Preparation method of a size-controlled ruthenium-carbon catalyst and its application in the preparation of tetramethylpiperidinol
By regulating the preparation process of the ruthenium carbon catalyst, a size-controllable ruthenium carbon catalyst was prepared, which solved the problems of many by-products and poor selectivity in the traditional synthesis of tetramethylpiperidinol, and realized the continuous production of tetramethylpiperidinol. production and efficient catalytic effect.
Patent Information
- Application Number
- CN202211546325.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-05
AI Technical Summary
In the existing synthesis method of tetramethylpiperidinol, the traditional intermittent hydrogenation reduction method results in many by-products and poor product selectivity, resulting in low product yield and prolonged production cycle, and the size of the active metal cannot be controlled to affect the reaction results.
By regulating the pH value and annealing temperature of the impregnation solution during the preparation process of the ruthenium carbon catalyst, a size-controllable ruthenium carbon catalyst is prepared, which is used to improve catalyst activity and reaction efficiency in continuous synthesis. The specific steps include mixing ruthenium trichloride with concentrated hydrochloric acid and ethanol, adding a dispersant and adjusting the pH to form an impregnating liquid, and then treating it in a sugar coating machine, then roasting and reduction annealing to prepare a nanoscale active metal ruthenium catalyst.
The continuous production of tetramethylpiperbutanol is realized, the stability of the catalyst and the conversion rate of raw materials are improved, the selectivity of the product is improved, the subsequent separation process is simplified, and the production cost is reduced.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tetramethyl piperidine alcohol preparation, and particularly relates to a preparation method of a size-controllable ruthenium-carbon catalyst and application of the catalyst in the preparation of tetramethyl piperidine alcohol. Background Art
[0002] At present, palladium, nickel, and ruthenium-based catalysts are mostly used to synthesize tetramethylpiperidinol, but all catalysts do not provide a method for regulating the size of active metals to affect the reaction results. In addition, the current synthesis method of tetramethylpiperidinol mainly adopts the traditional production mode, which is prepared by intermittent hydrogenation reduction. The tetramethylpiperidinol prepared by the intermittent reduction method has more by-products and poor product selectivity, resulting in a low product yield and subsequent separation difficulties. In addition, during the production process, each unit needs to be tested after production. Once a product is found to be unqualified in a certain link, all products in the same batch will be considered unqualified and withdrawn, which will lead to an extension of the production cycle and increase costs. Therefore, a new production method is urgently needed to solve the above problems. Summary of the invention
[0003] In view of the defects of the prior art, the present invention provides a method for preparing a size-controllable ruthenium-carbon catalyst and application thereof in the preparation of tetramethylpiperidinol. By regulating the influencing factors in the catalyst preparation process, the size of the active metal ruthenium can be controlled, thereby improving the activity of the catalyst, so that the prepared catalyst can be used for the continuous synthesis of tetramethylpiperidinol.
[0004] A method for preparing a size-controllable ruthenium-carbon catalyst comprises the following steps:
[0005] (1) Preparation of catalyst precursor: dissolving ruthenium trichloride in a mixture of concentrated hydrochloric acid and ethanol, adding a dispersant, stirring, and adjusting the pH to 0.1-7.0 to obtain an impregnation solution; washing the activated carbon with water to remove the powder, drying, and adding it to a sugar coater, then dripping the impregnation solution into the sugar coater, rotating the sugar coater for 12-18 hours, taking it out, drying, and calcining to obtain a ruthenium carbon catalyst precursor;
[0006] (2) Reduction treatment: The ruthenium carbon catalyst precursor is subjected to reduction annealing activation treatment in a mixed atmosphere of argon and hydrogen, the reduction annealing temperature is 150-700°C, the reduction annealing time is 2-6h, and then cooled to obtain a ruthenium carbon catalyst.
[0007] Preferably, the pH in step (1) is adjusted to 2.5-5.5, and the reduction annealing temperature in step (2) is 250-650°C.
[0008] More preferably, the pH in step (1) is adjusted to 4.5-5.5, and the reduction annealing temperature in step (2) is 450-550°C.
[0009] Preferably, the volume ratio of the concentrated hydrochloric acid to ethanol is 1:(1-16), the addition ratio of the mixed solution of ruthenium trichloride, activated carbon, concentrated hydrochloric acid and ethanol is (1-10) g:100 g:(100-300) mL, and the mass ratio of ruthenium trichloride to dispersant is 1:(1-10).
[0010] Preferably, the dispersant is oxalic acid, oxalic acid tetraacetic acid, oxalic acid tetraacetic acid disodium, sodium citrate or polyvinyl pyrrolidone.
[0011] Preferably, when adjusting the pH in step (1), anhydrous sodium carbonate, sodium hydroxide, potassium hydroxide, or sodium bicarbonate is added for adjustment.
[0012] Preferably, the speed of the sugar coating machine is 5.0-30.0 r / min; the average particle size of the activated carbon carrier is 0.3 mm-1.8 mm, and the specific surface area is 750 m 2 / g-1240m 2 g. Preferably, the drying conditions are: drying temperature is 50-180°C, and drying time is 12-36h;
[0013] The calcination conditions are: in a muffle furnace, heating from room temperature to 200-500° C. at a heating rate of 2-10° C. / min, and then calcining for 2-5 hours;
[0014] The flow rate of argon and hydrogen in step (2) is 100-500 mL / min, and the flow ratio of argon and hydrogen is 1:(3-12).
[0015] A method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalytic hydrogenation of 2,2,6,6-tetramethyl-4-piperidinone: loading a ruthenium carbon catalyst in a fixed bed reactor, dissolving 2,2,6,6-tetramethyl-4-piperidinone in a solvent to obtain a raw material liquid, continuously introducing the raw material liquid and hydrogen, and performing a hydrogenation reaction at 50-120° C. and 0.3-3 MPa, wherein the mass space velocity of 2,2,6,6-tetramethyl-4-piperidinone is 0.1-5 h -1 , the molar ratio of hydrogen to 2,2,6,6-tetramethyl-4-piperidone is (1-100): 1; the ruthenium-carbon catalyst is prepared by the above preparation method.
[0016] Preferably, the solvent is methanol, ethanol, tetrahydrofuran or isopropanol.
[0017] Preferably, the mass ratio of the 2,2,6,6-tetramethyl-4-piperidone to the solvent is 1:(2-20).
[0018] Advantages of the present invention:
[0019] The Ru / C catalyst prepared by the present invention can control the size of active metal ruthenium to reach the nanometer scale by regulating the pH value of the impregnation solution and the annealing reduction temperature during the catalyst preparation process. The catalyst has a clear structure. The prepared catalyst can also be used for catalyzing the hydrogenation of 2,2,6,6-tetramethyl-4-piperidone to prepare 2,2,6,6-tetramethyl-4-piperidinol. The catalyst has good stability, high raw material conversion rate and good product selectivity, and realizes the continuous production of 2,2,6,6-tetramethyl-4-piperidinol. DETAILED DESCRIPTION
[0020] Example 1
[0021] A method for preparing a size-controllable ruthenium-carbon catalyst comprises the following steps:
[0022] (1) Preparation of catalyst precursor: Take 20g of catalyst with an average particle size of 1.2mm and a specific surface area of 935m 2 / g activated carbon carrier, wash with water to remove powder, dry at 120℃ for 12h, and set aside; take 0.58g ruthenium trichloride and add it to a mixture of 10mL concentrated hydrochloric acid and 50mL ethanol, then add 1.16g sodium citrate, stir, and obtain an impregnation solution, and the pH of the system is measured to be 0.1; add the activated carbon carrier to a sugar coating machine, and then drop the impregnation solution on the activated carbon in the rotating sugar coating machine, the sugar coating machine rotates at a speed of 20r / min for 12h, take it out, dry it at 120℃ for 12h, and then place it in a muffle furnace, heat it from room temperature to 250℃ at a heating rate of 2℃ / min, and calcine it for 2h to obtain a ruthenium carbon catalyst precursor;
[0023] (2) Reduction treatment: The ruthenium carbon catalyst precursor is subjected to reduction annealing activation treatment in a mixed atmosphere of argon and hydrogen. The flow rate of the H2 / Ar mixed gas is 200 mL / min, the flow ratio of argon and hydrogen is 1:3, the reduction annealing temperature is 160°C, the reduction annealing time is 2 h, and the catalyst is cooled to obtain a ruthenium carbon catalyst.
[0024] Example 2
[0025] A method for preparing a size-controllable ruthenium-carbon catalyst comprises the following steps:
[0026] (1) Preparation of catalyst precursor: Take 20g of catalyst with an average particle size of 1.2mm and a specific surface area of 935m 2 / g activated carbon carrier, wash with water to remove powder, dry at 120℃ for 12h, and set aside; take 0.58g ruthenium trichloride and add it to a mixture of 10mL concentrated hydrochloric acid and 10mL ethanol, then add 1.16g sodium citrate, stir, and adjust the pH of the system to 1.0 by adding anhydrous sodium carbonate to obtain an impregnation solution; add the activated carbon carrier to a sugar coating machine, and then drop the impregnation solution on the activated carbon carrier in the rotating sugar coating machine, the sugar coating machine rotates at a speed of 20r / min for 12h, take it out, dry it at 120℃ for 12h, and then place it in a muffle furnace, heat it from room temperature to 250℃ at a heating rate of 2℃ / min, and calcine it for 2h to obtain a ruthenium carbon catalyst precursor;
[0027] (2) Reduction treatment: The ruthenium carbon catalyst precursor is subjected to reduction annealing activation treatment in a mixed atmosphere of argon and hydrogen. The flow rate of the H2 / Ar mixed gas is 200 mL / min, the flow ratio of argon and hydrogen is 1:3, the reduction annealing temperature is 150°C, the reduction annealing time is 2 h, and the catalyst is cooled to obtain a ruthenium carbon catalyst.
[0028] Example 3
[0029] In step (1), the pH is adjusted to 2.0, and the rest is the same as in Example 2.
[0030] Example 4
[0031] In step (1), the pH is adjusted to 3.0, and the rest is the same as in Example 2.
[0032] Example 5
[0033] In step (1), the pH is adjusted to 4.0, and the rest is the same as in Example 2.
[0034] Example 6
[0035] In step (1), the pH is adjusted to 5.0, and the rest is the same as in Example 2.
[0036] Example 7
[0037] A method for preparing a size-controllable ruthenium-carbon catalyst comprises the following steps:
[0038] (1) Preparation of catalyst precursor: Take 20g of catalyst with an average particle size of 1.2mm and a specific surface area of 935m 2 / g activated carbon carrier, wash with water to remove powder, dry at 120℃ for 12h, and set aside; take 0.58g ruthenium trichloride and add it to a mixture of 10mL concentrated hydrochloric acid and 10mL ethanol, then add 1.16g sodium citrate, stir, and adjust the pH of the system to 5.0 by adding anhydrous sodium carbonate to obtain an impregnation solution; add the activated carbon carrier to a sugar coating machine, and then drop the impregnation solution on the activated carbon carrier in the rotating sugar coating machine, the sugar coating machine rotates at a speed of 20r / min for 12h, take it out, dry it at 120℃ for 12h, and then place it in a muffle furnace, heat it from room temperature to 250℃ at a heating rate of 2℃ / min, and calcine it for 2h to obtain a ruthenium carbon catalyst precursor;
[0039] (2) Reduction treatment: The ruthenium carbon catalyst precursor is subjected to reduction annealing activation treatment in a mixed atmosphere of argon and hydrogen. The flow rate of the H2 / Ar mixed gas is 200 mL / min, the flow ratio of argon and hydrogen is 1:3, the reduction annealing temperature is 250°C, the reduction annealing time is 2 h, and the catalyst is cooled to obtain a ruthenium carbon catalyst.
[0040] Example 8
[0041] The reduction annealing temperature in step (2) is 350° C., and the rest is the same as in Example 7.
[0042] Example 9
[0043] The reduction annealing temperature in step (2) is 450° C., and the rest is the same as in Example 7.
[0044] Example 10
[0045] The reduction annealing temperature in step (2) is 550° C., and the rest is the same as in Example 7.
[0046] Embodiment 11
[0047] The reduction annealing temperature in step (2) is 650° C., and the rest is the same as in Example 7.
[0048] Example 12
[0049] In step (1), the pH is adjusted to 4.5, and in step (2), the reduction annealing temperature is 450° C., and the rest is the same as in Example 7.
[0050] Embodiment 13
[0051] In step (1), the pH is adjusted to 4.5, and in step (2), the reduction annealing temperature is 550° C., and the rest is the same as in Example 7.
[0052] Embodiment 14
[0053] In step (1), the pH is adjusted to 5.5, and in step (2), the reduction annealing temperature is 450° C., and the rest is the same as in Example 7.
[0054] Embodiment 15
[0055] In step (1), the pH is adjusted to 5.5, and in step (2), the reduction annealing temperature is 550° C., and the rest is the same as in Example 7.
[0056] Example 16
[0057] A method for preparing a size-controllable ruthenium-carbon catalyst comprises the following steps:
[0058] (1) Catalyst precursor preparation: Take 20g of catalyst with an average particle size of 1.8mm and a specific surface area of 750m 2 / g of activated carbon, wash with water to remove powder, dry at 50°C for 36h, and set aside; take 0.2g of ruthenium trichloride and add it to a mixture of 3mL of concentrated hydrochloric acid and 48mL of ethanol, then add 0.2g of oxalic acid tetraacetic acid, stir, and adjust the pH of the system to 7.0 by adding sodium hydroxide to obtain an impregnation solution; add the activated carbon to a sugar coating machine, and then drop the impregnation solution on the activated carbon in the rotating sugar coating machine, the sugar coating machine rotates at a speed of 5r / min for 18h, take it out, dry it at 50°C for 36h, place it in a muffle furnace, heat it from room temperature to 200°C at a heating rate of 10°C / min, and calcine it for 5h to obtain a ruthenium carbon catalyst precursor;
[0059] (2) Reduction treatment: The ruthenium carbon catalyst precursor is subjected to reduction annealing activation treatment in a mixed atmosphere of argon and hydrogen. The flow rate of the H2 / Ar mixed gas is 100 mL / min, the flow ratio of argon and hydrogen is 1:12, the reduction annealing temperature is 700°C, the reduction annealing time is 4 h, and then cooled to obtain a ruthenium carbon catalyst.
[0060] Embodiment 17
[0061] A method for preparing a size-controllable ruthenium-carbon catalyst comprises the following steps:
[0062] (1) Preparation of catalyst precursor: Take 20g of catalyst with an average particle size of 0.3mm and a specific surface area of 1240m 2 / g of activated carbon, wash with water to remove powder, dry at 180℃ for 12h, and set aside; take 2g of ruthenium trichloride and add it to a mixture of 10mL of concentrated hydrochloric acid and 50mL of ethanol, then add 20g of polyvinyl pyrrolidone, stir, and adjust the pH of the system to 7.0 by adding potassium hydroxide to obtain an impregnation solution; add the activated carbon to a sugar coating machine, and then drop the impregnation solution on the activated carbon in the rotating sugar coating machine, the sugar coating machine rotates at a speed of 30r / min for 12h, take it out, dry it at 180℃ for 12h, and then place it in a muffle furnace, heat it from room temperature to 500℃ at a heating rate of 2℃ / min, and calcine it for 2h to obtain a ruthenium carbon catalyst precursor;
[0063] (2) Reduction treatment: The ruthenium carbon catalyst precursor is subjected to reduction annealing activation treatment in a mixed atmosphere of argon and hydrogen. The flow rate of the H2 / Ar mixed gas is 500 mL / min, the flow ratio of argon and hydrogen is 1:12, the reduction annealing temperature is 700°C, the reduction annealing time is 4 h, and the catalyst is cooled to obtain a ruthenium carbon catalyst.
[0064] Performance Testing
[0065] A method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalytic hydrogenation of 2,2,6,6-tetramethyl-4-piperidinone: loading a ruthenium carbon catalyst in a fixed bed reactor, dissolving 2,2,6,6-tetramethyl-4-piperidinone in a solvent to obtain a raw material liquid, continuously introducing the raw material liquid and hydrogen, and performing a hydrogenation reaction at 50-120° C. and 0.3-3 MPa, wherein the mass space velocity of 2,2,6,6-tetramethyl-4-piperidinone is 0.1-5 h -1 , the molar ratio of hydrogen to 2,2,6,6-tetramethyl-4-piperidone is (1-100):1; the solvent is methanol, ethanol, tetrahydrofuran or isopropanol; the mass ratio of 2,2,6,6-tetramethyl-4-piperidone to the solvent is 1:(2-20); the reaction product is analyzed by Shimadzu GC-2014 gas chromatography, capillary column, column box temperature 80°C, chromatographic column temperature 160°C, split ratio 30, and area normalization method to quantify the content of each component; the size of active metal ruthenium in each catalyst, 2,2,6,6-tetramethyl-4-piperidone conversion rate, 2,2,6,6-tetramethyl-4-piperidinol selectivity and catalyst life are shown in Table 1.
[0066] Table 1 Summary of conditions and reaction results in hydrogenation reactions of various examples
[0067] .
Claims
1. A method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalytic hydrogenation of 2,2,6,6-tetramethyl-4-piperidone, characterized in that: The ruthenium carbon catalyst is loaded in a fixed bed reactor, 2,2,6,6-tetramethyl-4-piperidone is dissolved in a solvent to obtain a raw material liquid, the raw material liquid and hydrogen are continuously introduced, and a hydrogenation reaction is carried out at 50-120°C and 0.3-3MPa, wherein the mass space velocity of 2,2,6,6-tetramethyl-4-piperidone is 0.1-5 h -1 , the molar ratio of hydrogen to 2,2,6,6-tetramethyl-4-piperidone is (1-100): 1; wherein the ruthenium-carbon catalyst is prepared by the following method: (1) Preparation of catalyst precursor: dissolving ruthenium trichloride in a mixture of concentrated hydrochloric acid and ethanol, adding a dispersant, stirring, and adjusting the pH to 0.1-7 to obtain an impregnation solution; washing the activated carbon with water to remove the powder, drying, and adding it to a sugar coater, then dripping the impregnation solution into the sugar coater, rotating the sugar coater for 12-18 hours, taking it out, drying, and calcining to obtain a ruthenium carbon catalyst precursor; (2) Reduction treatment: subjecting the ruthenium-carbon catalyst precursor to reduction annealing and activation treatment in a mixed atmosphere of argon and hydrogen, the reduction annealing temperature being 150-700° C., the reduction annealing time being 2-6 h, and cooling to obtain a ruthenium-carbon catalyst; The speed of the sugar coating machine is 5.0-30.0 r / min; the average particle size of the activated carbon carrier is 0.3 mm-1.8 mm, and the specific surface area is 750 m 2 / g-1240m 2 g; The drying conditions are: the drying temperature is 50-180°C, and the drying time is 12-36h; the roasting conditions are: in a muffle furnace, the temperature is increased from room temperature to 200-500°C at a heating rate of 2-10°C / min, and then roasted for 2-5h; The flow rate of argon and hydrogen in step (2) is 50-600 mL / min, and the flow ratio of argon and hydrogen is 1:(3-12).
2. The method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalyzing the hydrogenation of 2,2,6,6-tetramethyl-4-piperidone according to claim 1, characterized in that: The pH is adjusted to 2.5-5.5 and the reduction annealing temperature is 250-650°C.
3. The method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalytic hydrogenation of 2,2,6,6-tetramethyl-4-piperidone according to claim 1 or 2, characterized in that: The volume ratio of the concentrated hydrochloric acid to ethanol is 1:(1-16), the addition ratio of the mixed solution of ruthenium trichloride, activated carbon, concentrated hydrochloric acid and ethanol is (1-10) g:100 g:(100-300) mL, and the mass ratio of ruthenium trichloride to dispersant is 1:(1-10).
4. The method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalyzing the hydrogenation of 2,2,6,6-tetramethyl-4-piperidone according to claim 3, characterized in that: The dispersant is oxalic acid, oxalic acid tetraacetic acid, oxalic acid tetraacetic acid disodium, sodium citrate or polyvinyl pyrrolidone.
5. The method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalyzing the hydrogenation of 2,2,6,6-tetramethyl-4-piperidone according to claim 4, characterized in that: When adjusting the pH in step (1), anhydrous sodium carbonate, sodium hydroxide, potassium hydroxide, or sodium bicarbonate is added for adjustment.
6. The method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalytic hydrogenation of 2,2,6,6-tetramethyl-4-piperidone according to claim 1, 2, 4 or 5, characterized in that: The solvent is methanol, ethanol, tetrahydrofuran or isopropanol.
7. The method for preparing 2,2,6,6-tetramethyl-4-piperidinol by catalyzing the hydrogenation of 2,2,6,6-tetramethyl-4-piperidone according to claim 6, characterized in that: The mass ratio of the 2,2,6,6-tetramethyl-4-piperidone to the solvent is 1:(2-20).
Citation Information
Patent Citations
Nano ruthenium carbon-supported metal hydrogenating catalyst and method for producing the same
CN101502798A