Impact-resistant silicone pressure-sensitive adhesive and preparation method thereof
By using a combination of MQ silicone resin and STF liquid in silicone pressure-sensitive adhesive, a three-dimensional network structure is formed to fix the nanoparticles, which solves the problem of insufficient impact resistance of traditional silicone pressure-sensitive adhesive and achieves high impact strength and stability. , and maintains bonding properties, suitable for high-temperature environments in the aerospace industry.
Patent Information
- Application Number
- CN202310074740.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-07
AI Technical Summary
Traditional silicone pressure-sensitive adhesives are difficult to meet the impact resistance requirements in the aerospace industry. When existing technologies improve impact resistance, they are often accompanied by problems such as reduced bonding performance or low production efficiency.
Using a combination of MQ silicone resin, STF liquid, cross-linking agent, inhibitor and platinum catalyst, the nanoparticles are fixed through a three-dimensional network structure, and the collision of nanoparticles is used to absorb impact energy, improve impact resistance and maintain bonding performance.
It achieves high impact strength and stability of impact-resistant silicone pressure-sensitive adhesive, avoids the reduction of bonding performance, and maintains good adhesion and heat resistance at high temperatures.
Smart Images

Figure BDA0004065722230000021 
Figure BDA0004065722230000031 
Figure BDA0004065722230000041
Abstract
Description
Technical Field
[0001] The invention relates to the field of pressure-sensitive adhesives, and in particular to an impact-resistant organic silicon pressure-sensitive adhesive and a preparation method thereof. Background Art
[0002] Silicone materials, such as silicone rubber, silicone resin, silicone grease, etc., have many excellent properties and are supporting materials for my country's aerospace industry. Spacecraft must undergo the test of orbital environments such as high and low temperatures, high vacuum, and low thermal shock. Therefore, adhesives are required to have not only a certain bonding strength, but also good temperature resistance and impact resistance. As a special pressure-sensitive adhesive material, silicone pressure-sensitive adhesive has the advantages of good adhesion to both high-energy and low-energy surfaces, corrosion resistance, high temperature resistance, and non-irritation. However, traditional silicone pressure-sensitive adhesives are difficult to meet the impact resistance requirements in aerospace industry production.
[0003] The patent with publication number CN111440572A discloses an impact-resistant polyacrylate pressure-sensitive adhesive layer in which a grafted anhydride-modified block copolymer is used as a crosslinking agent. The pressure-sensitive adhesive prepared by this method needs to add a certain proportion of anhydride-modified block copolymer to promote the crosslinking reaction. Since the block copolymer easily reacts with epoxy groups, it needs to be ready for use when used. The addition ratio and order need to be strictly controlled, and an online filtration process is used. In order to ensure that the anhydride fully reacts to crosslink the block copolymer into the colloid, a high temperature section of 120-130°C needs to be set for 30-55 seconds, which limits its application range to a certain extent.
[0004] The patent with publication number CN107987761A discloses a hot melt pressure-sensitive adhesive and its preparation method and application. By adding diblock SDS thermoplastic elastomer and SIS thermoplastic elastomer, the final product is obtained by mixing it with cyclohexane oil, polyisobutylene, etc. in a certain proportion and stirring and melting it. In the adhesive, the tackifying resin and the diblock SDS thermoplastic elastomer and SIS thermoplastic elastomer are very easy to phase separate. The pressure-sensitive adhesive tape prepared by this hot melt pressure-sensitive adhesive has a large difference in polarity between the diblock SDS thermoplastic elastomer, SIS thermoplastic elastomer and the tackifying resin component over time, resulting in the occurrence of two-phase separation, so that the thermoplastic elastomer is precipitated from the pressure-sensitive adhesive, reducing the bonding performance of the product. In severe cases, the pressure-sensitive adhesive product can be rendered ineffective. In addition, the reaction temperature in the preparation process of the hot melt pressure-sensitive adhesive is high (150°C), and the subsequent products require vacuum degassing treatment.
[0005] The patent with publication number CN114214002A discloses an acrylic hot melt pressure-sensitive adhesive and a preparation method thereof. A zinc stearate solution is used as an activator, and a certain proportion of plasticizer and filler are added to prepare an impact-resistant pressure-sensitive adhesive. After adding plasticizer and softener, the mixing time can be shortened, and the tear strength, waterproofness, stability and adhesion performance of the pressure-sensitive adhesive can be improved. By adding a certain proportion of filler, it has super heat resistance, adhesion and impact resistance. However, the added fillers such as titanium dioxide, mica powder and asbestos powder are not well dispersed in the adhesive, and agglomeration is prone to occur, and the viscosity will also be affected to a certain extent.
[0006] In addition to the above methods, improving the impact resistance of pressure-sensitive adhesives by cross-linking the carbon-carbon double bonds of polyacrylates and rubbers with peroxides is also a new solution. However, the reaction requires a higher temperature, and sufficient high temperature time must be ensured during the preparation of the pressure-sensitive tape. It is difficult to balance production efficiency and energy consumption, and it is easy to cause excessive cross-linking, resulting in a decrease in the bonding performance of the pressure-sensitive adhesive.
[0007] Therefore, it is very important to develop an impact-resistant silicone pressure-sensitive adhesive to expand the application of silicone pressure-sensitive adhesive in the aerospace field. Summary of the invention
[0008] In order to overcome the deficiencies of the prior art, the first object of the present invention is to provide an impact-resistant silicone pressure-sensitive adhesive, comprising the following raw materials in parts by weight:
[0009]
[0010]
[0011] Preferably, the M / Q value of the MQ silicone resin is 0.6-0.9.
[0012] Preferably, the crosslinking agent is at least one of benzoyl peroxide, aminosilane, and 2,4-dichlorobenzoyl peroxide.
[0013] Preferably, the inhibitor is at least one of 1-ethynylcyclohexanol and methylbutynol.
[0014] Preferably, the solvent is at least one of ethyl acetate, toluene and xylene.
[0015] Preferably, the platinum catalyst is at least one of a Speier catalyst and a Karstedt catalyst.
[0016] The second object of the present invention is to provide a method for preparing the impact-resistant silicone pressure-sensitive adhesive as described above, comprising the following steps:
[0017] Step 1: Dissolve the weighed methyl vinyl silicone rubber in the solvent and stir evenly;
[0018] Step 2: Add the weighed MQ silicone resin and STF liquid into the mixture under stirring conditions, and stir and disperse the mixture under high-speed ultrasonic stirring for 10 minutes to prepare a stable solution;
[0019] Step 3: Add the weighed cross-linking agent, inhibitor and platinum catalyst into the reaction kettle and stir evenly to obtain the silicone pressure-sensitive adhesive.
[0020] Preferably, the preparation method of MQ silicone resin in step 2 is:
[0021] Accurately weigh ethanol and hydrochloric acid and stir them thoroughly for 10 minutes to dissolve them in deionized water; weigh a certain amount of ethyl orthosilicate and hexamethyldisiloxane and stir them thoroughly; add each monomer into the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes; heat each solution to 80°C and react for 1 hour; extract, layer, wash with water until neutral, and distill under reduced pressure to obtain MQ resin.
[0022] Compared with the prior art, the beneficial effect of the present invention is as follows: the present invention provides an impact-resistant organic silicone pressure-sensitive adhesive, comprising the following raw materials by weight: 20-60 parts of MQ silicone resin; 20-40 parts of methyl vinyl silicone rubber; 0.2-0.4 parts of cross-linking agent; 0.2-4 parts of platinum catalyst; 0.02-0.04 parts of inhibitor; 1-5 parts of STF liquid; 30-40 parts of solvent. The present invention also relates to a preparation method thereof. The impact-resistant organic silicone pressure-sensitive adhesive prepared in this way has the following advantages:
[0023] 1. The impact resistance of the pressure-sensitive adhesive is achieved by utilizing the nanoparticles in the STF liquid to collide with each other, aggregate, absorb and dissipate the impact energy when subjected to external impact.
[0024] 2. Improve the impact resistance of pressure-sensitive adhesive without weakening the peeling performance.
[0025] 3. The three-dimensional network structure of the silicone pressure-sensitive adhesive is used to fix the nanoparticles, solving the dispersion problem. In addition, the low-viscosity polymer solution in the STF solution, such as polyethylene glycol, can improve the adhesion on the substrate and avoid debonding.
[0026] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention. The specific implementation of the present invention is given in detail by the following embodiments. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.
[0028] During the use of acrylic pressure-sensitive adhesive, small molecules will migrate to the surface, thus affecting the overall application effect. Moreover, the temperature resistance of acrylic pressure-sensitive adhesive is also significantly lower than that of silicone pressure-sensitive adhesive. In order to overcome the shortcomings of existing pressure-sensitive adhesives, the present invention relates to an impact-resistant silicone pressure-sensitive adhesive, comprising the following raw materials in parts by weight:
[0029]
[0030] In some embodiments, the M / Q value of the MQ silicone resin is 0.6-0.9. Since the STF liquid is a non-Newtonian fluid and is in the form of a suspension in a static state, the nanoparticles are dispersed in a low-viscosity polymer liquid to obtain a high-solid content suspension system with fluidity and a certain viscosity, but the nanoparticles are easy to agglomerate, resulting in the STF suspension system being easy to settle and unstable. By utilizing the three-dimensional network skeleton structure of the cross-linked system of the silicone pressure-sensitive adhesive, nanoparticles, such as carbon nanotubes and nano-silicon dioxide, can be fixed in the three-dimensional network skeleton structure, which can improve the stability of the STF liquid and avoid the sedimentation of the nanoparticles. In addition, when the STF liquid-silicone pressure-sensitive adhesive is subjected to external impact, the nanoparticles collide with each other, aggregate, and absorb and dissipate the impact energy to achieve the impact resistance of the pressure-sensitive adhesive, while improving the temperature resistance of the silicone pressure-sensitive adhesive. Therefore, the STF liquid can be used to modify the silicone pressure-sensitive adhesive to improve the impact resistance of the silicone pressure-sensitive adhesive.
[0031] In some embodiments, in order to meet the requirements of heat resistance and adhesion holding force of the pressure-sensitive adhesive at high temperature, the cross-linking agent is at least one of benzoyl peroxide, aminosilane, and 2,4-dichlorobenzoyl peroxide.
[0032] In some embodiments, in order to prolong the operation time, the inhibitor is at least one of 1-ethynylcyclohexanol and methylbutynol.
[0033] In some embodiments, in order to ensure the solubility of each raw material, the solvent is at least one of ethyl acetate, toluene, and xylene.
[0034] In some embodiments, in order to improve the reaction efficiency, the platinum catalyst is at least one of a Speier catalyst and a Karstedt catalyst.
[0035] The present invention also relates to a method for preparing an impact-resistant silicone pressure-sensitive adhesive, comprising the following steps:
[0036] Step 1: Dissolve the weighed methyl vinyl silicone rubber in the solvent and stir evenly;
[0037] Step 2: Add the weighed MQ silicone resin and STF liquid into the mixture under stirring conditions, and stir and disperse the mixture under high-speed ultrasonic stirring for 10 minutes to prepare a stable solution;
[0038] Step 3: Add the weighed crosslinking agent, inhibitor, and platinum catalyst into the reaction kettle and stir evenly to obtain the silicone pressure-sensitive adhesive. After the introduction of the STF solution into the silicone pressure-sensitive adhesive prepared by the present invention, the initial adhesion, the lasting adhesion, and the 70°C high temperature retention of the silicone pressure-sensitive adhesive are not reduced; the impact-resistant silicone pressure-sensitive adhesive not only solves the problem of the dispersibility of the STF solution, but also increases the pendulum impact strength from 1550KJ / m 2 Increased to 2400KJ / m 2 .
[0039] In some embodiments, the preparation method of MQ silicone resin in step 2 is:
[0040] Accurately weigh ethanol and hydrochloric acid and stir them thoroughly for 10 minutes to dissolve them in deionized water; weigh a certain amount of ethyl orthosilicate and hexamethyldisiloxane and stir them thoroughly; add the above monomers into the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes; heat the above solution to 80°C and react for 1 hour; extract, layer, wash with water until neutral, and distill under reduced pressure to obtain MQ resin.
[0041] Embodiment 1
[0042] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 60g of ethyl orthosilicate and 15g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.65.
[0043] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 2g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive.
[0044] Embodiment 2
[0045] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 60g of ethyl orthosilicate and 15g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.65.
[0046] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 6g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive.
[0047] Embodiment 3
[0048] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 60g of ethyl orthosilicate and 15g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.65.
[0049] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 10g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain the silicone pressure-sensitive adhesive.
[0050] Embodiment 4
[0051] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 60g of ethyl orthosilicate and 15g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.65.
[0052] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 120g of MQ silicone resin and 2g of STF liquid under stirring conditions, and stir and disperse at high speed for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst into the reactor and stir evenly to obtain the silicone pressure-sensitive adhesive.
[0053] Comparative Example 1
[0054] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 60g of ethyl orthosilicate and 15g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.65.
[0055] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, then add 100g of MQ silicone resin under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst into the reactor and stir evenly to obtain the silicone pressure-sensitive adhesive.
[0056] Comparative Example 2
[0057] Accurately weigh 7g of ethanol, 10g of hydrochloric acid, stir thoroughly for 10min and dissolve in 20g of deionized water, weigh 55g of ethyl orthosilicate, 15g of hexamethyldisiloxane and stir thoroughly, add the above monomers into the aqueous solution in sequence under stirring conditions, stir thoroughly and disperse for 10min. Heat the above solution to 80℃ and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.6.
[0058] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 2g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive.
[0059] Comparative Example 3
[0060] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 52g of ethyl orthosilicate and 24g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.9.
[0061] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 2g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive.
[0062] Comparative Example 4
[0063] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 54g of ethyl orthosilicate and 28g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 1.0.
[0064] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 2g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive.
[0065] Comparative Example 5
[0066] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 60g of ethyl orthosilicate and 15g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.65.
[0067] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 1g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive.
[0068] Comparative Example 6
[0069] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 60g of ethyl orthosilicate and 15g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.65.
[0070] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 100g of MQ silicone resin and 15g of STF liquid under stirring conditions, and stir at high speed and ultrasonically disperse for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive.
[0071] Comparative Example 7
[0072] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 52g of ethyl orthosilicate and 24g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.9.
[0073] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 80g of MQ silicone resin and 2g of STF liquid under stirring conditions, and stir and disperse at high speed for 10 minutes to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst into the reactor and stir evenly to obtain the silicone pressure-sensitive adhesive.
[0074] Comparative Example 8
[0075] Accurately weigh 7g of ethanol and 10g of hydrochloric acid and stir them thoroughly for 10 minutes to dissolve in 20g of deionized water. Weigh 52g of ethyl orthosilicate and 24g of hexamethyldisiloxane and stir them thoroughly. Add the above monomers to the aqueous solution in sequence under stirring conditions and stir and disperse them thoroughly for 10 minutes. Heat the above solution to 80°C and react for 1h. Extract, layer, wash with water until neutral, and distill under reduced pressure to obtain a white powdery MQ resin with an M / Q ratio of 0.9.
[0076] Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate, stir evenly, add 60g of MQ silicone resin and 2g of STF liquid under stirring, and stir at high speed and ultrasonically disperse for 10min to make a stable solution. Add 1g of crosslinking agent, 0.1g of inhibitor, and 1g of platinum catalyst to the reactor and stir evenly to obtain a silicone pressure-sensitive adhesive. The comparison method of Examples 1-4 and Comparative Examples 1-8 of the present invention is as follows:
[0077] The silicone pressure-sensitive adhesive prepared according to the above examples and comparative examples was coated on a polyethylene terephthalate (PET) film with a thickness of 50 μm using a scraper, and cured at 130 degrees Celsius for 2 minutes to obtain a silicone pressure-sensitive adhesive tape with a dry adhesive thickness of 40 μm. The mechanical properties of the silicone pressure-sensitive adhesive tape were tested, wherein the initial adhesion of the ring was about 1600 gf / 25mm; the holding force was 72H; the 1800 peel strength was about 2500 gf / 25mm; the pendulum impact absorption strength was about 2400 KJ / m 2 ; No transfer at 70℃ for 48 hours. Specific test data are shown in Table 1.
[0078] Table 1 Detection performance of different embodiments Table 1
[0079]
[0080]
[0081] By comparing the test data in the table, it can be seen that increasing the amount of STF liquid can greatly increase the impact strength of the adhesive. This is mainly because when the silicone pressure-sensitive adhesive is subjected to external impact, the nanoparticles in the STF liquid collide with each other, aggregate, absorb and dissipate the impact energy to achieve the impact resistance of the pressure-sensitive adhesive.
[0082] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation methods. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the embodiments shown here.
Claims
1. An impact-resistant silicone pressure-sensitive adhesive, characterized in that: Including the following quality ingredients: MQ silicone resin 100g, its M / Q ratio is 0.65; Methyl vinyl silicone rubber 100g; Cross-linking agent 1g; Platinum catalyst 1g; Inhibitor 0.1 g; STF liquid 10g; the preparation method of the silicone pressure-sensitive adhesive comprises the following steps: Step 1: Dissolve 100g of methyl vinyl silicone rubber in ethyl acetate solvent and stir evenly; Step 2: add weighed 100g MQ silicone resin and 10g STF liquid under stirring, and stir at high speed for 10 minutes to form a stable solution; Step 3: Add 1g of a cross-linking agent, 0.1g of an inhibitor, and 1g of a platinum catalyst into a reaction kettle and stir evenly to obtain a silicone pressure-sensitive adhesive; the cross-linking agent is at least one of benzoyl peroxide, aminosilane, and 2,4-dichlorobenzoyl peroxide.
2. The impact-resistant silicone pressure-sensitive adhesive according to claim 1, characterized in that: The inhibitor is at least one of 1-ethynylcyclohexanol and methylbutynol.
3. The impact-resistant silicone pressure-sensitive adhesive according to claim 1, characterized in that: The platinum catalyst is at least one of a Speier catalyst and a Karstedt catalyst.
Citation Information
Patent Citations
Hot-melt pressure-sensitive adhesive as well as preparation method and application thereof
CN107987761A
Impact-resistant polyacrylate pressure-sensitive adhesive layer and preparation method thereof and pressure-sensitive adhesive tape
CN111440572A
Acrylate hot-melt pressure-sensitive adhesive and preparation method thereof
CN114214002A
Self-adhesive organic silicon press-sensitive adhesive and preparation method thereof
CN104152104A
Modified foaming polyurethane and preparation method thereof
CN113583431A