and after the reaction is completed, the acid hydrolyzed liquid is pumped into the filter press for filtration and washing, and the discharged acid hydrolyzed liquid is sent to frozen crystallization for decalcification; S2, freezing separation: the discharged acid hydrolysis liquid is pumped into a crystallizer, cooled to -5°C to -8°C under stirring to obtain a frozen crystal slurry, and calcium nitrate in the frozen crystal slurry is crystallized and precipitated, and the crystals are precipitated as Ca(NO3)2·4H2O; the frozen crystal slurry is sent to a double drum filter for filtration to obtain a filter cake and an acid hydrolysis filtrate, the filter cake is washed with a nitric acid solution with a mass concentration of 62% and water in turn, and the washed acid obtained by washing is returned to the acid hydrolysis separation process for use; the acid hydrolysis filtrate obtained in this step is a nitric acid solution containing calcium ions.

2. The method for preparing and purifying calcium sulfate from a nitric acid solution according to claim 1, characterized in that: The calcium ion content of the nitric acid solution containing calcium ions is 10-70 g / L, and the nitric acid content of the nitric acid solution containing calcium ions is 10-200 g / L.

3. The method for preparing and purifying calcium sulfate from a nitric acid solution according to claim 1, characterized in that: The insoluble matter is post-processed, including: first drying the insoluble matter at 90-100° C., crushing the dried matter through a 50-100 mesh sieve to obtain a dried matter, washing the dried matter with alcohol 2-3 times, and drying the dried matter at 70-80° C. to obtain purified calcium sulfate.

4. The method for preparing and purifying calcium sulfate from a nitric acid solution according to claim 3, characterized in that: The alcohol is industrial alcohol.

5. The method for preparing and purifying calcium sulfate from a nitric acid solution according to claim 4, characterized in that: The weight of the industrial alcohol is 3 to 5 times that of the dry substance.

Citation Information

Patent Citations

  • Method for preparing industrial-grade phosphoric acid by decomposing mid-low-grade phosphorite with nitric acid

    CN102718200A

  • Method for co-production of chemical synthetic fertilizer by industrial calcium products

    CN106517293A