Catalyst for preparing unsaturated carbonate, preparation method and application thereof

Through the composite catalyst of titanium silicon molecular sieve-zinc metal organic framework compound, the problem of low conversion and selectivity of unsaturated carbonate in direct synthesis is solved, and high efficiency and high selectivity of unsaturated carbonate synthesis is achieved, especially in Extremely high catalytic performance under specific conditions.

CN116020560BActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111241475.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-25
Publication Date
2024-11-01
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

The current direct synthesis method has low conversion and selectivity for the preparation of unsaturated carbonates and lacks catalysts with high activity and good selectivity.

Method used

Using titanium silicon molecular sieve-zinc metal organic frame compound composite catalyst, a catalyst with a molar ratio of titanium silicon molecular sieve and zinc metal organic frame compound was prepared with a molar ratio of titanium and zinc element of 0.6-1.2:1, and a specific preparation method was used. Improve the performance of the catalyst.

Benefits of technology

The high conversion and selectivity of the direct synthesis of unsaturated carbonate between olefins and carbon dioxide is achieved. The catalyst has the characteristics of short process flow, high efficiency and low energy consumption, especially under specific conditions, which can achieve a styrene conversion rate of 99.8% and 99.9% selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116020560B_ABST
    Figure CN116020560B_ABST
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing unsaturated carbonate, a preparation method and application thereof. The catalyst is a titanium silicon molecular sieve-zinc metal organic framework compound composite catalyst, wherein, in the catalyst, the molar ratio of titanium element to zinc element is 0.6-1.2:1. The catalyst of the invention is used for directly preparing unsaturated carbonate from olefin and carbon dioxide, has a short production process, high efficiency, low energy consumption, and has the characteristics of outstanding catalytic performance, high conversion rate and high selectivity of unsaturated carbonate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparing unsaturated carbonate esters, and in particular to a catalyst for preparing unsaturated carbonate esters, a preparation method thereof and an application thereof. Background Art

[0002] Considering the fixation of chemical carbon dioxide and considering the use of carbon dioxide as a carbon source, research has been actively carried out, and among them, unsaturated carbonates are a class of excellent solvents and fine chemical intermediates, and are potential basic raw materials for organic chemical industry.

[0003] In the prior art, the synthesis of unsaturated carbonates by reacting epoxy compounds with CO2 is a good fixation method. The process reaction equation is as follows:

[0004] Wherein R is an alkyl group or an aromatic group.

[0005] In this catalytic system, most of them use binary homogeneous catalysts composed of Lewis acid metal compounds and Lewis bases. Among them, the homogeneous catalytic systems used in the early stage are mainly Lewis acid metal compounds including alkaline (earth) metal halides, transition metal salts, transition metals or main group metal complexes, and the Lewis bases used are organic bases (such as DMF, DMAP, etc.), quaternary ammonium salts, quaternary phosphonium salts, imidazole salts, crown ethers, etc. The later heterogeneous catalytic systems include metal oxide systems (such as CeO2-ZrO2, alkaline zeolite systems (such as Cs / KX), etc. In the process route, the preparation process of epoxy compounds mainly comes from the oxidation of olefins. Therefore, in fact, the process flow of unsaturated carbonates is based on the oxidation of olefins, and after obtaining the intermediate raw material epoxy compound, it is obtained through the addition reaction of carbon dioxide.

[0006] Another method is to directly prepare unsaturated carbonates using olefins and carbon dioxide as raw materials, that is, in the presence of an oxidant, olefins react with carbon dioxide to form cyclic unsaturated carbonates. The reaction equation is as follows:

[0007] Wherein R is an alkyl group or an aromatic group.

[0008] From the perspective of economic benefits and energy utilization, the direct synthesis method using olefins as the initial raw material has more practical application value than the general synthesis method using epoxides as the initial raw materials. On the one hand, olefins are cheaper and more widely available; on the other hand, the direct synthesis method can greatly reduce the separation steps of intermediate products. However, the current problem with the direct synthesis method is that the yield and selectivity of the product are not high. Therefore, the development of a direct synthesis catalyst with high activity and selectivity has always been a difficult problem to be solved in this field. Summary of the invention

[0009] In order to solve the problem of low conversion rate and selectivity in the preparation of unsaturated carbonate by direct synthesis in the prior art, the present invention provides a catalyst for preparing unsaturated carbonate and its preparation method and application. The catalyst of the present invention is used for directly preparing unsaturated carbonate from olefin and carbon dioxide, has short production process, high efficiency, low energy consumption, and has outstanding catalytic performance, high conversion rate and high selectivity of unsaturated carbonate.

[0010] The first aspect of the present invention provides a catalyst for preparing unsaturated carbonates, which is a titanium silicon molecular sieve-zinc metal organic framework compound composite catalyst, wherein in the catalyst, the molar ratio of titanium element to zinc element is 0.6-1.2:1.

[0011] In the technical solution of the above catalyst, preferably, the titanium content in the titanium silicon molecular sieve is 0.01-5% by weight, preferably 0.1-3% by weight, such as 0.01% by weight, such as 0.05% by weight, such as 1% by weight, such as 1.5% by weight, such as 2% by weight, such as 2.5% by weight, such as 3% by weight, such as 3.5% by weight, such as 4% by weight, such as 4.5% by weight, such as 5% by weight, and any value therebetween.

[0012] In the technical solution of the above catalyst, preferably, the zinc metal organic framework compound includes but is not limited to MOF-177, MOF-38, and ZIF-8, and further preferably, the zinc metal organic framework compound is ZIF-8.

[0013] In the technical solution of the above catalyst, preferably, in the process of preparing the catalyst, the titanium silicon molecular sieve is obtained by mixing the titanium silicon molecular sieve as it is with a nitric acid solution and sequentially performing a temperature rising and standing treatment, separation, washing, drying and calcining in an air atmosphere. The titanium silicon molecular sieve of the present invention has a higher degree of exposure of titanium on its surface and a slightly different structural form.

[0014] The second aspect of the present invention provides a method for preparing a catalyst for preparing unsaturated carbonates, comprising: mixing a titanium silicon molecular sieve with a zinc metal organic framework compound; wherein the titanium silicon molecular sieve is obtained by mixing the titanium silicon molecular sieve as it is with a nitric acid solution and sequentially subjecting the mixture to a temperature rising and standing treatment, separation, washing, drying and calcining in an air atmosphere.

[0015] In the above technical solution, preferably, the preparation method comprises:

[0016] (1) mixing and crystallizing a silicon source, a titanium source, an organic template, an alkali and water, and filtering, washing and drying the crystallized product to obtain a titanium silicon molecular sieve as is; mixing the titanium silicon molecular sieve as is with a nitric acid solution and sequentially performing a temperature-raising and standing treatment, separation, drying and calcining in an air atmosphere to obtain a titanium silicon molecular sieve;

[0017] (2) mixing a zinc precursor and 2-methylimidazole, sealing, and sequentially performing a hydrothermal reaction, filtering, and drying to obtain a zinc metal organic framework compound;

[0018] (3) Mixing the titanium silicon molecular sieve obtained in step (1) and the zinc metal organic framework compound obtained in step (2).

[0019] In the present invention, there is no order of precedence for the above steps (1) and (2). Step (1) may be performed first and then step (2), step (2) may be performed first and then step (1), or step (1) and step (2) may be performed simultaneously.

[0020] In the technical solution of the above preparation method, preferably, the concentration of nitric acid is 0.5-3 mol / L, such as 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, and any value therebetween.

[0021] In the technical solution of the above preparation method, preferably, the weight ratio of the titanium silicon molecular sieve to nitric acid is 1:20-40, for example, 1:20, 1:22, 1:24, 1:26, 1:28, 1:30, 1:32, 1:34, 1:36, 1:38, 1:40, etc.

[0022] In the technical solution of the above preparation method, preferably, the conditions for the temperature rising and standing treatment include: a temperature of 80-100° C. and a time of 4-48 h.

[0023] In the technical solution of the above preparation method, preferably, the calcination conditions include: temperature of 400-700°C and time of 4-24h.

[0024] In the technical solution of the above preparation method, preferably, the titanium content in the titanium silicon molecular sieve is 0.01-5% by weight, such as 0.01% by weight, such as 0.05% by weight, such as 1% by weight, such as 1.5% by weight, such as 2% by weight, such as 2.5% by weight, such as 3% by weight, such as 3.5% by weight, such as 4% by weight, such as 4.5% by weight, such as 5% by weight, and any value therebetween.

[0025] In the technical solution of the above preparation method, preferably, the silicon source is selected from at least one of silica sol, silicate and solid silicon oxide.

[0026] In the technical solution of the above preparation method, preferably, the titanium source is selected from at least one of titanium tetrachloride, titanium trichloride, titanium chlorate and titanium sulfate.

[0027] In the technical solution of the above preparation method, preferably, the organic template is selected from at least one of tetrapropylammonium hydroxide, tetrapropylammonium bromide, tetrabutylammonium hydroxide, tetrabutylammonium bromide and tetraethylammonium bromide.

[0028] In the technical scheme of the above preparation method, preferably, the base used is selected from at least one of ammonia water, ethylamine, n-propylamine, n-butylamine, ethylenediamine, hexamethylenediamine and tripropylamine.

[0029] In the technical solution of the above preparation method, preferably, the zinc precursor is selected from at least one of zinc nitrate, zinc chloride and zinc sulfate.

[0030] In the technical solution of the above preparation method, preferably, the molar ratio of the silicon source, the titanium source, the organic template, the base and the water is 1:0.01-0.03:0.03-0.15:0.4-2:20-100.

[0031] In the technical solution of the above preparation method, preferably, the crystallization conditions include: a temperature of 160-220° C. and a crystallization time of 1-30 days.

[0032] In the technical solution of the above preparation method, preferably, the molar ratio of the zinc precursor to 2-methylimidazole is 1:1-2, for example, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, etc.

[0033] In the technical solution of the above preparation method, preferably, the conditions of the hydrothermal reaction include: temperature of 60-200° C. and time of 1-24 h.

[0034] In the technical solution of the above preparation method, preferably, in step (3), the molar ratio of titanium element to zinc element is 0.6-1.2:1, for example, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, etc.

[0035] In the present invention, there is no limitation on the equipment for mixing and reacting, which can be any device that can achieve mixing or reacting in the art. For example, the equipment for mixing and reacting can be a reactor or a reaction kettle.

[0036] In the present invention, there is no limitation on the filtration and drying in steps (1) and (2), and any existing method that can achieve filtration and drying can be used. The drying temperature is preferably 60-150° C., and the drying temperature is 100° C. in the embodiment of the present invention for exemplary description, but the present invention is not limited thereto. The present invention does not particularly limit the drying time, as long as the solvent can be removed, and those skilled in the art can make appropriate selections according to actual conditions.

[0037] In the present invention, in the process of mixing the titanium silicon molecular sieve as is with the nitric acid solution and sequentially subjecting it to temperature rising and standing treatment, separation, drying and calcination in air atmosphere, washing may or may not be performed between separation and drying, but the washing is preferably performed.

[0038] In the present invention, in step (2), during the hydrothermal reaction, filtration and drying, washing may or may not be performed between filtration and drying, but the washing is preferably performed. In the present invention, there is no limitation on the washing in step (2), as long as the purpose of washing can be achieved.

[0039] A specific implementation of the above preparation method may include but is not limited to:

[0040] (1) After a silicon source, a titanium source, an organic template, an alkali and water are uniformly mixed in a stoichiometric ratio, after crystallization, the product is filtered, washed with water and dried to obtain a titanium silicon molecular sieve as is; after the obtained titanium silicon molecular sieve as is is mixed with a nitric acid solution, the temperature is raised and allowed to stand for treatment, the solid is separated and then washed, dried, and then calcined in an air atmosphere to obtain a titanium silicon molecular sieve;

[0041] (2) mixing the zinc precursor and 2-methylimidazole, stirring, sealing, performing a hydrothermal reaction, filtering, and drying to obtain a zinc metal organic framework compound;

[0042] (3) The solid titanium silicon molecular sieve obtained in step (1) and the zinc metal organic framework compound obtained in step (2) are mixed to obtain a composite catalyst system.

[0043] The third aspect of the present invention provides a catalyst for preparing unsaturated carbonate prepared according to the above preparation method, wherein in the catalyst, the molar ratio of titanium element to zinc element is 0.6-1.2:1.

[0044] In the technical solution of the above catalyst, preferably, the titanium content in the titanium silicon molecular sieve is 0.01-5% by weight, such as 0.01% by weight, such as 0.05% by weight, such as 1% by weight, such as 1.5% by weight, such as 2% by weight, such as 2.5% by weight, such as 3% by weight, such as 3.5% by weight, such as 4% by weight, such as 4.5% by weight, such as 5% by weight, and any value therebetween.

[0045] The fourth aspect of the present invention provides a method for preparing unsaturated carbonates, comprising: using olefins, an oxidant and carbon dioxide as raw materials, contacting the raw materials with a catalyst for reaction to obtain unsaturated carbonates, wherein the catalyst is the above-mentioned catalyst or a catalyst prepared according to the above-mentioned preparation method.

[0046] In the above technical scheme for preparing unsaturated carbonate, preferably, the reaction temperature is 30-200°C.

[0047] In the above technical solution of the method for preparing unsaturated carbonate, preferably, the reaction pressure is 0.1-10 MPa.

[0048] In the above-mentioned technical scheme for preparing unsaturated carbonate, preferably, the reaction time is 1-24h.

[0049] In the above technical solution for preparing unsaturated carbonate, preferably, the molar ratio of olefin, oxidant and titanium element in the catalyst is 1:0.5-5:0.0001-1.

[0050] In the above-mentioned technical scheme for preparing unsaturated carbonates, preferably, the olefin is an alkyl olefin or an aromatic olefin, such as ethylene, propylene, butylene, butadiene, styrene, allyl chloride, chlorostyrene, etc.; the oxidant is oxygen or peroxide, wherein the peroxide includes but is not limited to cumene peroxide, tert-butyl peroxide, hydrogen peroxide, etc.

[0051] Beneficial effects of the present invention:

[0052] (1) The catalyst provided by the present invention has a specific composition and is a co-metal-zinc metal organic framework compound composite catalytic system. The metal particle size is small and when used for the direct synthesis of unsaturated carbonates, excellent conversion rate and unsaturated carbonate selectivity can be obtained.

[0053] (2) When the catalyst of the present invention is used for direct synthesis of unsaturated carbonates from styrene and carbon dioxide, especially under the conditions of a reaction temperature of 100° C., a pressure of 3 MPa, and a reaction time of 12 h, the styrene conversion rate and product selectivity can reach a maximum of 99.8% and 99.9%, respectively. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is the XRD diagram of the sample provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0055] In order to make the present invention more easily understood, the present invention will be described in detail below in conjunction with embodiments. These embodiments are only for illustration and are not intended to limit the application scope of the present invention.

[0056] In the present invention, XRD is measured on a Bruker D8 AdvanceSS X-ray diffractometer, with CuKα radiation, 40 kV, 300 mA, and a scanning speed of 2° / min. The structure of the catalyst prepared in the present invention can be measured by XRD characterization analysis.

[0057] [Example 1]

[0058] Silica sol (40 wt%), titanium tetrachloride, tetrapropylammonium hydroxide, ammonia water and water were stirred and mixed in a stoichiometric ratio (molar ratio) of 1:0.01:0.03:0.4:20, and crystallized at 180°C for 20 days. The product was filtered, washed with water and dried to obtain a silicon-titanium molecular sieve as is. The obtained silicon-titanium molecular sieve as is was mixed with a 2 mol / L nitric acid solution in a weight ratio of 1:30, and the mixture was heated to 85°C and allowed to stand for 24 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 500°C in an air atmosphere for 12 hours to obtain a titanium silicon molecular sieve Ti-Si-1, wherein the titanium content was 2.5 wt%.

[0059] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, carry out hydrothermal reaction at 160 ° C for 18 hours, filter, wash with methanol, dry at 100 ° C, cool to room temperature, take out the sample and obtain the zinc metal organic metal framework compound Zn-ZIF-1.

[0060] The obtained Ti-Si-1 and Zn-ZIF-1 were mixed in a molar ratio of titanium element to zinc element of 1:1 to obtain catalyst S1. XRD characterization analysis was performed on catalyst S1. Figure 1 shown.

[0061] [Example 2]

[0062] Ti-Si-1 and Zn-ZIF-1 were prepared according to the method of Example 1. The obtained Ti-Si-1 and Zn-ZIF-1 were mixed at a molar ratio of titanium element:zinc element of 0.9:1 to obtain catalyst sample S2.

[0063] [Example 3]

[0064] Ti-Si-1 and Zn-ZIF-1 were prepared according to the method of Example 1. The obtained Ti-Si-1 and Zn-ZIF-1 were mixed at a molar ratio of titanium element:zinc element of 1.1:1 to obtain catalyst sample S3.

[0065] [Example 4]

[0066] Methyl orthosilicate, tetrabutyl titanate, tetrabutylammonium bromide, ammonia water and water were stirred and mixed in a stoichiometric ratio of 1:0.02:0.06:0.8:20, and crystallized at 200°C for 15 days. The product was filtered, washed with water and dried to obtain a silicon titanium molecular sieve as is. The obtained silicon titanium molecular sieve as is was mixed with a 2 mol / L nitric acid solution in a weight ratio of 1:25, and the mixture was heated to 80°C and allowed to stand for 40 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 500°C in an air atmosphere for 12 hours to obtain a titanium silicon molecular sieve Ti-Si-4, wherein the titanium content was 2.4 wt%.

[0067] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, carry out hydrothermal reaction at 160 ° C for 18 hours, filter, wash with methanol, dry at 100 ° C, cool to room temperature, take out the sample and obtain the zinc metal organic metal framework compound Zn-ZIF-4.

[0068] The obtained Ti-Si-4 and Zn-ZIF-4 were mixed in a molar ratio of titanium element:zinc element of 1:1 to obtain catalyst S4.

[0069] [Example 5]

[0070] Methyl orthosilicate, tetrabutyl titanate, tetrabutylammonium bromide, ammonia water and water were stirred and mixed in a stoichiometric ratio of 1:0.02:0.06:0.8:20, and the mixture was crystallized at 200°C for 15 days. The product was filtered, washed with water and dried to obtain a silicon titanium molecular sieve as is. The silicon titanium molecular sieve as is obtained was mixed with a 1.5 mol / L nitric acid solution in a weight ratio of 1:30, and the mixture was heated to 90°C and allowed to stand for 36 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 550°C in an air atmosphere for 12 hours to obtain a titanium silicon molecular sieve Ti-Si-5, wherein the titanium content was 2.4 wt%.

[0071] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, carry out hydrothermal reaction at 160 ° C for 18 hours, filter, wash with methanol, dry at 100 ° C, cool to room temperature, take out the sample and obtain the zinc metal organic metal framework compound Zn-ZIF-5.

[0072] The obtained Ti-Si-5 and Zn-ZIF-5 were mixed at a molar ratio of titanium element:zinc element of 1.1:1 to obtain catalyst S5.

[0073] [Example 6]

[0074] Ethyl orthosilicate, tetrabutyl titanate, tetrabutylammonium bromide, diamine and water were stirred and mixed in a stoichiometric ratio of 1:0.02:0.06:0.8:20, and crystallized at 200°C for 15 days. The product was filtered, washed with water and dried to obtain a silicon-titanium molecular sieve as is. The obtained silicon-titanium molecular sieve as is was mixed with a 3 mol / L nitric acid solution in a weight ratio of 1:22, and the mixture was heated to 90°C and allowed to stand for 36 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 600°C in an air atmosphere for 12 hours to obtain a titanium silicon molecular sieve Ti-Si-6, wherein the titanium content was 2.5 wt%.

[0075] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, carry out hydrothermal reaction at 160 ° C for 18 hours, filter, wash with methanol, dry at 100 ° C, cool to room temperature, take out the sample and obtain the zinc metal organic metal framework compound Zn-ZIF-6.

[0076] The obtained Ti-Si-6 and Zn-ZIF-6 were mixed at a molar ratio of titanium element:zinc element of 0.9:1 to obtain catalyst S6.

[0077] [Example 7]

[0078] Ti-Si-1 and Zn-ZIF-1 were prepared according to the method of Example 1. The obtained Ti-Si-1 and Zn-ZIF-1 were mixed at a molar ratio of titanium element:zinc element of 0.6:1 to obtain catalyst sample S7.

[0079] [Example 8]

[0080] Ti-Si-1 and Zn-ZIF-1 were prepared according to the method of Example 1. The obtained Ti-Si-1 and Zn-ZIF-1 were mixed at a molar ratio of titanium element:zinc element of 1.2:1 to obtain catalyst sample S8.

[0081] [Example 9]

[0082] Ti-Si-1 was prepared according to the method of Example 1, except that the conditions for heating and standing were different, namely:

[0083] Silica sol (40 wt%), titanium tetrachloride, tetrapropylammonium hydroxide, ammonia water and water were stirred and mixed in a stoichiometric ratio (molar ratio) of 1:0.01:0.03:0.4:20, and then crystallized at 180°C for 20 days. The product was filtered, washed with water and dried to obtain the silicon-titanium molecular sieve as is. The obtained silicon-titanium molecular sieve as is was mixed with a 2 mol / L nitric acid solution in a weight ratio of 1:30, and then heated to 100°C and allowed to stand for 24 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 500°C in an air atmosphere for 12 hours to obtain titanium silicon molecular sieve Ti-Si-9.

[0084] Then, Zn-ZIF-1 was prepared according to the method of Example 1. The obtained Ti-Si-9 and Zn-ZIF-1 were mixed in a molar ratio of titanium element:zinc element of 1:1 to obtain catalyst sample S9.

[0085] [Example 10]

[0086] Ti-Si-1 was prepared according to the method of Example 1, except that the conditions for heating and standing were different, namely:

[0087] Silica sol (40 wt%), titanium tetrachloride, tetrapropylammonium hydroxide, ammonia water and water were stirred and mixed in a stoichiometric ratio (molar ratio) of 1:0.01:0.03:0.4:20, and then crystallized at 180°C for 20 days. The product was filtered, washed with water and dried to obtain the silicon-titanium molecular sieve as is. The obtained silicon-titanium molecular sieve as is was mixed with a 2 mol / L nitric acid solution in a weight ratio of 1:30, and then heated to 85°C and allowed to stand for 4 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 500°C in an air atmosphere for 12 hours to obtain titanium silicon molecular sieve Ti-Si-10.

[0088] Then, Zn-ZIF-1 was prepared according to the method of Example 1. The obtained Ti-Si-10 and Zn-ZIF-1 were mixed in a molar ratio of titanium element:zinc element of 1:1 to obtain a catalyst sample S10.

[0089] [Example 11]

[0090] Ti-Si-1 was prepared according to the method of Example 1, except that the obtained silicon titanium molecular sieve was replaced with 1:40 at a weight ratio of 1:30 to obtain titanium silicon molecular sieve Ti-Si-11.

[0091] Then, Zn-ZIF-1 was prepared according to the method of Example 1. The obtained Ti-Si-11 and Zn-ZIF-1 were mixed in a molar ratio of titanium element:zinc element of 1:1 to obtain a catalyst sample S11.

[0092] [Comparative Example 1]

[0093] Silica sol (40 wt %), titanium tetrachloride, tetrapropylammonium hydroxide, ammonia water and water were stirred and mixed in a stoichiometric ratio of 1:0.01:0.03:0.4:20, and crystallized at 180°C for 20 days. The product was filtered, washed with water and dried to obtain the silicon-titanium molecular sieve as is. The obtained silicon-titanium molecular sieve as is was mixed with a 2 mol / L nitric acid solution in a weight ratio of 1:30, and the mixture was heated to 85°C and allowed to stand for 24 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 500°C in an air atmosphere for 12 hours to obtain catalyst D1.

[0094] [Comparative Example 2]

[0095] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, conduct hydrothermal reaction at 160°C for 18 hours, filter, wash with methanol, dry at 100°C, and cool to room temperature to obtain catalyst D2.

[0096] [Comparative Example 3]

[0097] Silica sol (40 wt %), titanium tetrachloride, tetrapropylammonium hydroxide, ammonia water and water were stirred and mixed in a stoichiometric ratio of 1:0.01:0.03:0.4:20, and then crystallized at 180°C for 20 days. The product was filtered, washed with water and dried to obtain the silicon titanium molecular sieve as is. The obtained silicon titanium molecular sieve as is was mixed with a 2 mol / L nitric acid solution in a weight ratio of 1:30, and then heated to 85°C and allowed to stand for 24 hours. The solid was separated and washed, and dried at 100°C overnight to obtain an acid-treated sample, which was then calcined at 500°C in an air atmosphere for 12 hours to obtain a titanium silicon molecular sieve Ti-Si-D3.

[0098] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, carry out hydrothermal reaction at 160 ° C for 18 hours, filter, wash with methanol, dry at 100 ° C, cool to room temperature, take out the sample and obtain the zinc metal organic metal framework compound Zn-ZIF-D3.

[0099] The obtained Ti-Si-D3 and Zn-ZIF-D3 were mixed at a molar ratio of titanium element:zinc element of 0.4:1 to obtain catalyst D3.

[0100] [Comparative Example 4]

[0101] Silica sol (40 wt %), titanium tetrachloride, tetrapropylammonium hydroxide, ammonia water and water were stirred and mixed in a stoichiometric ratio of 1:0.01:0.03:0.4:20, and then crystallized at 180° C. for 20 days. The product was filtered, washed with water and dried to obtain the silicon-titanium molecular sieve as is. The obtained silicon-titanium molecular sieve as is was mixed with a 2 mol / L nitric acid solution in a weight ratio of 1:30, and then heated to 85° C. and allowed to stand for 24 hours. The solid was separated and washed, and dried at 100° C. overnight to obtain an acid-treated sample, which was then calcined at 500° C. in an air atmosphere for 12 hours to obtain a titanium silicon molecular sieve Ti-Si-D4.

[0102] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, carry out hydrothermal reaction at 160 ° C for 18 hours, filter, wash with methanol, dry at 100 ° C, cool to room temperature, take out the sample and obtain the zinc metal organic metal framework compound Zn-ZIF-D4.

[0103] The obtained Ti-Si-D4 and Zn-ZIF-D4 were mixed at a molar ratio of titanium element to zinc element of 2:1 to obtain catalyst D4.

[0104] [Comparative Example 5]

[0105] Silica sol (40 wt%), titanium tetrachloride, tetrapropylammonium hydroxide, ammonia water and water were stirred and mixed in a stoichiometric ratio of 1:0.01:0.03:0.4:20, and crystallized at 180°C for 20 days. The product was filtered, washed with water, dried, and then calcined at 500°C in an air atmosphere for 12 hours to obtain titanium silicon molecular sieve Ti-Si-D5.

[0106] In a 50 ml beaker, add 1.4 g of zinc nitrate and stir, then add 0.4 g of 2-methylimidazole, stir and seal, carry out hydrothermal reaction at 160 ° C for 18 hours, filter, wash with methanol, dry at 100 ° C, cool to room temperature, take out the sample and obtain the zinc metal organic metal framework compound Zn-ZIF-D5.

[0107] The obtained Ti-Si-D5 and Zn-ZIF-D5 were mixed at a molar ratio of titanium element to zinc element of 1:1 to obtain catalyst D5.

[0108]

Test example

[0109] The catalysts of Examples 1-11 and Comparative Examples 1-5 were evaluated respectively.

[0110] 0.05g of the prepared catalyst, 2.08g of tert-butyl peroxide and 2.08g of styrene were placed in a 50ml high-pressure reactor, and the reactor was heated to 100°C, and carbon dioxide was introduced to maintain the system pressure at 3MPa, and the reaction was carried out for 12h. After the reaction was completed, the heating was turned off, and the lid of the reactor was opened after cooling to room temperature. The reactor liquid was taken for analysis on a gas chromatograph, and the styrene conversion rate and the product styrene carbonate selectivity were calculated based on the measurement results. The results are shown in Table 1.

[0111] Table 1

[0112]

[0113]

[0114] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this field, under the technical enlightenment provided by the present invention, as common knowledge in the field, other equivalent variations and improvements can also be made, which should also be regarded as the protection scope of the present invention.

Claims

1. A catalyst for preparing unsaturated carbonate, the catalyst being a titanium silicon molecular sieve-zinc metal organic framework compound composite catalyst, wherein: In the catalyst, the molar ratio of titanium element to zinc element is 0.6-1.2:

1. The titanium content in the titanium silicon molecular sieve is 0.01-5% by weight.

2. The catalyst according to claim 1, characterized in that The titanium silicon molecular sieve is obtained by mixing the titanium silicon molecular sieve as it is with a nitric acid solution and sequentially subjecting the mixture to a temperature-raising and standing treatment, separation, drying and calcination in an air atmosphere.

3. A method for preparing a catalyst for preparing unsaturated carbonate according to claim 1 or 2, comprising: The titanium silicon molecular sieve is mixed with a zinc metal organic framework compound; wherein the titanium silicon molecular sieve is obtained by mixing the titanium silicon molecular sieve as it is with a nitric acid solution and sequentially subjecting the mixture to a temperature-raising and standing treatment, separation, drying and calcination in an air atmosphere.

4. The preparation method according to claim 3, characterized in that: The preparation method comprises: (1) mixing and crystallizing a silicon source, a titanium source, an organic template, an alkali and water, and filtering, washing and drying the crystallized product to obtain a titanium silicon molecular sieve as is; mixing the titanium silicon molecular sieve as is with a nitric acid solution and sequentially performing a temperature-raising and standing treatment, separation, drying and calcining in an air atmosphere to obtain a titanium silicon molecular sieve; (2) mixing a zinc precursor and 2-methylimidazole, sealing, and sequentially performing a hydrothermal reaction, filtering, and drying to obtain a zinc metal organic framework compound; (3) Mixing the titanium silicon molecular sieve obtained in step (1) and the zinc metal organic framework compound obtained in step (2).

5. The preparation method according to claim 3 or 4, characterized in that: The nitric acid concentration is 0.5-3 mol / L; and / or, The weight ratio of the titanium silicate molecular sieve to nitric acid is 1:20-40; and / or, The conditions for the temperature rising and standing treatment include: a temperature of 80-100° C. and a time of 4-48 hours; and / or, The calcination conditions include: temperature of 400-700° C. and time of 4-24 hours.

6. The preparation method according to claim 4, characterized in that: The silicon source is selected from at least one of silica sol, silicate and solid silicon oxide; and / or, The titanium source is selected from at least one of titanium tetrachloride, titanium trichloride, titanium chlorate and titanium sulfate; and / or, The organic template is selected from at least one of tetrapropylammonium hydroxide, tetrapropylammonium bromide, tetrabutylammonium hydroxide, tetrabutylammonium bromide and tetraethylammonium bromide; and / or, The base used is at least one selected from ammonia water, ethylamine, n-propylamine, n-butylamine, ethylenediamine, hexamethylenediamine and tripropylamine; and / or, The zinc precursor is selected from at least one of zinc nitrate, zinc chloride and zinc sulfate.

7. The preparation method according to claim 4, characterized in that: The molar ratio of the silicon source, the titanium source, the organic template, the base and the water is 1:0.01-0.03:0.03-0.15:0.4-2:20-100; and / or, The crystallization conditions include: a temperature of 160-220° C. and a crystallization time of 1-30 days; The molar ratio of the zinc precursor to 2-methylimidazole is 1:1-2; and / or, The conditions of the hydrothermal reaction include: temperature of 60-200° C., time of 1-24 h; and / or, In step (3), the molar ratio of titanium element to zinc element is 0.6-1.2:

1.

8. A method for preparing unsaturated carbonate, comprising: Olefin, oxidant and carbon dioxide are used as raw materials, and the raw materials are contacted with a catalyst for reaction to obtain an unsaturated carbonate, wherein the catalyst is the catalyst according to any one of claims 1 to 2 or the catalyst prepared according to the preparation method according to any one of claims 3 to 7.

9. The method according to claim 8, characterized in that The reaction temperature is 30-200° C.; and / or, the reaction pressure is 0.1-10 MPa; and / or, the reaction time is 1-24 h.

10. The method according to claim 8 or 9, characterized in that: The molar ratio of olefin, oxidant and titanium element in the catalyst is 1:0.5-5:0.0001-1.