A hydrogen storage cylinder with fiber-wound plastic liner
By designing the matching structure and fiber winding layer between the buffer tank and the bottle nozzle joint in the hydrogen storage cylinder, the sealing problem caused by material differences is solved, and the sealing and safety of the hydrogen storage cylinder is improved to prevent hydrogen leakage.
Patent Information
- Application Number
- CN202310149779.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-22
AI Technical Summary
The fully wound gas cylinder of plastic inner liner fibers causes the sealing structure to fail when the bottle nozzle is pressed due to differences in material modulus, elastic strain and thermal expansion rate, which is prone to hydrogen leakage, which poses safety hazards.
Design hydrogen storage cylinders that include plastic inner liner, metal bottle nozzle joint and fiber wrapping layer. The design of the buffer groove and bottle nozzle joint is matched by the design of the fixing sleeve support and fiber wrapping layer enhancement, improve sealing and connection strength, and reduce plastic inner liner Deform to prevent hydrogen leakage.
Maintain good sealing when subjected to pressure shock, reduce the risk of hydrogen leakage, and improve the safety and service life of hydrogen storage cylinders.
Smart Images

Figure CN116006899B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a hydrogen storage cylinder with a fiber-wound plastic liner, belonging to the technical field of hydrogen storage cylinders. Background Art
[0002] At present, hydrogen storage cylinders are mainly divided into four types: all-metal cylinders, metal liner fiber hoop-wrapped cylinders, metal liner fiber fully wrapped cylinders and plastic liner fiber fully wrapped cylinders. At present, plastic liner fiber fully wrapped cylinders have gradually become the research focus of hydrogen storage cylinders due to their light weight and high hydrogen storage density.
[0003] The plastic liner fiber fully wrapped gas cylinder is composed of a plastic liner, a metal bottle mouth joint and a fiber winding layer. Due to the large differences in the modulus, elastic strain and thermal expansion rate of the metal bottle mouth joint and the plastic, when the bottle mouth is subjected to reciprocating pressure shock, the plastic liner will be significantly deformed, causing the sealing structure to fail, affecting the product's sealing. Therefore, hydrogen leakage is prone to occur, posing a huge safety hazard. Summary of the invention
[0004] In order to solve the above problems, the present application proposes a fiber-wound plastic liner hydrogen storage cylinder, in which the fixed sleeve can support the bottle mouth and reduce the deformation of the bottle mouth. The coordinated setting of the buffer groove of the plastic liner and the bottle mouth joint can improve the shear strength of the shoulder of the hydrogen storage cylinder, reduce the deformation of the plastic liner, and improve the connectivity between the plastic liner and the metal bottle mouth joint, so that when the hydrogen storage cylinder is subjected to reciprocating pressure shock, it can still maintain good sealing to prevent hydrogen leakage.
[0005] The present application provides a filament-wound plastic liner hydrogen storage cylinder, comprising:
[0006] A plastic liner, wherein the interior of the plastic liner is hollow to form a receiving cavity, a bottle mouth is opened on the top of the plastic liner, the bottle mouth is connected to the receiving cavity, and a shoulder seal of the plastic liner is recessed inward to form a buffer groove;
[0007] A bottle mouth joint, the bottom shape of which matches the shape of the buffer groove, so that the bottle mouth joint is embedded in the buffer groove, the upper profile of the bottle mouth joint is smoothly transitioned with the shoulder seal of the plastic liner, a sealing opening is opened at the center of the bottle mouth joint, the lower end of the sealing opening is clamped on the outer side of the bottle mouth and sealed by a first sealing ring, and the upper end of the sealing opening is connected to a high-pressure gas cylinder valve;
[0008] A fixing sleeve, which is arranged at the inner side of the bottle mouth and is used to support the bottle mouth, and the bottle mouth joint and the fixing sleeve are made of metal;
[0009] The winding layer is formed by winding fibers around the outer peripheral surface of the plastic liner and the bottle mouth joint.
[0010] Optionally, the buffer groove is provided with at least two clamping surfaces in the circumference thereof, the bottle mouth joint is provided with a clamping portion cooperating with the clamping surfaces in the circumference thereof, and the bottle mouth joint and the buffer groove are clamped together through the clamping surfaces and the clamping portions; or
[0011] The top of the buffer groove is provided with a protrusion, the bottom of the bottle mouth joint is provided with a groove, and the bottle mouth joint and the buffer groove are engaged with each other through the protrusion and the groove.
[0012] Optionally, the bottle mouth joint includes a connecting piece, a sealing pressing block and a locking nut;
[0013] The bottom shape of the connecting piece matches the shape of the buffer groove, a connecting port is provided at the center of the connecting piece, the sealing block is connected to the connecting port through threads, a sealing port is provided at the center of the sealing block, and the locking nut is arranged at the top of the connecting piece and is connected to the outer periphery of the sealing block through threads;
[0014] Preferably, the bottle mouth, the sealing port and the connecting port are arranged on a common central axis.
[0015] Optionally, a groove is provided at the bottom of the connecting port, the groove is used to place a second sealing ring, and the bottom of the sealing pressing block abuts against the second sealing ring.
[0016] Optionally, the plastic liner comprises an inner layer and an outer layer, and the outer layer is arranged on the outer side of the inner layer;
[0017] In parts by weight, the inner layer comprises 80-100 parts of PA11, 20-30 parts of diisocyanate, 3-5 parts of polyisocyanate, 10-20 parts of EVOH, 5-10 parts of mica flakes and 2-5 parts of plasticizer;
[0018] In parts by weight, the outer layer includes 80-100 parts of PA11, 30-50 parts of a compound containing two or more hydroxyl groups or a compound containing two or more amino groups, 10-20 parts of epoxy resin, 3-5 parts of anhydride curing agent, 2-5 parts of a plasticizer and 1-3 parts of a catalyst.
[0019] Both the inner and outer layer materials are based on PA11, which can ensure the mechanical strength of the plastic liner. The EVOH added to the inner layer can improve the inner layer's resistance to hydrogen permeation, and the mica flakes can extend the gas permeation path, thereby working together with EVOH to improve the plastic liner's resistance to hydrogen permeation. The epoxy resin added to the outer layer can be cured under heating to improve the mechanical strength, corrosion resistance and density of the outer layer. The diisocyanate and polyisocyanate in the inner layer and the compound containing two or more hydroxyl groups or the compound containing two or more amino groups in the outer layer can react in the presence of a catalyst to form a cross-linked polymer network, thereby increasing the bonding strength and toughness between the inner and outer layers, preventing delamination of the plastic liner, improving the deformation resistance of the plastic liner, reducing the deformation difference between the plastic liner and the bottle mouth cap under pressure shock, and further improving the sealing of the hydrogen storage cylinder.
[0020] Optionally, the catalyst is selected from at least one of triethylamine, triethanolamine, DMEA, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylenediamine, and dibutyltin dilaurate.
[0021] Optionally, the thickness of the inner layer is 2-3 mm, and the thickness of the outer layer is 2-3 mm. The above thickness can not only make the inner layer and the outer layer play their respective roles, but also enhance the bonding strength between the inner layer and the outer layer, doubly preventing hydrogen leakage and deformation of the hydrogen cylinder.
[0022] Optionally, the mica flakes have a thickness of 50-1000 nm and a flake diameter of 20-200 μm. The mica flakes are a lamellar structure, and the mica flakes of the above thickness and flake diameter can be evenly dispersed in the inner layer, effectively blocking hydrogen and improving the bonding force between the inner layer and the outer layer.
[0023] Preferably, the mica flakes are composed of a first part and a second part, wherein the particle size of the first part is 50-200nm, the flake diameter is 20-25μm, and the proportion is 20%, and the particle size of the second part is 500-1000nm, the flake diameter is 150-200μm, and the proportion is 80%. This proportion is the weight percentage of the first part or the second part to the total mica flakes. The mica flakes of the second part have a large layer structure, which can effectively block hydrogen and extend the permeation path of hydrogen. The mica flakes of the first part have a small layer structure and tend to be granular, which can be filled in the gaps of the second part, so that the mica flakes form a dense multi-layer protective structure in the inner layer, thereby effectively reducing the permeation of hydrogen.
[0024] Optionally, the mica flakes are mica flakes modified with butyl orthosilicate and dibutyl phthalate, and the preparation steps of mica flakes modified with butyl orthosilicate and dibutyl phthalate are as follows:
[0025] The mica flakes are washed and dried, placed in an ethanol solution for activation at 50-60°C for at least 3 hours, then the butyl orthosilicate and dibutyl phthalate are added to the ethanol solution, modified at 50-60°C for 2-3 hours, filtered and dried to obtain the mica flakes, wherein the butyl orthosilicate accounts for 2%-6% of the weight of the mica flakes, and the dibutyl phthalate accounts for 1%-2.5% of the weight of the mica flakes.
[0026] The above-mentioned modification treatment can improve the dispersibility of mica flakes in the inner layer, and improve its adhesion with epoxy resin, EVOH, diisocyanate, polyisocyanate and plasticizer, so that the mica flakes can form a multi-layer protective structure in the inner layer, thereby improving the sealing of the plastic liner itself; and through the modification of the two substances of butyl orthosilicate and dibutyl phthalate, the mica flakes are promoted to form hydrogen bonds with other substances in the inner layer, thereby increasing the number of hydrogen bonds in the inner layer, which can improve the mechanical strength of the inner layer and increase the deformation resistance of the substances in the inner layer, and can maintain the original shape even under repeated pressure shocks, thereby improving the sealing between the plastic liner and the bottle mouth joint and preventing hydrogen leakage at the bottle mouth.
[0027] Activation in ethanol can increase the attachment sites of butyl orthosilicate and dibutyl phthalate, and increase the amount of butyl orthosilicate and dibutyl phthalate on mica flakes.
[0028] Optionally, before the winding step, a slurry is coated on the outer circumference of the plastic liner and the bottle mouth joint to form a connecting layer, and the winding layer is wound on the outer circumference of the connecting layer. The slurry includes 20-30 parts of diisocyanate, 1-2 parts of polyisocyanate, 0.5-1 part of catalyst, 5-10 parts of ZIF-8, 70-80 parts of epoxy resin and 2-5 parts of imidazole curing agent by weight.
[0029] Optionally, the thickness of the connecting layer is 0.5-0.6 mm.
[0030] The diisocyanate and polyisocyanate contained in the connecting layer can react with the compound containing two or more hydroxyl groups or the compound containing two or more amino groups in the outer layer, thereby enhancing the bonding force between the connecting layer and the outer layer and improving the adhesion between the winding layer and the outer layer; and the above-mentioned substances can be cured and formed on the outer peripheral surface of the bottle mouth joint, thereby improving the bonding strength between the bottle mouth joint and the winding layer, thereby effectively avoiding stratification of the hydrogen storage cylinder, and improving the integrity of the hydrogen storage cylinder, effectively combining the bottle mouth joint and the plastic liner, and improving the deformation resistance of the hydrogen storage cylinder.
[0031] ZIF-8 is a porous material, and the cross-linked network formed by epoxy resin, diisocyanate, and polyisocyanate can be interspersed between the micropores, improving the connectivity and compactness of the connecting layer, and can also play the role of a cross-linking point, increasing the adhesion of the connecting layer to the winding layer, so that the winding layer can be tightly wound on the outer peripheral surface of the plastic liner and the bottle mouth joint, improving the bonding strength between the layers of the hydrogen storage cylinder, so that the overall sealing, deformation resistance and mechanical strength of the hydrogen storage cylinder are improved. The above-mentioned ZIF-8 plays the role of a cross-linking point, which means that not only the polymer network can pass through the micropores of ZIF-8, but also the endpoints of many polymer molecular chains are adsorbed on ZIF-8. At this time, ZIF-8 is equivalent to a cross-linking center point, which can connect multiple polymer molecular chains, thereby forming a cross-linked polymer network at the microscopic level.
[0032] Optionally, the anhydride curing agent is 3,3'-dithiodipropionic anhydride;
[0033] The compound containing two or more hydroxyl groups is selected from at least one of 1,4-butanediol, glycerol, diethylene glycol, 4,4'-dihydroxydiphenyl sulfide, and 3,3'-dihydroxydiphenyl disulfide;
[0034] The compound containing two or more amino groups is selected from at least one of ethylenediamine, 1,2-propylenediamine, 1,6-hexanediamine, p-phenylenediamine, 2,3-diaminopyridine, 3,3'-iminobis-1-propanol, 4,4'-diaminodiphenyl disulfide, and 3,3'-diaminodiphenyl disulfide.
[0035] The 3,3'-dithiodipropionic anhydride used as an anhydride curing agent can introduce disulfide bonds into the inner layer, so that the plastic liner can self-repair when microcracks occur, extending the service life of the plastic liner. Compounds containing more than two hydroxyl groups and compounds containing more than two amino groups can also contain disulfide bonds, which can further improve the self-repair effect of the plastic liner. In addition, the mica flakes contained in the inner layer form hydrogen bonds with other substances. When the plastic liner is subjected to a scratch with a width of no more than 50μm, it can be heated to 120℃ for 8h and can be repaired by more than 80%. The initial scratch width is set as W0, and the width of the scratch after repair is W1. The calculation formula of the repair percentage is: (W0-W1) / W0×100%.
[0036] Optionally, the inner layer and the outer layer are made by a double-layer rotational molding process, so that the outer layer is coated on the outside of the inner layer. The outer layer is first rotationally molded, and the inner layer is then rotationally molded in the outer layer. The rotational molding of the inner layer can initially form a cross-linked network of polyurethane in the outer layer and the inner layer, thereby improving the connection strength between the inner layer and the outer layer. After the winding layer is wound, the final curing is performed. During the curing process, the inner layer and the outer layer form a final polyurethane cross-linked network, so that the inner layer and the outer layer are tightly combined, and under the action of the connecting layer, the inner layer, the outer layer, the connecting layer and the winding layer form a whole, thereby avoiding delamination of the hydrogen storage cylinder.
[0037] Optionally, the fiber is a carbon fiber impregnated in a preservative, wherein the preservative comprises 50-60 parts of water, 20-30 parts of ethanol, 40-60 parts of water-based epoxy resin and 5-10 parts of dopamine by weight, the pH of the slurry is 8-9, and the amount of the carbon fiber impregnated is 17-20wt%.
[0038] Impregnation of carbon fiber with epoxy resin can enhance the mechanical strength of the winding layer, provide chemical protection for the winding layer, and improve the corrosion resistance of the hydrogen storage cylinder. Dopamine can be dispersed on the carbon fiber. Since dopamine contains hydrogen bonds and amino groups, it can react with diisocyanates and polyisocyanates in the connecting layer to form polyurethane, thereby improving the bonding ability and density of the winding layer and the connecting layer, and further preventing the penetration of hydrogen and delamination of the hydrogen storage cylinder.
[0039] The impregnated carbon fiber contains glue. If it is directly wound on the outside of the plastic liner, the glue is easy to drip, resulting in uneven slurry in the final winding layer and waste of raw materials. The impregnated carbon fiber is wrapped on the connecting layer. The porous structure of ZIF-8 can absorb the glue, so that the slurry is evenly distributed in the winding layer, and the waste of raw materials is reduced, the cleanliness of the operating environment is improved, and the substances in the slurry can react with the substances in the connecting layer. ZIF-8 can also act as a cross-linking point between the connecting layer and the winding layer, further improving the bonding strength between the connecting layer and the winding layer.
[0040] Optionally, the thickness of the winding layer is 25-30 mm.
[0041] Optionally, the impregnating material further comprises 5-10 parts of an amine chain extender containing a disulfide bond.
[0042] Preferably, the disulfide bond-containing amine chain extender is selected from any one or more of 4,4'-diaminodiphenyl disulfide, 3,3'-diaminodiphenyl disulfide, bis(2-aminophenyl) disulfide, and 4,4'-bis(2-amino-6-methylpyrimidinyl) disulfide.
[0043] The above-mentioned disulfide bond-containing amine chain extender reacts with diisocyanate and polyisocyanate to generate a polyurethane network, which can introduce disulfide bonds between the winding layer and the connecting layer, so that the winding layer and the connecting layer have self-repairing capabilities, further improving the service life of the hydrogen storage cylinder. In addition, the reasonable ratio of the disulfide bond-containing amine chain extender and dopamine makes the polymerization degree of the polyurethane network moderate, increases the mobility of the molecular chain, and thus can provide buffering under the action of external force, thereby reducing the deformation of the hydrogen storage cylinder.
[0044] Optionally, the preparation method of the filament-wound plastic liner hydrogen storage cylinder is:
[0045] Making the plastic liner: mixing the raw materials of the outer layer in proportion, and preparing the outer layer by rotational molding, then mixing the raw materials of the inner layer in proportion, and then adding the raw materials of the inner layer to the outer layer for rotational molding to form the inner layer, thereby forming the plastic liner;
[0046] Assembly: fix the fixing sleeve to the inner side of the bottle mouth, and then fit the bottle mouth joint into the buffer groove;
[0047] Slurry coating: The slurry is coated on the outer peripheral surface of the plastic liner and the bottle mouth joint, and a connecting layer is formed after heating and curing:
[0048] Winding: Winding the fibers on the outer peripheral surface of the connecting layer, heating and curing to form the winding layer, thereby obtaining the fiber-wound plastic liner hydrogen storage cylinder.
[0049] In the double-layer rotational molding process of the plastic liner, a preliminary chemical connection has been formed between the inner layer and the outer layer. During the subsequent curing of the slurry coating, the chemical connection between the inner layer and the outer layer is further strengthened, and the outer layer also forms a chemical connection with the connecting layer. The bottle mouth joint is also tightly combined with the plastic liner through the connecting layer. Finally, during the heating and curing of the winding layer, the winding layer forms a chemical connection with the connecting layer. At this time, the inner layer, outer layer, connecting layer and winding layer are all tightly connected, so that the hydrogen storage cylinder forms a whole.
[0050] The beneficial effects of this application include but are not limited to:
[0051] 1. The fiber-wound plastic liner hydrogen storage cylinder provided in the present application can reduce the weight of the hydrogen storage cylinder itself and improve the hydrogen permeability resistance and fatigue performance of the hydrogen storage cylinder. The shape of the plastic liner and the bottle mouth joint can improve the connectivity between the plastic liner and the bottle mouth joint, thereby improving the sealing of the hydrogen storage cylinder and preventing hydrogen leakage.
[0052] 2. The fiber-wound plastic liner hydrogen storage cylinder provided in the present application, the arrangement of the connecting parts, the sealing block and the locking nut can facilitate the replacement of the first sealing ring and the sealing block, improve the replacement efficiency of parts, thereby improving the sealing effect of the hydrogen storage cylinder and the service life of the hydrogen storage cylinder.
[0053] 3. The fiber-wound plastic liner hydrogen storage cylinder provided in the present application has a plastic liner divided into an inner layer and an outer layer, which can improve the hydrogen permeability resistance, mechanical strength and deformation resistance of the plastic liner, improve the sealing of the hydrogen storage cylinder, and prevent delamination of the plastic liner.
[0054] 4. The fiber-wound plastic liner hydrogen storage cylinder provided in the present application, the setting of the connecting layer and the winding layer can increase the integrity of the hydrogen storage cylinder, enhance the connection strength between the various layers, and further improve the sealing and deformation resistance of the hydrogen storage cylinder. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0056] Figure 1 This is a structural schematic diagram of a hydrogen storage cylinder involved in Example 2 of the present application;
[0057] Figure 2 This is another structural schematic diagram of the hydrogen storage cylinder involved in Example 2 of the present application;
[0058] Figure 3 This is another structural schematic diagram of the hydrogen storage cylinder involved in Example 2 of the present application;
[0059] List of parts and reference numerals:
[0060] 10. Plastic liner; 11. Accommodating cavity; 12. Bottle mouth; 13. Buffer groove; 14. Snap-on table; 15. Protrusion; 20. Bottle mouth joint; 21. Connector; 22. Sealing block; 23. Locking nut; 24. Sealing mouth; 25. Groove; 30. Fixing sleeve; 40. First sealing ring; 41. Second sealing ring. DETAILED DESCRIPTION
[0061] In order to more clearly illustrate the overall concept of the present application, a detailed description is given below in an illustrative manner in conjunction with the accompanying drawings.
[0062] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0063] In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application may also be implemented in other ways different from those described herein. Therefore, the scope of protection of the present application is not limited to the specific embodiments disclosed below.
[0064] In addition, in the description of the present application, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0065] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0066] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0067] In the present application, unless otherwise clearly specified and limited, a first feature "above" or "below" a second feature may be that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in an appropriate manner in any one or more embodiments or examples.
[0068] Example 1
[0069] The present embodiment relates to the processing and production of a plastic liner, which includes an inner layer and an outer layer. By weight, the inner layer includes 80-100 parts of PA11, 20-30 parts of diisocyanate, 3-5 parts of polyisocyanate, 10-20 parts of EVOH, 5-10 parts of mica flakes and 2-5 parts of plasticizer; the outer layer includes 80-100 parts of PA11, 30-50 parts of a compound containing two or more hydroxyl groups or a compound containing two or more amino groups, 10-20 parts of epoxy resin, 3-5 parts of anhydride curing agent, 2-5 parts of plasticizer and 1-3 parts of catalyst. The outer layer and the inner layer are formed by a double-layer rotational molding process in the prior art so that the outer layer is coated on the outside of the inner layer, and the plastic liner is obtained.
[0070] According to the above processing and production method, plastic liners 1#-9# and comparative plastic liners D1#-D4# were prepared as follows:
[0071] Plastic liner 1#
[0072] 90 parts of PA11, 40 parts of 4,4'-dihydroxydiphenyl sulfide, 15 parts of epoxy resin, 4 parts of 3,3'-dithiodipropionic anhydride, 4 parts of plasticizer and 2 parts of dibutyltin dilaurate were mixed, and the outer layer with a thickness of 3 mm was obtained by mold rotation molding at 230°C. Then, 90 parts of PA11, 25 parts of diisocyanate, 3 parts of polyisocyanate, 15 parts of EVOH, 8 parts of mica flakes and 4 parts of plasticizer were added to the outer layer, wherein the mica flakes had a thickness of 500nm and a sheet diameter of 100μm, and the inner layer with a thickness of 2mm was obtained by rotation molding at 230°C. After cooling, plastic liner 1# was obtained.
[0073] Plastic liner 2#
[0074] 80 parts of PA11, 50 parts of 4,4'-diaminodiphenyl disulfide, 10 parts of epoxy resin, 3 parts of 3,3'-dithiodipropionic anhydride, 5 parts of plasticizer and 1 part of dibutyltin dilaurate were mixed, and the outer layer with a thickness of 2.5 mm was obtained by mold rotation molding at 280°C. Then, 80 parts of PA11, 30 parts of diisocyanate, 5 parts of polyisocyanate, 10 parts of EVOH, 10 parts of mica flakes and 2 parts of plasticizer were added to the outer layer, wherein the thickness of the mica flakes was 50nm and the diameter of the flakes was 20μm. The inner layer with a thickness of 2.5 mm was obtained by rotation molding at 280°C, and the plastic liner 2# was obtained after cooling.
[0075] Plastic liner 3#
[0076] 100 parts of PA11, 30 parts of ethylenediamine, 20 parts of epoxy resin, 5 parts of 3,3'-dithiodipropionic anhydride, 2 parts of plasticizer and 3 parts of dibutyltin dilaurate were mixed, and the outer layer with a thickness of 2 mm was obtained by mold rotation molding at 280°C. Then, 100 parts of PA11, 20 parts of diisocyanate, 3 parts of polyisocyanate, 20 parts of EVOH, 5 parts of mica flakes and 5 parts of plasticizer were added to the outer layer, wherein the thickness of the mica flakes was 1000nm and the diameter of the flakes was 200μm. The inner layer with a thickness of 3mm was obtained by rotation molding at 280°C, and the plastic liner 3# was obtained after cooling.
[0077] Plastic liner 4#
[0078] The difference between the present plastic liner and the plastic liner 1# is that the mica flakes are mica flakes modified by butyl orthosilicate and dibutyl phthalate, and the preparation steps of the mica flakes modified by butyl orthosilicate and dibutyl phthalate are as follows:
[0079] Wash and dry the mica flakes, place them in an ethanol solution and activate them at 60°C for 3 hours, then add butyl orthosilicate and dibutyl phthalate to the ethanol solution, modify them at 60°C for 2 hours, filter and dry them to obtain the product. Butyl orthosilicate accounts for 2% of the weight of the mica flakes, and dibutyl phthalate accounts for 1% of the weight of the mica flakes. The remaining ingredients and preparation method are the same as those of plastic liner 1#, to obtain plastic liner 4#.
[0080] Plastic liner 5#
[0081] The difference between the present plastic liner and the plastic liner 1# is that the mica flakes are mica flakes modified by butyl orthosilicate and dibutyl phthalate, and the preparation steps of the mica flakes modified by butyl orthosilicate and dibutyl phthalate are as follows:
[0082] Wash and dry the mica flakes, place them in an ethanol solution and activate them at 50°C for 5 hours, then add butyl orthosilicate and dibutyl phthalate to the ethanol solution, modify them at 50°C for 3 hours, filter and dry them to obtain butyl orthosilicate accounting for 6% of the weight of the mica flakes, and dibutyl phthalate accounting for 2.5% of the weight of the mica flakes. The remaining ingredients and preparation method are the same as those of plastic liner 1#, to obtain plastic liner 5#.
[0083] Plastic liner 6#
[0084] The difference between the present plastic liner and the plastic liner 1# is that the mica flakes are mica flakes modified by bis-[3-(triethoxysilyl)propyl]-tetrasulfide, and the preparation steps of the mica flakes modified by bis-[3-(triethoxysilyl)propyl]-tetrasulfide are as follows:
[0085] The mica flakes are washed and dried, placed in an ethanol solution for activation at 50°C for 5 hours, then bis-[3-(triethoxysilyl)propyl]-tetrasulfide is added to the ethanol solution, modified at 50°C for 3 hours, filtered and dried to obtain bis-[3-(triethoxysilyl)propyl]-tetrasulfide, which accounts for 8.5% of the weight of the mica flakes. The remaining ingredients and preparation method are the same as those of plastic liner 1#, to obtain plastic liner 6#.
[0086] Plastic liner 7#
[0087] The difference between this plastic liner and plastic liner 5# is that the mica flakes consist of a first part and a second part, wherein the particle size of the first part is 50nm, the flake size is 20μm, and the proportion is 20%, and the particle size of the second part is 1000nm, the flake size is 150μm, and the proportion is 80%. The remaining ingredients and preparation method are the same as those of plastic liner 5#, so as to obtain plastic liner 7#.
[0088] Plastic liner 8#
[0089] The difference between this plastic liner and plastic liner 5# is that the mica flakes consist of a first part and a second part, wherein the particle size of the first part is 200nm, the flake diameter is 25μm, and the proportion is 20%, and the particle size of the second part is 500nm, the flake diameter is 200μm, and the proportion is 80%. The remaining ingredients and preparation method are the same as those of plastic liner 5#, namely plastic liner 8# is obtained.
[0090] Plastic liner 9#
[0091] The difference between this plastic liner and plastic liner 1# is that the thickness of the inner layer is 1.5mm, the thickness of the outer layer is 3.5mm, and the remaining components and preparation method are the same as those of plastic liner 1#, so as to obtain plastic liner 9#.
[0092] Compare plastic liner D1#
[0093] The difference between this comparative plastic liner and plastic liner 1# is that there is no diisocyanate and polyisocyanate in the inner layer, and the remaining components and preparation method are the same as those of plastic liner 1#, namely comparative plastic liner D1#.
[0094] Compare plastic liner D2#
[0095] The difference between this comparative plastic liner and plastic liner 1# is that there is no EVOH in the inner layer, and the remaining components and preparation method are the same as those of plastic liner 1#, namely comparative plastic liner D2#.
[0096] Compare plastic liner D3#
[0097] The difference between this comparative plastic liner and plastic liner 1# is that there is no mica flake in the inner layer, and the remaining components and preparation method are the same as those of plastic liner 1#, namely comparative plastic liner D3#.
[0098] Compare plastic liner D4#
[0099] The difference between this comparative plastic liner and plastic liner 1# is that there is no 4,4'-dihydroxydiphenyl sulfide and dibutyltin dilaurate in the outer layer, and the remaining ingredients and preparation method are the same as those of plastic liner 1#, namely, comparative plastic liner D4#.
[0100] The hydrogen permeability coefficient, tensile strength, elongation at break, notched impact strength at room temperature, and notched impact strength at -40°C were tested on the plastic liners 1#-9# and comparative plastic liners D1#-D4# prepared above, wherein the hydrogen permeability coefficient was tested in accordance with GB / T 1038-2000.
[0101] The specific test results are shown in Table 1 below:
[0102] Table 1
[0103]
[0104] The plastic liners 3#, D1#, and D4# in this embodiment have no self-repairing ability. The remaining plastic liners can be heated to 120°C for 8 hours when scratched with a width of no more than 50 μm. The width of the scratch before repair is recorded as W. 0 , the width of the scratch after repair is recorded as W 1 The calculation formula of the repair rate is [(W 0 -W 1 ) / W 0 ]×100%, proving that it can repair more than 80%.
[0105] Example 2
[0106] refer to Figure 1-3, showing the mouth structure of the hydrogen storage cylinder, the body structure of the hydrogen storage cylinder can adopt the shape in the prior art, the present embodiment relates to a fiber-wound plastic liner hydrogen storage cylinder, the hydrogen storage cylinder comprises: a plastic liner 10, the interior of the plastic liner 10 is hollowed out to form a receiving chamber 11, the top of the plastic liner 10 is provided with a bottle mouth 12, the bottle mouth 12 is connected to the receiving chamber 11, the shoulder seal of the plastic liner 10 is recessed inward to form a buffer groove 13; a bottle mouth joint 20, the bottom shape of the bottle mouth joint 20 matches the shape of the buffer groove 13, so that the bottle mouth joint 20 Embedded in the buffer groove 13, the upper mold surface of the bottle mouth joint 20 and the shoulder head of the plastic liner 10 are smoothly transitioned, a sealing port 24 is opened in the center of the bottle mouth joint 20, the lower end of the sealing port 24 is clamped on the outside of the bottle mouth 12, and is sealed by a first sealing ring 40, and the upper end of the sealing port 24 is connected to a high-pressure gas cylinder valve; a fixing sleeve 30, the fixing sleeve 30 is arranged on the inner side of the bottle mouth 12, and is used to support the bottle mouth 12, the bottle mouth joint 20 and the fixing sleeve 30 are made of metal; a winding layer, the fiber is wound on the outer peripheral surface of the plastic liner 10 and the bottle mouth joint 20 to form a winding layer.
[0107] The plastic liner 10 is used in the hydrogen storage cylinder, which can reduce the weight of the hydrogen storage cylinder itself and improve the hydrogen permeability and deformation resistance of the hydrogen storage cylinder. The fixed sleeve 30 used can support the bottle mouth 12, thereby reducing the deformation of the bottle mouth 12. The matching arrangement of the buffer groove 13 of the plastic liner 10 and the bottle mouth joint 20 can improve the shear strength of the shoulder of the hydrogen storage cylinder, reduce the deformation of the plastic liner 10, and improve the connectivity between the plastic liner 10 and the bottle mouth joint, so that when the hydrogen storage cylinder is subjected to reciprocating pressure shock, it can still maintain good sealing to prevent hydrogen leakage.
[0108] Since the bottom shape of the bottle mouth joint 20 matches the shape of the buffer groove 13, the bottom of the bottle mouth joint 20 is designed to be thicker than the existing bottle mouth joint 20. The bottle mouth joint 20 made of metal material can meet the shear strength requirements of the shoulder of the hydrogen storage cylinder and improve the mechanical strength of the hydrogen storage cylinder; and the upper profile of the bottle mouth joint 20 and the shoulder head of the plastic liner 10 have a smooth transition to ensure that the winding layer is smoothly attached to the bottle mouth joint 20 and the plastic liner 10, avoiding the occurrence of fiber overhead and enhancing the connectivity between the winding layer and the plastic liner 10 and the bottle mouth joint 20.
[0109] The lower end of the sealing mouth 24 is engaged with the outer side of the bottle mouth 12 and is sealed by the first sealing ring 40. In the process of filling the accommodating chamber 11 with hydrogen, the plastic liner 10 is inevitably deformed outward by the hydrogen pressure. Therefore, the design of the first sealing ring 40 can ensure the sealing between the plastic liner 10 and the bottle mouth joint 20, and the sealing effect is enhanced with the increase of the internal pressure. The fixing sleeve 30 is made of metal material, which can ensure the deformation strength and improve the anti-deformation ability of the hydrogen storage bottle.
[0110] As an embodiment, the buffer groove 13 is provided with at least two clamping surfaces 14 in the circumference, the bottle mouth joint 20 is provided with a clamping portion matched with the clamping surface 14 in the circumference, and the bottle mouth joint 20 and the buffer groove 13 are clamped by the clamping surface 14 and the clamping portion; or
[0111] A protrusion 15 is provided on the top of the buffer groove 13 , and a groove 25 is provided on the bottom of the bottle mouth joint 20 . The bottle mouth joint 20 and the buffer groove 13 are engaged with each other through the protrusion 15 and the groove 25 .
[0112] The above arrangement can, firstly, prevent the bottle mouth joint 20 and the plastic liner 10 from rotating, thereby facilitating the fiber to be wound around the bottle mouth joint 20 and the outside of the plastic liner 10 to form a winding layer; secondly, it can increase the contact area between the bottle mouth joint 20 and the plastic liner 10, reduce the contact gap between the two, and thus improve the connection strength between the two.
[0113] As an embodiment, the bottle mouth joint 20 includes a connecting piece 21, a sealing block 22 and a locking nut 23; the bottom shape of the connecting piece 21 matches the shape of the buffer groove 13, a connecting port is opened in the center of the connecting piece 21, the sealing block 22 is connected to the connecting port through threads, a sealing port 24 is opened in the center of the sealing block 22, and the locking nut 23 is arranged on the top of the connecting piece 21 and is connected to the outer periphery of the sealing block 22 through threads.
[0114] Since the bottle mouth joint 20 and the plastic liner 10 are both wrapped with fibers to form a winding layer, when the sealing of the hydrogen storage cylinder decreases and hydrogen leakage occurs, the bottle mouth joint 20 cannot be directly disassembled and replaced, and the entire hydrogen storage cylinder can only be replaced. The bottle mouth joint 20 under this setting is divided into three parts. The first part is the connecting piece 21, which can ensure the connectivity with the plastic liner 10 and improve the integrity of the hydrogen storage cylinder; the second part is the sealing block 22, which mainly plays the role of connecting the plastic liner 10 and the high-pressure cylinder valve, and is easy to disassemble. First, it is easy to replace parts and extend the service life of the bottle mouth joint 20. Even if the sealing of the hydrogen storage cylinder decreases, the sealing block 22 can be replaced without replacing a new hydrogen storage cylinder, reducing maintenance costs; second, it is easy to replace the first sealing ring 40. As time goes by, The first sealing ring 40 is extended, and the first sealing ring 40 will be deformed under the reciprocating pressure impact, thereby reducing the sealing effect of the hydrogen storage cylinder. Therefore, this arrangement can remove the sealing block 22 and replace the first sealing ring 40, which is convenient for improving the sealing effect of the hydrogen storage cylinder; the third part is a locking nut 23. When the sealing block 22 is screwed into the connecting port through a thread, the connecting piece 21 and the sealing block 22 are initially fixed. The locking nut 23 further locks the sealing block 22 to improve the stability of the sealing block 22, thereby facilitating the subsequent connection of the high-pressure cylinder valve and the filling and discharge of hydrogen.
[0115] As an embodiment, the bottle mouth 12, the sealing port 24 and the connecting port are arranged on a common central axis. This arrangement can improve the consistency of the sealing performance of the hydrogen storage bottle in the circumferential direction, thereby improving the sealing effect of the hydrogen storage bottle and facilitating the processing and production of the hydrogen storage bottle.
[0116] As an embodiment, a groove 25 is provided at the bottom of the connection port, and the groove 25 is used to place the second sealing ring 41, and the bottom of the sealing block 22 abuts against the second sealing ring 41. The design of the second sealing ring 41 can further improve the sealing between the connector 21 and the sealing block 22, and cooperate with the first sealing ring 40 to double prevent hydrogen from leaking from the gap between the sealing block 22 and the connector 21. The design position of the groove 25 can also replace the second sealing ring 41 when the sealing block 22 is disassembled, thereby improving the replacement efficiency and maintenance convenience of the hydrogen storage cylinder parts.
[0117] As an embodiment, a connecting layer is further included between the outer circumference of the plastic liner 10 and the bottle mouth joint 20 and the winding layer, and the connecting layer is used to connect the winding layer, the plastic liner 10 and the bottle mouth joint 20. Figure 1-3 The connecting layer and the winding layer are not shown in the figure. The setting of the connecting layer can improve the connection strength between the above-mentioned plastic liner 10 and the bottle mouth joint 20 and the winding layer, and further improve the sealing and deformation resistance of the hydrogen storage cylinder.
[0118] Example 3
[0119] This embodiment relates to a method for preparing a filament-wound plastic liner hydrogen storage cylinder, comprising the following steps:
[0120] Making the plastic liner: mix the raw materials of the outer layer according to the ratio, and prepare the outer layer by rotational molding, then mix the raw materials of the inner layer according to the ratio, and then add the raw materials of the inner layer to the outer layer for rotational molding to form the inner layer, thus forming the plastic liner;
[0121] Assembly: Fix the fixing sleeve on the inner side of the bottle mouth, and then fit the bottle mouth joint into the buffer groove;
[0122] Slurry coating: The slurry is coated on the outer surface of the plastic liner and the bottle mouth joint, and heated and cured at 100°C for 8-10 hours to form a connecting layer. The thickness of the connecting layer is 0.5-0.6mm. The slurry includes 20-30 parts of diisocyanate, 1-2 parts of polyisocyanate, 0.5-1 parts of catalyst, 5-10 parts of ZIF-8, 70-80 parts of epoxy resin and 2-5 parts of imidazole curing agent by weight:
[0123] Winding: Wind the fiber on the outer peripheral surface of the connecting layer, heat and cure at 80-120°C for 2-6 hours to form a winding layer, the thickness of the winding layer is 25-30mm, and the fiber-wound plastic liner hydrogen storage cylinder is obtained. The fiber is a carbon fiber impregnated in an impregnating material, which includes 50-60 parts of water, 20-30 parts of ethanol, 40-60 parts of water-based epoxy resin and 5-10 parts of dopamine by weight, the pH of the slurry is 8-9, and the impregnation amount of the carbon fiber is 17-20wt%.
[0124] As a preferred solution, the impregnating material also includes 5-10 parts of a disulfide bond-containing amine chain extender, which is selected from any one or more of 4,4'-diaminodiphenyl disulfide, 3,3'-diaminodiphenyl disulfide, bis(2-aminophenyl) disulfide, and 4,4'-bis(2-amino-6-methylpyrimidinyl) disulfide.
[0125] The following steps of assembly, slurry coating and winding are performed based on the plastic liner 1# to obtain hydrogen storage cylinders 1#-9#, wherein the assembly steps are the same and will not be described in detail, and the slurry coating and winding steps are specifically as follows:
[0126] The preparation method of ZIF-8 used in the following is: zinc nitrate hexahydrate and 2-methylimidazole are dissolved in a methanol solution at a weight ratio of 1:2.5, and then the zinc nitrate hexahydrate solution is poured into the 2-methylimidazole solution and mixed and stirred for 10 hours. ZIF 8 is obtained after centrifugal separation, methanol washing, and drying.
[0127] Hydrogen storage tank 1#
[0128] The slurry is coated on the outer peripheral surface of the plastic liner and the bottle mouth joint, and heated and cured at 100°C for 8 hours to form a connecting layer with a thickness of 0.5 mm, wherein the slurry includes 25 parts of diisocyanate, 2 parts of polyisocyanate, 1 part of dibutyltin dilaurate, 8 parts of ZIF-8, 70 parts of epoxy resin and 4 parts of 2-methylimidazole; then the carbon fiber impregnated in the impregnating material is wound on the outer peripheral surface of the connecting layer, and heated and cured at 100°C for 5 hours to form a winding layer with a thickness of 30 mm, the impregnating material includes 550 parts of water, 250 parts of ethanol, 50 parts of water-based epoxy resin and 8 parts of dopamine, the pH of the slurry is 9, and the impregnation amount of the carbon fiber is 20wt%, so as to obtain hydrogen storage cylinder 1#.
[0129] Hydrogen storage tank 2#
[0130] The slurry is coated on the outer peripheral surface of the plastic liner and the bottle mouth joint, and heated and cured at 100°C for 10 hours to form a connecting layer with a thickness of 0.5 mm, wherein the slurry includes 20 parts of diisocyanate, 1 part of polyisocyanate, 0.5 parts of dibutyltin dilaurate, 5 parts of ZIF-8, 70 parts of epoxy resin and 2 parts of 2-methylimidazole; then the carbon fiber impregnated in the impregnating material is wound on the outer peripheral surface of the connecting layer, and heated and cured at 80°C for 6 hours to form a winding layer with a thickness of 25 mm, the impregnating material includes 500 parts of water, 300 parts of ethanol, 60 parts of water-based epoxy resin and 5 parts of dopamine, the pH of the slurry is 8, and the amount of carbon fiber impregnation is 17wt%, so as to obtain hydrogen storage cylinder 2#.
[0131] Hydrogen storage tank 3#
[0132] The slurry is coated on the outer peripheral surface of the plastic liner and the bottle mouth joint, and heated and cured at 100°C for 8 hours to form a connecting layer with a thickness of 0.6 mm, wherein the slurry includes 30 parts of diisocyanate, 2 parts of polyisocyanate, 1 part of dibutyltin dilaurate, 10 parts of ZIF-8, 80 parts of epoxy resin and 5 parts of 2-methylimidazole; thereafter, the carbon fiber impregnated in the impregnating material is wound on the outer peripheral surface of the connecting layer, and heated and cured at 120°C for 2 hours to form a winding layer with a thickness of 30 mm, the impregnating material includes 600 parts of water, 200 parts of ethanol, 40 parts of water-based epoxy resin and 10 parts of dopamine, the pH of the slurry is 9, and the impregnation amount of the carbon fiber is 20wt%, so as to obtain hydrogen storage cylinder 3#.
[0133] Hydrogen storage tank 4#
[0134] The difference between this hydrogen storage cylinder and hydrogen storage cylinder 1# is that the impregnating material also includes 5 parts of 4,4'-diaminodiphenyl disulfide, and the remaining ingredients and steps are the same as those of hydrogen storage cylinder 1#, so as to obtain hydrogen storage cylinder 4#.
[0135] Hydrogen storage tank 5#
[0136] The difference between this hydrogen storage cylinder and hydrogen storage cylinder 1# is that the impregnating material also includes 10 parts of 4,4'-bis(2-amino-6-methylpyrimidinyl) disulfide, and the remaining ingredients and steps are the same as those of hydrogen storage cylinder 1#, so as to obtain hydrogen storage cylinder 5#.
[0137] Hydrogen storage tank 6#
[0138] The difference between this hydrogen storage cylinder and hydrogen storage cylinder 1# is that the thickness of the connecting layer is 1.0 mm, and the remaining components and steps are the same as those of hydrogen storage cylinder 1#, so as to obtain hydrogen storage cylinder 6#.
[0139] Hydrogen storage tank 7#
[0140] The difference between this hydrogen storage cylinder and hydrogen storage cylinder 1# is that the thickness of the winding layer is 20 mm, and the remaining components and steps are the same as those of hydrogen storage cylinder 1#, so as to obtain hydrogen storage cylinder 7#.
[0141] Hydrogen storage tank 8#
[0142] The difference between this hydrogen storage cylinder and hydrogen storage cylinder 1# is that the slurry does not contain ZIF-8, and the remaining components and steps are the same as those of hydrogen storage cylinder 1#, that is, hydrogen storage cylinder 8# is obtained.
[0143] Hydrogen storage tank 9#
[0144] The difference between this hydrogen storage cylinder and hydrogen storage cylinder 1# is that the impregnating material does not contain dopamine, and the remaining ingredients and steps are the same as those of hydrogen storage cylinder 1#, so as to obtain hydrogen storage cylinder 9#.
[0145] The hydrogen storage cylinders 1#-9# prepared above were subjected to hydrogen permeability coefficient, deformation resistance test, fatigue life and peel strength test, wherein the deformation resistance test was carried out according to the external measurement method in GB / T 9251-2022, and the volume residual deformation rate of the hydrogen storage cylinder was calculated. The fatigue life was tested according to the T / CATSI02 007-2020 standard, and the hydrogen storage cylinders 1#-9# were cyclically inflated at 70MPa until the cylinders leaked, and the number of cycles when they finally leaked was recorded. In the peel strength test, the hydrogen storage cylinder is cut into strips with a width of 150mm×200mm, and the plastic liner and the winding layer are pre-peeled off 50mm along the length direction. The sample is placed in an environment with a temperature of 23±2℃ and a relative humidity of 50±5% for 4 days. The two ends of the peeled part of the sample are clamped on the upper and lower clamps of the tensile testing machine respectively, so that the peeled part of the sample is in a vertical state and the unpeeled part is in a horizontal state. The testing machine is turned on for peeling, and the test speed is set to 100mm / min. The peel strength is calculated.
[0146] The specific test results are shown in Table 2 below:
[0147] Table 2
[0148]
[0149]
[0150] The above hydrogen storage cylinder was subjected to corrosion resistance and chemical resistance tests. It was found that the above hydrogen storage cylinder could meet the corrosion resistance and chemical resistance requirements of hydrogen cylinders in the industry. In addition, the heat resistance of the hydrogen storage cylinder is also good, which can meet the temperature resistance requirements of automotive hydrogen storage cylinders.
[0151] In this embodiment, since a disulfide bond-containing amine chain extender is added to the impregnating material of hydrogen storage cylinders 4# and 5#, the bonding strength between the connecting layer and the winding layer can be further improved, thereby improving the hydrogen permeability resistance, deformation resistance and anti-delamination effects. In addition, the study found that when the winding layer of the hydrogen storage cylinder is scratched no more than 50μm, it can be heated to 120°C for 8h and repaired by more than 60%.
[0152] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0153] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included within the scope of the claims of the present application.
Claims
1. A filament-wound plastic liner hydrogen storage cylinder, characterized in that: include: A plastic liner, wherein the interior of the plastic liner is hollow to form a receiving cavity, a bottle mouth is opened on the top of the plastic liner, the bottle mouth is connected to the receiving cavity, and a shoulder seal of the plastic liner is recessed inward to form a buffer groove; A bottle mouth joint, the bottom shape of which matches the shape of the buffer groove, so that the bottle mouth joint is embedded in the buffer groove, the upper profile of the bottle mouth joint is smoothly transitioned with the shoulder seal of the plastic liner, a sealing opening is opened at the center of the bottle mouth joint, the lower end of the sealing opening is clamped on the outer side of the bottle mouth and sealed by a first sealing ring, and the upper end of the sealing opening is connected to a high-pressure gas cylinder valve; A fixing sleeve, which is arranged at the inner side of the bottle mouth and is used to support the bottle mouth, and the bottle mouth joint and the fixing sleeve are made of metal; A winding layer, wherein fibers are wound around the plastic liner and the outer peripheral surface of the bottle mouth joint to form the winding layer; The buffer groove is provided with at least two clamping surfaces in the circumference thereof, the bottle mouth joint is provided with a clamping part matched with the clamping surfaces in the circumference thereof, and the bottle mouth joint and the buffer groove are clamped together through the clamping surfaces and the clamping parts; or The top of the buffer groove is provided with a protrusion, the bottom of the bottle mouth joint is provided with a groove, and the bottle mouth joint and the buffer groove are engaged with each other through the protrusion and the groove; The bottle mouth joint comprises a connecting piece, a sealing pressing block and a locking nut; The bottom shape of the connecting piece matches the shape of the buffer groove, a connecting port is provided at the center of the connecting piece, the sealing block is connected to the connecting port through threads, a sealing port is provided at the center of the sealing block, and the locking nut is arranged at the top of the connecting piece and is connected to the outer periphery of the sealing block through threads; The bottle mouth, the sealing port and the connecting port are arranged on a common central axis; A groove is provided at the bottom of the connecting port, and the groove is used to place a second sealing ring. The bottom of the sealing pressing block abuts against the second sealing ring.
2. The filament-wound plastic liner hydrogen storage cylinder according to claim 1, characterized in that: The plastic liner comprises an inner layer and an outer layer, wherein the outer layer is arranged on the outer side of the inner layer; In parts by weight, the inner layer comprises 80-100 parts of PA11, 20-30 parts of diisocyanate, 3-5 parts of polyisocyanate, 10-20 parts of EVOH, 5-10 parts of mica flakes and 2-5 parts of plasticizer; In terms of weight, the outer layer comprises 80-100 parts of PA11, 30-50 parts of a compound containing two or more hydroxyl groups or a compound containing two or more amino groups, 10-20 parts of epoxy resin, 3-5 parts of anhydride curing agent, 2-5 parts of a plasticizer and 1-3 parts of a catalyst.
3. The filament-wound plastic liner hydrogen storage cylinder according to claim 2, characterized in that: The thickness of the mica flakes is 50-1000nm, and the flake diameter is 20-200μm.
4. The filament-wound plastic liner hydrogen storage cylinder according to claim 3, characterized in that: The mica flakes are mica flakes modified by butyl orthosilicate and dibutyl phthalate, and the preparation steps of the mica flakes modified by butyl orthosilicate and dibutyl phthalate are as follows: The mica flakes are washed and dried, placed in an ethanol solution for activation at 50-60°C for at least 3 hours, then the butyl orthosilicate and dibutyl phthalate are added to the ethanol solution, modified at 50-60°C for 2-3 hours, filtered and dried to obtain the mica flakes, wherein the butyl orthosilicate accounts for 2%-6% of the weight of the mica flakes, and the dibutyl phthalate accounts for 1%-2.5% of the weight of the mica flakes.
5. The filament-wound plastic liner hydrogen storage cylinder according to claim 2, characterized in that: Before the winding step, a slurry is coated on the outer circumference of the plastic liner and the bottle mouth joint to form a connecting layer. The winding layer is wound on the outer circumference of the connecting layer. The slurry includes 20-30 parts of diisocyanate, 1-2 parts of polyisocyanate, 0.5-1 parts of catalyst, 5-10 parts of ZIF-8, 70-80 parts of epoxy resin and 2-5 parts of imidazole curing agent by weight.
6. The filament-wound plastic liner hydrogen storage cylinder according to claim 2, characterized in that: The acid anhydride curing agent is 3,3'-dithiodipropionic anhydride; The compound containing two or more hydroxyl groups is selected from at least one of 1,4-butanediol, glycerol, diethylene glycol, 4,4'-dihydroxydiphenyl sulfide, and 3,3'-dihydroxydiphenyl disulfide; The compound containing two or more amino groups is selected from at least one of ethylenediamine, 1,2-propylenediamine, 1,6-hexanediamine, p-phenylenediamine, 2,3-diaminopyridine, 3,3'-iminobis-1-propanol, 4,4'-diaminodiphenyl disulfide, and 3,3'-diaminodiphenyl disulfide.
7. The filament-wound plastic liner hydrogen storage cylinder according to claim 2, characterized in that: The inner layer and the outer layer are made by a rotational molding process, so that the outer layer is coated on the outer side of the inner layer.
Citation Information
Cited By
Hot water container and manufacturing method thereof
CN121655127A