Catalyst for olefin polymerization, catalyst system and application thereof, and olefin polymerization method
By using a catalyst prepared from sulfur-containing magnesium compounds and α-cyanosuccinate compounds, the problems of narrow molecular weight distribution and long settling time of existing catalysts were solved, achieving olefin polymerization with high activity and wide molecular weight distribution, and improving production stability and processing performance.
Patent Information
- Application Number
- CN202111258057.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-27
AI Technical Summary
Existing olefin polymerization catalysts suffer from narrow molecular weight distribution and long polymer particle settling time, which affect production stability and processing performance.
A novel catalyst system was prepared by using a sulfur-containing magnesium compound as a support and an α-cyanosuccinate compound as an internal electron donor. By combining an alkylaluminum compound and an external electron donor, the catalyst particle size was controlled to be less than 30 micrometers, and the catalyst morphology and molecular weight distribution were optimized.
This resulted in catalysts with small particle size, high activity, and wide molecular weight distribution, as well as short polymer fall time, thereby improving production stability and polymer processing performance.
Smart Images

Figure BDA0003324735030000011 
Figure BDA0003324735030000021 
Figure BDA0003324735030000031
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a catalyst for olefin polymerization, a catalyst system and its application, and an olefin polymerization method. Background Art
[0002] Molecular weight distribution affects the performance of polypropylene resin. Generally speaking, polypropylene resin with wide molecular weight distribution has better processing performance and mechanical properties, and achieves a better balance of rigidity and toughness. In recent years, the polypropylene industry has developed rapidly, and competition has also intensified. Therefore, seeking polypropylene resin with special properties has become the goal of many manufacturers. At the same time, polypropylene manufacturers are also working hard to use catalysts with better process performance to achieve long-term stable production. Generally speaking, small-particle carriers can not only reduce the fine powder of the polymer obtained by the prepared catalyst, but also can be widely used in various gas-phase polymerization processes.
[0003] The falling time of polymer particles is also one of the important indicators of catalyst performance. If the falling time of polymer particles is too long, it will often cause bridging or poor material discharge in the reactor, affecting production stability and even causing production suspension.
[0004] Therefore, it is of great significance to develop a new olefin polymerization catalyst having special properties and being able to overcome the defects of the prior art. Summary of the invention
[0005] In order to solve the above problems in the prior art, the present invention proposes a catalyst for olefin polymerization, a catalyst system and its application and an olefin polymerization method.
[0006] In a first aspect, the present invention provides a catalyst for olefin polymerization, comprising component A and component B;
[0007] The component A is a carrier, specifically a sulfur-containing magnesium compound, and its structure is shown in formula (I).
[0008]
[0009] In formula (I), R1 is a C1-C8 straight-chain alkyl group, a C3-C8 branched-chain alkyl group, or a C3-C8 cycloalkyl group;
[0010] R2 and R3 are the same or different, and are each independently hydrogen, a C1-C5 straight chain alkyl group, or a C3-C5 branched chain alkyl group;
[0011] X is a halogen;
[0012] m is 0.1-1.9, n is 0.1-1.9, m+n=2, 0 <q≤0.5;
[0013] Preferably, for R1, R2 and R3, one or more hydrogen atoms on the alkyl group may be independently replaced by a halogen atom;
[0014] More preferably, R3 is a C1-C5 straight-chain alkyl group, a C3-C5 branched-chain alkyl group, a halogen-substituted C1-C5 straight-chain alkyl group, or a halogen-substituted C3-C5 branched-chain alkyl group, such as -CH3 or -CH2Cl;
[0015] Preferably, X is chlorine or bromine;
[0016] Preferably, m is 0.8-1.2, n is 0.8-1.2, and 0.005≤q≤0.2.
[0017] The component B is an internal electron donor compound, specifically α-cyanosuccinate or substituted α-cyanosuccinate, and its structure is shown in formula (II).
[0018]
[0019] In formula (II), R'1 to R'2 are the same or different and are independently H, C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkyl or C7-C 10 Aralkyl;
[0020] R″′3~R″′4 are the same or different, and each independently represents C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkyl or C7-C 10 Aralkyl;
[0021] Preferably, R″′1 and R″′2 can bond to each other to form one or more condensed ring structures;
[0022] Preferably, R'3 and R'4 are the same or different and are independently C1 to C 10 Straight or branched alkyl, C3~C 10 Cycloalkyl, C6~C 20 Aryl, C7~C 20 Alkyl or C7~C 20 Aromatic hydrocarbon group;
[0023] Preferably, the hydrogen atoms on the benzene ring in the aryl group, alkylaryl group or aromatic hydrocarbon group may be optionally replaced by other atoms.
[0024] As a specific embodiment of the present invention, the catalyst component further comprises titanium and chlorine; the titanium and chlorine are derived from titanium tetrachloride.
[0025] As a specific embodiment of the present invention, the synthetic raw materials of component A include elemental sulfur, magnesium halide, alcohol, and ethylene oxide compounds.
[0026] As a specific embodiment of the present invention, the general formula of the magnesium halide is MgX1Y, X1 is a halogen, Y is a halogen, a C1-C5 alkyl, a C1-C5 alkoxy, a C6-C 10 Aryl or C6-C 10 of aryloxy.
[0027] As a specific embodiment of the present invention, the general formula of the alcohol is R1OH, R1 is a C1-C8 alkyl group, a C3-C8 branched alkyl group or a C3-C8 cycloalkyl group; preferably, the hydrogen atoms on the R1 alkyl group can be independently replaced by halogen atoms; and / or
[0028] As a specific embodiment of the present invention, the structure of the ethylene oxide compound is shown in formula (III):
[0029]
[0030] In formula (III), R2 and R3 are the same or different and are independently hydrogen, a C1-C5 straight-chain alkyl group or a C3-C5 branched-chain alkyl group;
[0031] Preferably, in R2 and R3, one or more hydrogen atoms on the alkyl group may be independently replaced by a halogen atom.
[0032] As a specific embodiment of the present invention, the method for preparing the sulfur-containing magnesium compound comprises the following steps:
[0033] S1: mixing elemental sulfur, magnesium halide of the general formula MgX1Y, a compound of the general formula R1OH, an inert liquid medium, and a surfactant and heating to obtain a liquid mixture;
[0034] S2: The liquid mixture obtained in S1 is contacted with an ethylene oxide compound for reaction.
[0035] As a specific embodiment of the present invention, in S1, the inert liquid medium is at least one of kerosene, paraffin oil, vaseline oil, white oil, methyl silicone oil, ethyl silicone oil, methylethyl silicone oil, phenyl silicone oil and methylphenyl silicone oil; preferably, white oil;
[0036] The amount of the inert liquid medium is 0.8-10L, preferably 2-8L, based on 1 mol of magnesium halide with the general formula MgX1Y;
[0037] The surfactant is at least one of polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG), polyvinyl alcohol, polyacrylic acid, polyacrylic acid salt, polyacrylamide, polystyrene sulfonate, naphthalenesulfonic acid formaldehyde condensate, condensed alkyl phenyl ether sulfate, condensed alkylphenol polyoxyethylene ether phosphate, oxyalkyl acrylate copolymer modified polyethyleneimine, 1-dode-4-vinylpyridinium bromide polymer, polyvinyl benzyl trimethylamine salt, polyethylene oxide propylene oxide block copolymer, polyvinyl pyrrolidone vinyl acetate copolymer, alkylphenyl polyoxyethylene ether and polyalkyl methacrylate; preferably, at least one of polyvinyl pyrrolidone, polyvinyl pyrrolidone vinyl acetate copolymer and polyethylene glycol;
[0038] The amount of the surfactant used is 1-20 g based on 1 mol of magnesium halide with the general formula MgX1Y;
[0039] The heating temperature is 80-120°C, and the reaction time is 0.5-5 hours; preferably, the temperature is 80-100°C, and the reaction time is 0.5-3 hours;
[0040] In S2, the contact reaction temperature is 40-120°C, and the reaction time is 15-60 minutes; preferably, the contact reaction temperature is 60-100°C, and the reaction time is 20-50 minutes.
[0041] As a specific embodiment of the present invention, the above-mentioned preparation method may further include solid-liquid separation of the product obtained by the contact reaction, washing the separated solid phase product and drying it. The solid-liquid separation may be any existing method capable of achieving solid-liquid separation, such as suction filtration, filter pressing or centrifugal separation. Preferably, the solid-liquid separation method is filter pressing. The present invention does not particularly limit the conditions for filter pressing, and is subject to achieving the separation of the solid phase and the liquid phase as fully as possible. The washing may be performed by a method known to those skilled in the art to wash the obtained solid phase product, for example, an inert hydrocarbon solvent (for example: pentane, hexane, heptane, petroleum ether and gasoline) may be used to wash the obtained solid phase product. The present invention does not particularly limit the conditions for the drying, for example: the drying temperature may be 20-70°C, and the drying time may be 0.5-10 hours. According to the present invention, the drying may be performed under normal pressure or reduced pressure.
[0042] As a specific embodiment of the present invention, the content of the above components in the spherical carrier of the olefin polymerization catalyst can be selected and varied within a large range. Preferably, based on 1 mol of magnesium halide with the general formula MgX1Y, the amount of elemental sulfur is 0.0001-0.5 mol, the amount of the compound with the general formula R1OH is 4-30 mol, and the amount of the ethylene oxide compound is 1-10 mol. Further preferably, based on 1 mol of magnesium halide with the general formula MgX1Y, the amount of the compound with the general formula R1OH is 6-20 mol, and the amount of the ethylene oxide compound is 2-6 mol.
[0043] As a specific embodiment of the present invention, the elemental sulfur can be any subtype of elemental sulfur, including but not limited to at least one of α-sulfur, β-sulfur, γ-sulfur and polymeric sulfur. The elemental sulfur can be anhydrous elemental sulfur or elemental sulfur containing bound water. The above elemental sulfur can be commercially available.
[0044] As a specific embodiment of the present invention, in the general formula MgX1Y, X1 is preferably chlorine or bromine, and Y is preferably chlorine, bromine, C1-C5 alkoxy or C6-C 10 The C1-C5 alkyl group may be, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl or neopentyl; the C1-C5 alkoxy group may be, for example, methoxy, ethoxy, propoxy, isopropoxy, butoxy or isobutoxy; the C6-C 10 The aryl group may be, for example, phenyl, o-tolyl, m-tolyl, p-tolyl, o-ethylphenyl, m-ethylphenyl, p-ethylphenyl or naphthyl. 10 The aryloxy group may be, for example, a phenoxy group or a naphthoxy group. The magnesium halide of the general formula MgX1Y may be a single magnesium halide or a mixture of multiple magnesium halides. Specific examples of the magnesium halide of the general formula MgX1Y may be, but are not limited to, at least one of magnesium chloride, magnesium bromide, phenoxymagnesium chloride, isopropoxymagnesium chloride and n-butoxymagnesium chloride. From the perspective of the availability of raw materials, magnesium chloride is preferred.
[0045] As a specific embodiment of the present invention, in the general formula R1OH, R1 can be a C1-C8 alkyl group or a C3-C8 cycloalkyl group, wherein the carbon atoms in the C3-C8 cycloalkyl group can all participate in the ring formation, or can also participate in the ring formation partially, and the C3-C8 cycloalkyl group can be, for example, a cyclopentyl group, a cyclopentylmethyl group, a cyclopentylethyl group, a cyclohexyl group or a cyclohexylmethyl group. R1 is preferably a C1-C8 alkyl group; the C1-C8 alkyl group can be, for example, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, a n-pentyl group, an isopentyl group, a tert-pentyl group, a neopentyl group, a hexyl group, an isohexyl group, a heptyl group, an isoheptyl group, an octyl group or an isooctyl group. Specific examples of the compound of the general formula R1OH can be, but are not limited to, at least one of ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, n-hexanol, 2-ethylhexanol and n-octanol.
[0046] As a specific embodiment of the present invention, in the oxirane compound shown in formula (III), R2 and R3 are preferably independently hydrogen, C1-C3 alkyl or C1-C3 haloalkyl. Specific examples of the oxirane compound may be, but are not limited to, at least one of ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epichlorohydrin, epibromohydrin and epibromobutylene.
[0047] As a specific embodiment of the present invention, the carrier is a spherical carrier. The average particle size of the spherical carrier can be controlled within a wide range, for example, 10-100 microns.
[0048] According to a preferred embodiment of the present invention, the average particle diameter (D50) of the spherical carrier can be controlled to be less than or equal to 30 microns, preferably controlled to be less than or equal to 20 microns, and the particle size distribution ((D90-D10) / D50) is less than 1.2; preferably, the particle size distribution is less than or equal to 0.8. In this preferred embodiment, the catalyst prepared from the spherical carrier can obtain an olefin polymer with a higher bulk density. In the present invention, the average particle diameter and particle size distribution of the spherical carrier can be measured using a Master Sizer 2000 laser particle size analyzer (manufactured by Malvern Instruments Ltd).
[0049] As a specific embodiment of the present invention, the spherical carrier may contain water, and the contained water comes from the trace water carried by the synthetic raw materials and the reaction medium. According to the present invention, the trace water in the above-mentioned reactants can also participate in the reaction of forming the spherical carrier.
[0050] As a specific embodiment of the present invention, in the above-mentioned compound of general formula (II), the preferred groups are: R″′1~R″′2 are each independently methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, cyclopentyl, cyclohexyl, benzyl, p-tolylmethyl or phenethyl; R″′3~R″′4 are each independently methyl, ethyl, n-propyl, isopropyl, n-butyl, phenyl, p-tolyl, o-tolyl, m-tolyl or benzyl.
[0051] In the above-mentioned compounds of general formula (II), the particularly preferred groups are: R"'1 to R"'2 are isopropyl; and R"'3 to R"'4 are ethyl.
[0052] The compound represented by the general formula (II) can be: 2,3-diisopropyl-2-cyanosuccinic acid diethyl ester, 3-methyl-2-isopropyl-2-cyanosuccinic acid diethyl ester, 3-ethyl-2-isopropyl-2-cyanosuccinic acid diethyl ester, 3-propyl-2-isopropyl-2-cyanosuccinic acid diethyl ester, 3-butyl-2-isopropyl-2-cyanosuccinic acid diethyl ester, 3-phenyl-2-isopropyl-2-cyanosuccinic acid diethyl ester, etc.
[0053] The compound of formula (IV) (diethyl 2,3-diisopropyl-2-cyanosuccinate) is particularly preferred.
[0054]
[0055] It should be noted that in the present invention, the compound represented by the general formula (II) is selected as the internal electron donor compound because α-cyano succinate or substituted α-cyano succinate has the ability to construct a variety of active centers, and the molecular chain lengths of the polymers catalyzed by the catalyst component are quite different, resulting in a wide molecular weight distribution. However, the types of active centers that can be constructed by the dimethoxypropane compound are relatively small, resulting in a narrow molecular weight distribution. Therefore, the selection of the compound represented by the general formula (II) can effectively control the width of the molecular weight distribution width of the final polymer.
[0056] The mass ratio of titanium element, magnesium element in component A and component B (internal electron donor compound) is 1:(5-15):(2-15), preferably 1:(6-13):(3-12).
[0057] The above raw materials in the present invention can be prepared in-house or commercially available, and the present invention is not particularly limited thereto.
[0058] In a second aspect, the present invention provides a catalyst system for olefin polymerization, the catalyst system comprising:
[0059] (1) the catalyst;
[0060] (2) alkyl aluminum compounds; and
[0061] (3) Optional external electron donor compound.
[0062] The alkyl aluminum compound may be any of various alkyl aluminum compounds commonly used in the field of olefin polymerization that can be used as a co-catalyst for a Ziegler-Natta type catalyst.
[0063] Preferably, the alkylaluminum compound may be, but is not limited to, at least one of trimethylaluminum, triethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum monohydrogenate, diisobutylaluminum monohydrogenate, diethylaluminum monochloride, diisobutylaluminum monochloride, sesquiethylaluminum chloride and ethylaluminum dichloride.
[0064] Preferably, the external electron donor compound may be any external electron donor compound commonly used in the field of olefin polymerization and capable of being used as a co-catalyst for a Ziegler-Natta catalyst.
[0065] Preferably, the external electron donor compound may be, but is not limited to, trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxytriethylmethoxysilane, triethylethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, ethylisopropyldimethoxysilane, propylisopropyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, isopropylisobutyldimethoxysilane, di-tert-butyldimethoxysilane, tert-butylmethyldimethoxysilane, tert-butylethyldimethoxysilane, tert-butylpropyldimethoxysilane, tert-butylisopropyldimethoxysilane, tert-butyl Butyldimethoxysilane, tert-butylisobutyldimethoxysilane, tert-butyl(sec-butyl)dimethoxysilane, tert-butylpentyldimethoxysilane, tert-butylnonyldimethoxysilane, tert-butylhexyldimethoxysilane, tert-butylheptyldimethoxysilane, tert-butyloctyldimethoxysilane, tert-butyldecyldimethoxysilane, tert-butylmethyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylethyldimethoxysilane, cyclohexylpropyldimethoxysilane, cyclohexylisobutyldimethoxysilane, dicyclohexyldimethoxysilane, cyclohexyltert-butyldimethoxysilane, cyclopentylmethyldimethoxysilane , cyclopentylethyldimethoxysilane, cyclopentylpropyldimethoxysilane, cyclopentyltert-butyldimethoxysilane, dicyclopentyldimethoxysilane, cyclopentylcyclohexyldimethoxysilane, bis(2-methylcyclopentyl)dimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, phenyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, isopropyltrimethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, isobutyltrimethoxysilane, tert-butyltrimethoxysilane, sec-butyltrimethoxysilane At least one of methoxysilane, amyl trimethoxysilane, isopentyl trimethoxysilane, cyclopentyl trimethoxysilane, cyclohexyl trimethoxysilane, diphenyl dimethoxysilane, diphenyl diethoxysilane, phenyl trimethoxysilane, phenyl triethoxysilane, n-propyl trimethoxysilane, vinyl trimethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, 2-ethylpiperidinyl-2-tert-butyl dimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyl dimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyl dimethoxysilane. More preferably, the external electron donor compound can be at least one of dicyclopentyl dimethoxysilane, diisopropyl dimethoxysilane, diisobutyl dimethoxysilane, cyclohexyl methyl dimethoxysilane, methyl tert-butyl dimethoxysilane and tetramethoxysilane.
[0066] In addition, in the catalyst system of the present invention, there is no particular limitation on the amounts of the catalyst, the alkyl aluminum compound and the external electron donor compound, and any amounts known in the art may be used.
[0067] A third aspect is the use of the catalyst system of the present invention in olefin polymerization reactions.
[0068] In a fourth aspect, the present invention provides a method for olefin polymerization, which comprises: contacting one or more olefins with the catalyst system under olefin polymerization conditions.
[0069] The olefin is at least one olefin represented by the formula CH2=CHR, wherein R is hydrogen or a C1-C6 straight chain or C3-C6 branched alkyl. Specific examples of the olefin represented by the formula CH2=CHR may include: ethylene, propylene, 1-n-butene, 1-n-pentene, 1-n-hexene, 1-n-octene, 4-methyl-1-pentene. Preferably, the olefin represented by the formula CH2=CHR is ethylene, propylene, 1-n-butene, 1-n-hexene, 4-methyl-1-pentene. More preferably, the olefin represented by the formula CH2=CHR is propylene.
[0070] The olefin polymerization method of the present invention may be the homopolymerization of a single olefin or the copolymerization of multiple olefins.
[0071] According to the olefin polymerization method of the present invention, the olefin polymerization conditions can be conventional conditions in the art. Generally, the olefin polymerization conditions include: temperature of 0-150°C, time of 0.1-8 hours, and pressure of 0.01-10MPa. Preferably, the olefin polymerization conditions include: temperature of 50-100°C, time of 0.5-3 hours, and pressure of 0.5-5MPa. The amount of the olefin polymerization catalyst can be various conventional amounts of olefin catalysts in the prior art.
[0072] It should be noted that the internal electron donor compound (component B) in the catalyst not only participates in the construction of the active center, but also affects the process of magnesium chloride recrystallization and thus affects the structure and morphology of the carrier (component A). Due to the morphology replication effect, the structure and morphology of the catalyst also ultimately affect the structure and morphology of the polymer. The catalyst morphology constructed with the participation of the internal electron donor compound (component B) is more conducive to the fluidity of the polymer, so the falling time of the obtained polymer is shorter.
[0073] Compared with the prior art, the present invention has the following beneficial effects:
[0074] 1. The present invention uses the sulfur-containing magnesium compound (component A) shown in formula (I) as a carrier and the II compound (component B) as an internal electron donor to obtain a catalyst with a novel composition. The catalyst particles have good morphology, a particle size of less than 30 microns, and a narrow particle size distribution. When the catalyst is used for propylene polymerization, polypropylene with a wide molecular weight distribution can be obtained, and the falling time of the polymer produced by the catalyst, especially polypropylene particles, can be improved.
[0075] 2. The catalyst system prepared by the olefin polymerization catalyst of the present invention has small particle size, high activity, wide polymer molecular weight distribution, short falling time, and great industrial application prospects. DETAILED DESCRIPTION
[0076] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.
[0077] In each of the examples and comparative examples of the present invention, the average particle diameter and particle size distribution of the olefin polymerization catalyst carrier were measured using a Masters Sizer 2000 particle size analyzer (manufactured by Malvern Instruments Ltd).
[0078] In each of the examples and comparative examples of the present invention, the surface morphology of the olefin polymerization catalyst carrier was observed by an optical microscope of model Eclipse E200 purchased from Nikon Corporation.
[0079] In each of the examples and comparative examples of the present invention, melt flow rate (MFR) is measured according to ISO 1133, at 230° C. and under a load of 2.16 kg.
[0080] In each of the embodiments and comparative examples of the present invention, the bulk density of the polyolefin powder is measured using the method specified in GB / T 1636-2008.
[0081] In each of the embodiments and comparative examples of the present invention, the polymer powder passes through the funnel of the bulk density tester, and the time for all the materials to pass through is recorded, which is the falling time.
[0082] Preparation Example 1
[0083] This preparation example is used to illustrate the spherical carrier of olefin polymerization catalyst used in the present invention and its preparation method.
[0084] In a 0.6L reactor, add 8.0g (0.08mol) of magnesium chloride, 56mL (0.96mol) of ethanol, 1g (0.03mol) of α-sulfur, and 1g of PVP (polyvinylpyrrolidone) as a surfactant, heat to 90°C with stirring, and add 38mL (0.48mol) of epichlorohydrin after constant temperature reaction for 2 hours. Continue to react at 90°C for half an hour and then filter. Wash the filter product with hexane 5 times and finally dry the product in vacuum to obtain a spherical catalyst carrier Z1 for olefin polymerization.
[0085] The average particle diameter (D50) of the olefin polymerization catalyst spherical carrier Z1 is 15 microns, and the particle size distribution ((D90-D10) / D50) is 0.6. The particle morphology of the olefin polymerization catalyst spherical carrier Z1 is relatively regular, the surface is smooth, and it is basically spherical. The particle size distribution is relatively concentrated, and there are basically no irregular particles.
[0086] According to GC-MS, elemental analysis and NMR characterization, the structural formula of Z1 is:
[0087]
[0088] Preparation Example 2
[0089] This preparation example is used to illustrate the spherical carrier of olefin polymerization catalyst used in the present invention and its preparation method.
[0090] In a 0.6L reactor, add 300mL white oil, 8.0g (0.08mol) magnesium chloride, 28mL (0.48mol) ethanol, 0.3g (0.009mol) β-sulfur, and 1g PVP (polyvinyl pyrrolidone) as a surfactant, heat to 100°C with stirring, and add 12.5mL (0.16mol) epichlorohydrin after isothermal reaction for 1 hour. Continue isothermal reaction at 100°C for 20 minutes and then filter. Wash the filter product with hexane 5 times and finally dry the product in vacuum to obtain a spherical carrier Z2 for olefin polymerization catalyst.
[0091] The average particle diameter (D50) of the olefin polymerization catalyst spherical carrier Z2 is 18 microns, and the particle size distribution ((D90-D10) / D50) is 0.7. The particle morphology of the olefin polymerization catalyst spherical carrier Z2 is relatively regular, the surface is smooth, and it is basically spherical. The particle size distribution is relatively concentrated, and there are basically no irregular particles.
[0092] According to GC-MS, elemental analysis and NMR characterization, the structural formula of Z2 is:
[0093]
[0094] Preparation Example 3
[0095] This preparation example is used to illustrate the spherical carrier of olefin polymerization catalyst used in the present invention and its preparation method.
[0096] In a 0.6L reactor, add 300mL white oil, 8.0g (0.08mol) magnesium chloride, 28mL (0.48mol) ethanol, 0.2g (0.006mol) α-sulfur, and 1g PVP (polyvinyl pyrrolidone) as a surfactant, heat to 100°C with stirring, and add 12.5mL (0.16mol) epichlorohydrin after isothermal reaction for 1 hour. Continue isothermal reaction at 100°C for 20 minutes and then filter. Wash the filter product with hexane 5 times and finally dry the product in vacuum to obtain a spherical carrier Z3 for olefin polymerization catalyst.
[0097] The average particle diameter (D50) of the olefin polymerization catalyst spherical carrier Z3 is 20 microns, and the particle size distribution ((D90-D10) / D50) is 0.8. The particle morphology of the olefin polymerization catalyst spherical carrier Z3 is relatively regular, the surface is smooth, and it is basically spherical. The particle size distribution is relatively concentrated, and there are basically no irregular particles.
[0098] According to GC-MS, elemental analysis and NMR characterization, the structural formula of Z3 is:
[0099]
[0100] Preparation Example 4
[0101] This preparation example is used to illustrate the spherical carrier of olefin polymerization catalyst used in the present invention and its preparation method.
[0102] In a 0.6L reactor, add 8.0g (0.08mol) of magnesium chloride, 59mL (0.48mol) of cyclohexylmethanol, 0.3g (0.009mol) of β-sulfur, and 1g of PVP (polyvinyl pyrrolidone) as a surfactant, heat to 60°C with stirring, and add 12.5mL (0.16mol) of epichlorohydrin after isothermal reaction for 1 hour. Continue isothermal reaction at 60°C for 20 minutes and then filter. Wash the filter product with hexane 5 times and finally dry the product in vacuum to obtain a spherical carrier Z4 for olefin polymerization catalyst.
[0103] The average particle diameter (D50) of the olefin polymerization catalyst spherical carrier Z4 is 25 microns, and the particle size distribution ((D90-D10) / D50) is 0.9. The particle morphology of the olefin polymerization catalyst spherical carrier Z4 is relatively regular, the surface is smooth, and it is basically spherical. The particle size distribution is relatively concentrated, and there are basically no irregular particles.
[0104] According to GC-MS, elemental analysis and NMR characterization, the structural formula of Z4 is:
[0105]
[0106] Preparation Example 5
[0107] This preparation example is used to illustrate the spherical carrier of olefin polymerization catalyst used in the present invention and its preparation method.
[0108] In a 0.6L reactor, add 8.0g (0.08mol) of magnesium chloride, 28mL (0.48mol) of ethanol, 0.3g (0.009mol) of α-sulfur, and 1g of PVP (polyvinyl pyrrolidone) as a surfactant, heat to 70°C with stirring, and add 11.2mL (0.16mol) of propylene oxide after isothermal reaction for 1 hour. Continue isothermal reaction at 70°C for 20 minutes and then filter press. Wash the filter press product with hexane 5 times and finally dry the product in vacuum to obtain a spherical carrier Z5 for olefin polymerization catalyst.
[0109] The average particle diameter (D50) of the olefin polymerization catalyst spherical carrier Z5 is 26 microns, and the particle size distribution ((D90-D10) / D50) is 0.9. The particle morphology of the olefin polymerization catalyst spherical carrier Z5 is relatively regular, the surface is smooth, and it is basically spherical. The particle size distribution is relatively concentrated, and there are basically no irregular particles.
[0110] According to GC-MS, elemental analysis and NMR characterization, the structural formula of Z5 is:
[0111]
[0112] Comparative Preparation Example 1
[0113] This comparative preparation example is used to illustrate a reference olefin polymerization catalyst support and a preparation method thereof.
[0114] In a 0.6L reactor, add 0.08mol magnesium chloride, 0.96mol ethanol, and 1g PVP (polyvinyl pyrrolidone) as a surfactant, heat to 90°C with stirring, and add 38mL (0.48mol) epichlorohydrin after constant temperature reaction for 2 hours. Continue constant temperature reaction at 90°C for half an hour and then filter press. Wash the filter press product with hexane 5 times and finally dry the product in vacuum to obtain the catalyst carrier DZ1 for olefin polymerization.
[0115] The average particle diameter (D50) of the olefin polymerization catalyst carrier DZ1 is 60 micrometers, and the particle size distribution ((D90-D10) / D50) is 1.3. The particle morphology observed by optical microscope shows that there are irregular-shaped particles in the olefin polymerization catalyst carrier DZ1, and the surface is relatively rough.
[0116] Comparative Preparation Example 2
[0117] In a 0.6L reactor, add 8.0g (0.08mol) of magnesium chloride, 59mL (0.48mol) of cyclohexylmethanol, and 1g of PVP (polyvinylpyrrolidone) as a surfactant, heat to 60°C with stirring, and add 12.5mL (0.16mol) of epichlorohydrin after isothermal reaction for 1 hour. Continue isothermal reaction at 60°C for 20 minutes and then filter press. Wash the filter press product with hexane 5 times and finally dry the product in vacuum to obtain a spherical carrier DZ2 for olefin polymerization catalyst.
[0118] The average particle diameter (D50) of the catalyst carrier DZ2 for olefin polymerization is 80 micrometers, and the particle size distribution ((D90-D10) / D50) is 1.5. The particle morphology is observed using an optical microscope, and there are irregular particles in DZ2, and the surface is relatively rough.
[0119] Comparative Preparation Example 3
[0120] In a 0.6L reactor, add 8.0g (0.08mol) of magnesium chloride, 28mL (0.48mol) of ethanol, and 1g of PVP (polyvinyl pyrrolidone) as a surfactant, heat to 70°C with stirring, and add 11.2mL (0.16mol) of propylene oxide after isothermal reaction for 1 hour. Continue isothermal reaction at 70°C for 20 minutes and then filter press. Wash the filter press product with hexane 5 times and finally dry the product in vacuum to obtain a spherical carrier DZ3 for olefin polymerization catalyst.
[0121] The average particle diameter (D50) of the olefin polymerization catalyst carrier DZ3 is 88 micrometers, and the particle size distribution ((D90-D10) / D50) is 1.7. The particle morphology is observed using an optical microscope, and there are irregular particles in DZ3, and the surface is relatively rough.
[0122] Example 1
[0123] This example is used to illustrate the catalyst components and catalyst preparation and propylene polymerization method provided by the present invention, and the specific details are as follows:
[0124] (1) Preparation of olefin polymerization catalyst
[0125] In a 300mL glass reaction bottle, add 100mL of titanium tetrachloride, cool to -20°C, add 40g of the olefin polymerization catalyst carrier Z1 obtained in Preparation Example 1, and stir at -20°C for 30min. Then, slowly heat up to 110°C, add 1.5mL of diethyl 2,3-diisopropyl-2-cyanosuccinate during the heating process, maintain at 110°C for 30min, and filter out the liquid. Then, add titanium tetrachloride and wash twice, and finally wash 5 times with hexane, and obtain olefin polymerization catalyst C1 after drying.
[0126] (3) Propylene polymerization
[0127] A 5L stainless steel autoclave was purged with nitrogen gas, and then 1mmol of triethylaluminum hexane solution (triethylaluminum concentration was 0.5mmol / mL), 0.05mmol of methylcyclohexyldimethoxysilane, 10mL of anhydrous hexane, 10mg of olefin polymerization catalyst C1 obtained in step (1), 1.5L (standard volume) of hydrogen and 2.5L of liquid propylene were introduced into the nitrogen gas flow. The temperature was raised to 70°C, and the reaction was carried out at this temperature for 1 hour, and the temperature was lowered, the pressure was released, and the material was dried to obtain polypropylene powder P1.
[0128] The average particle diameter (D50) of the olefin polymerization catalyst C1 is 14 microns, the particle size distribution is 0.6, the sulfur and magnesium in the component A of the catalyst, the ratio of the amount of sulfur to the amount of magnesium is 0.0021, the activity of the catalyst is 30.3 kgPP / g·cat, the melt flow rate index of the polypropylene powder P1 is 8.1 g / 10min, the molecular weight distribution width is 10.1, and the falling time is 6.3s. In addition, the polypropylene powder has a good particle morphology and basically no irregular particles exist.
[0129] Example 2
[0130] This example is used to illustrate the catalyst component and catalyst preparation and propylene polymerization method provided by the present invention.
[0131] The preparation of olefin polymerization catalyst and propylene polymerization were carried out according to the method of Example 1, except that the olefin polymerization catalyst carrier Z1 was replaced by the olefin polymerization catalyst carrier Z2 obtained in Preparation Example 2, to obtain olefin polymerization catalyst C2 and polypropylene powder P2.
[0132] The average particle diameter (D50) of the olefin polymerization catalyst C2 is 17 microns, the particle size distribution is 0.6, the sulfur and magnesium in the component A of the catalyst, the ratio of the amount of sulfur to the amount of magnesium is 0.0011, the activity of the catalyst is 31.4 kgPP / g·cat, the melt flow rate index of the polypropylene powder P2 is 8.5 g / 10min, the molecular weight distribution width is 10.6, and the falling time is 6.4s. In addition, the polypropylene powder has a good particle morphology and basically no irregular particles.
[0133] Example 3
[0134] This example is used to illustrate the catalyst component and catalyst preparation and propylene polymerization method provided by the present invention.
[0135] The preparation of olefin polymerization catalyst and propylene polymerization were carried out according to the method of Example 1, except that the olefin polymerization catalyst carrier Z1 was replaced by the olefin polymerization catalyst carrier Z3 obtained in Preparation Example 3, to obtain olefin polymerization catalyst C3 and polypropylene powder P3.
[0136] The average particle diameter (D50) of the olefin polymerization catalyst C3 is 19 microns, the particle size distribution is 0.7, the ratio of the amount of sulfur to the amount of magnesium in component A of the catalyst is 0.00061, the activity of the catalyst is 31.1 kgPP / g·cat, the melt flow rate index of the polypropylene powder P3 is 8.0 g / 10 min, the molecular weight distribution width is 10.5, and the falling time is 6.4 s. In addition, the polypropylene powder has a good particle morphology and basically no irregular particles exist.
[0137] Embodiment 4-6
[0138] This example is used to illustrate the catalyst component and catalyst preparation and propylene polymerization method provided by the present invention.
[0139] The preparation of olefin polymerization catalyst and propylene polymerization were carried out according to the method of Examples 1-3, except that 6.5L instead of 1.5L (standard volume) of hydrogen was added to obtain polypropylene powders P4, P5, and P6, respectively. The activities of olefin polymerization catalysts C1, C2, and C3 were 31.4kgPP / g·cat, 31.2kgPP / g·cat, and 31.8kgPP / g·cat, respectively, the melt flow rate index was 25.1g / 10min, 26.8g / 10min, and 25.3g / 10min, respectively, the molecular weight distribution width was 10.5, 10.8, and 10.3, respectively, and the falling time was 6.6s, 6.5s, and 6.5s, respectively. In addition, the particle morphology of polypropylene powders P4, P5, and P6 was good, and there was basically no irregular material.
[0140] Example 7
[0141] The preparation of olefin polymerization catalyst and propylene polymerization reaction were carried out according to the method of Example 1, except that the olefin polymerization catalyst spherical carrier Z1 was replaced by the olefin polymerization catalyst spherical carrier Z4 obtained in Preparation Example 4, to obtain olefin polymerization catalyst C7 and polypropylene powder P7.
[0142] The average particle diameter (D50) of the olefin polymerization catalyst C7 is 23 microns, the particle size distribution is 0.8, the sulfur and magnesium in the component A of the catalyst, the ratio of the amount of sulfur to the amount of magnesium is 0.0012, the activity is 30.1 kgPP / g·cat, the melt flow rate index of the polypropylene powder P5 is 8.3 g / 10min, the molecular weight distribution width is 10.3, and the falling time is 6.6s. In addition, the particle morphology of the polypropylene powder is good, and there is basically no irregular material.
[0143] Example 8
[0144] The preparation of olefin polymerization catalyst and propylene polymerization reaction were carried out according to the method of Example 1, except that the olefin polymerization catalyst spherical carrier Z1 was replaced by the olefin polymerization catalyst spherical carrier Z5 obtained in Preparation Example 5, to obtain olefin polymerization catalyst C8 and polypropylene powder P8.
[0145] The average particle diameter (D50) of the olefin polymerization catalyst C8 is 25 microns, the particle size distribution is 0.8, the sulfur and magnesium in the component A of the catalyst, the ratio of the amount of sulfur to the amount of magnesium is 0.0013, the activity is 31.0 kgPP / g·cat, the melt flow rate index of the polypropylene powder P7 is 8.2 g / 10min, the molecular weight distribution width is 10.4, and the falling time is 6.6 s. In addition, the particle morphology of the polypropylene powder is good, and there is basically no irregular material.
[0146] Example 9
[0147] The preparation of olefin polymerization catalyst and propylene polymerization reaction were carried out according to the method of Example 1, except that 2,3-diisopropyl-2-cyanosuccinic acid diethyl ester was replaced by an equal amount of 3-ethyl-2-isopropyl-2-cyanosuccinic acid diethyl ester to obtain olefin polymerization catalyst C9 and polypropylene powder P9.
[0148] The activity of olefin polymerization catalyst C9 is 21.5 kgPP / g·cat, the melt flow rate index of polypropylene powder P9 is 10 g / 10 min, the falling time is 6.5 s, the molecular weight distribution width is 10.1, and the particle morphology of the polypropylene powder is good, and there is basically no irregular material.
[0149] Comparative Example 1
[0150] This comparative example serves to illustrate a reference preparation of catalyst components and catalysts.
[0151] The preparation of olefin polymerization catalyst and propylene polymerization were carried out according to the method of Example 1, except that diisobutyl phthalate was used instead of diethyl 2,3-diisopropyl-2-cyanosuccinate, to obtain olefin polymerization catalyst DC1 and polypropylene powder DP3.
[0152] The average particle diameter (D50) of the olefin polymerization catalyst DC1 is 14 microns, the particle size distribution is 0.6, the activity is 38.9 kgPP / g·cat, the melt flow rate index of the polypropylene powder DP3 is 12.0 g / 10 min, the molecular weight distribution width is 4.8, and the falling time is 7.0 s.
[0153] It can be seen from the above results that the catalyst prepared by the olefin polymerization catalyst of the present invention has small particle size, high activity, wide polymer molecular weight distribution, short falling time, and has great industrial application prospects.
[0154] Any numerical value mentioned in the present invention, if there is only an interval of two units between any minimum value and any maximum value, includes all values from the minimum value to the maximum value each time increasing by one unit. For example, if the amount of a component, or the value of a process variable such as temperature, pressure, time, etc. is declared to be 50-90, in this specification it means that 51-89, 52-88... and 69-71 and 70-71 are specifically listed. For non-integer values, 0.1, 0.01, 0.001 or 0.0001 can be appropriately considered as a unit. These are just some specially specified examples. In this application, in a similar manner, all possible combinations of numerical values between the listed minimum and maximum values are considered to have been disclosed.
[0155] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A catalyst for olefin polymerization, characterized in that Comprising component A and component B; The catalyst also includes titanium and chlorine; the titanium and chlorine are from titanium tetrachloride; The component A is a carrier, and the carrier is a sulfur-containing magnesium compound, and its structure is shown in formula (I). In formula (I), R11 is a C1-C8 straight-chain alkyl group, a C3-C8 branched-chain alkyl group, or a C3-C8 cycloalkyl group; R2 and R3 are the same or different, and are each independently hydrogen, a C1-C5 straight chain alkyl group, or a C3-C5 branched chain alkyl group; X is a halogen; m is 0.1-1.9, n is 0.1-1.9, m+n=2, 0 <q≤0.5; The component B is used as an internal electron donor compound, and the internal electron donor compound is α-cyanosuccinate or substituted α-cyanosuccinate, and its structure is shown in formula (II). In formula (II), R'1 and R'2 are the same or different and are independently H, C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkyl or C7-C 10 Aralkyl; R'3 and R'4 are the same or different and are independently C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkyl or C7-C 10 Aralkyl; Optionally, hydrogen atoms on the aromatic rings of the aryl, alkaryl or aralkyl groups are replaced by other atoms.
2. The catalyst for olefin polymerization according to claim 1, characterized in that In formula (I), for R1, R2 and R3, one or more hydrogen atoms on the alkyl group are independently replaced by halogen atoms; X is chlorine or bromine; m is 0.8-1.2, n is 0.8-1.2, 0.005≤q≤0.2; In formula (II), R"'1 and R"'2 are bonded to each other to form one or more condensed ring structures; R'3 and R'4 are the same or different and are independently C1 to C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3~C 10 Cycloalkyl, C6~C 10 Aryl, C7~C 10 Alkyl or C7~C 10 Aralkyl.
3. The catalyst for olefin polymerization according to claim 1 or 2, characterized in that The synthetic raw materials of component A include elemental sulfur, magnesium halide, alcohol, and ethylene oxide compounds; The general formula of the magnesium halide is MgX1Y, X1 is a halogen, Y is a halogen, a C1-C5 alkyl, a C1-C5 alkoxy, a C6-C 10 Aryl or C6-C 10 Aryloxy; The alcohol has a general formula of R1OH, where R1 is a C1-C8 straight-chain alkyl group, a C3-C8 branched-chain alkyl group, or a C3-C8 cycloalkyl group; The structure of the ethylene oxide compound is shown in formula (III): In formula (III), R2 and R3 are the same or different and are each independently hydrogen, a C1-C5 straight-chain alkyl group or a C3-C5 branched-chain alkyl group.
4. The catalyst for olefin polymerization according to claim 3, characterized in that In the formula R1OH, the hydrogens on the R1 alkyl group are each independently replaced by a halogen atom; In formula (III), for R2 and R3, one or more hydrogen atoms on the alkyl group are each independently replaced by a halogen atom.
5. The catalyst for olefin polymerization according to claim 3, characterized in that The preparation method of the sulfur-containing magnesium compound comprises the following steps: S1: mixing elemental sulfur, magnesium halide of the general formula MgX1Y, a compound of the general formula R1OH, an inert liquid medium, and a surfactant and heating to obtain a liquid mixture; S2: The liquid mixture obtained in S1 is contacted with an ethylene oxide compound for reaction.
6. The catalyst for olefin polymerization according to claim 5, characterized in that In S1, the inert liquid medium is at least one of kerosene, paraffin oil, vaseline oil, white oil, methyl silicone oil, ethyl silicone oil, methylethyl silicone oil, phenyl silicone oil and methylphenyl silicone oil; and / or The amount of the inert liquid medium is 0.8-10 L based on 1 mol of magnesium halide with the general formula MgX1Y; and / or The surfactant is at least one of polyvinyl pyrrolidone, polyethylene glycol, polyvinyl alcohol, polyacrylic acid, polyacrylic acid salt, polyacrylamide, polystyrene sulfonate, naphthalenesulfonic acid formaldehyde condensate, condensed alkyl phenyl ether sulfate, condensed alkylphenol polyoxyethylene ether phosphate, oxyalkyl acrylate copolymer modified polyethyleneimine, polymer of 1-dode-4-vinylpyridinium bromide, polyvinyl benzyl trimethylamine salt, polyethylene oxide propylene oxide block copolymer, polyvinyl pyrrolidone vinyl acetate copolymer, alkylphenyl polyoxyethylene ether and polyalkyl methacrylate; and / or The amount of the surfactant used is 1-20 g based on 1 mol of magnesium halide with the general formula MgX1Y; and / or The heating temperature is 80-120° C. and the reaction time is 0.5-5 hours; and / or In S2, the temperature of the contact reaction is 40-120° C., and the reaction time is 15-60 minutes.
7. The catalyst for olefin polymerization according to claim 6, characterized in that The inert liquid medium is white oil; The amount of the inert liquid medium is 2-8 L based on 1 mol of magnesium halide with the general formula MgX1Y; The surfactant is at least one of polyvinyl pyrrolidone, polyvinyl pyrrolidone vinyl acetate copolymer and polyethylene glycol.
8. The catalyst for olefin polymerization according to claim 1, characterized in that The mass ratio of titanium element, magnesium element in component A and component B is 1:(5-15):(2-15).
9. The catalyst for olefin polymerization according to claim 8, characterized in that The mass ratio of titanium element, magnesium element in component A and component B is 1:(6-13):(3-12).
10. A catalyst system for olefin polymerization, characterized in that: The catalyst system contains: (1) The catalyst according to any one of claims 1 to 9; (2) alkyl aluminum compounds; and (3) Optional external electron donor compound.
11. Use of the catalyst system according to claim 10 in olefin polymerization.
12. A method for olefin polymerization, the method comprising: One or more olefins are contacted with the catalyst system of claim 11 under olefin polymerization conditions.