A compound containing a phosphate group, a preparation method thereof and its application

By using phosphate-containing compounds as interface modification materials in perovskite optoelectronic devices, the problems of nonradiative recombination and surface defects at the interface were solved, the carrier transport and stability of the devices were improved, and high-efficiency optoelectronic performance was achieved.

CN116041392BActive Publication Date: 2024-11-12CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310060701.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-12
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

In existing perovskite optoelectronic devices, nonradiative recombination at the interface and surface defects affect device performance and stability, and commonly used hole transport materials such as PEDOT:PSS corrode the anode, leading to device degradation.

Method used

Compounds containing phosphate groups are used as interface modification materials. By interacting with inorganic metal oxides, the energy level arrangement of the electron or hole transport layer is adjusted, and the phosphate group is used to passivate the surface defects of the perovskite film and reduce non-radiative recombination.

Benefits of technology

This improves the carrier transport performance and overall performance of perovskite optoelectronic devices, enhances device stability and efficiency, and maintains the structure and luminescence properties of the perovskite thin film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004061185040000021
    Figure BDA0004061185040000021
  • Figure BDA0004061185040000031
    Figure BDA0004061185040000031
  • Figure BDA0004061185040000037
    Figure BDA0004061185040000037
Patent Text Reader

Abstract

The present invention provides a compound containing a phosphate group as shown in formula (I), and the present application also provides a preparation method and application of the compound containing a phosphate group. The compound containing a phosphate group provided in the present application utilizes the interaction between the phosphate group and the carrier transport layer to form a self-assembled layer, effectively improves wettability, and adjusts the structure of the perovskite film; and the phosphorus oxygen group can passivate the unsaturated coordinated lead defects in the perovskite lattice, reduce non-radiative energy loss, and improve the fluorescence quantum yield and carrier transport performance of the perovskite film; further, different substituents are introduced into the compound containing a phosphate group, which can further adjust the defect passivation effect and make the interface energy level more matched. Therefore, the light-emitting device obtained by using the compound containing a phosphate group as the interface modification layer can achieve high device external quantum efficiency and basically does not affect the structure and luminescence characteristics of the perovskite itself.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of perovskite photoelectric materials, and in particular to a compound containing a phosphate group, a preparation method thereof and an application thereof. Background Art

[0002] Metal halide perovskite materials are an emerging class of semiconductor materials with unlimited potential. They have the characteristics of low cost, solution processing, adjustable bandgap, high light absorption coefficient, high photoluminescence quantum yield, high carrier mobility and long diffusion length, and the ability to achieve bipolar transmission. At present, they have shown potential application value in the fields of perovskite solar cells, light-emitting diodes, lasers and photodetectors. After nearly 10 years of efforts, perovskite-based optoelectronic devices have made rapid progress. The highest certified efficiency of perovskite solar cells has reached 25.5%, which is comparable to crystalline silicon solar cells; the external quantum efficiency of perovskite electroluminescent devices has also exceeded 20%; in the field of lasers, high-quality low-threshold lasers can be achieved by regulating the morphology of perovskite materials. How to obtain perovskite devices with excellent performance has become the goal pursued by the scientific and industrial communities.

[0003] In recent years, the main research work on perovskite devices has focused on improving the film-forming process of perovskite materials, optimizing the components of the perovskite light-absorbing layer or light-emitting layer, and improving the interface transport layer materials. The interface exists between the adjacent functional layers of the perovskite device. The photogenerated carriers complete the extraction, transmission and collection process through the interface during the operation of the perovskite solar cell. The non-radiative recombination at the interface will cause energy loss in the perovskite solar cell, affecting the stability and performance of the device. In addition, the surface defects of the interface can not only quench the photoluminescence emission, but also damage the crystallinity and stability of the perovskite layer. At the same time, the energy level arrangement of the two adjacent materials at the interface will also affect the injection and transmission of charges. Therefore, the interface characteristics are also one of the key factors affecting the performance and stability of perovskite devices.

[0004] Currently, the most commonly used p-type hole transport material is PEDOT:PSS. However, PEDOT:PSS will severely corrode the indium tin oxide (ITO) anode, resulting in the release of In and Sn atoms, which diffuse into the perovskite layer, leading to exciton quenching and accelerating the degradation of the perovskite device, posing a serious threat to the long-term stability of the device. Inorganic p-type semiconductors such as carbon quantum dots, NiO x , and copper sulfide have excellent carrier mobility, high transmittance, and good chemical and physical stability, and are alternative hole transport materials for perovskite light-emitting devices. x NiO is particularly attractive due to its p-type properties such as wide bandgap, easily tunable electronic structure and good electron blocking ability. x-Surface traps and energy level mismatch at the perovskite interface adversely affect both the radiative recombination rate and device performance. A novel interface engineering method using sodium dodecyl sulfate-oxygen plasma (SDS-OP) can significantly deepen the NiO x The SDS-OP layer passivates the electron surface trap states of the perovskite film, inhibiting the electrons from being injected into the perovskite film. x Currently, the careful modification of the NiOx-perovskite interface and its impact on electroluminescence remain largely unexplored.

[0005] On the other hand, efficient perovskite solar cells require an ideal electron transport layer. Commonly used electron transport layer materials include TiO2, ZnO and SnO2. Interface modification can change the band structure of the charge transport layer, reduce interface recombination and regulate the morphology of the perovskite film, thereby improving device performance. The TiO2 electron transport layer modified with fullerene molecules can accelerate charge transfer and passivate the TiO2 / perovskite interface, thus achieving efficient and hysteresis-free perovskite cells; the ZnO surface is modified with alanine self-assembled molecular layer to match the interface energy level, which can induce the growth of high-quality perovskite films and improve the photoelectric conversion efficiency; the SnO2 / perovskite light absorption layer interface is modified with a self-assembled molecular layer formed by the hydrolysis of 3-aminopropyltriethoxysilane (APTES), which increases the surface energy and affinity of SnO2, thereby inducing the formation of high-quality perovskite films with better morphology and crystallinity, and the photoelectric conversion efficiency of the device is increased to 18.3%. In addition, (2-(9H-carbazole-9-yl)ethyl)phosphonic acid (2PACz) and its derivatives as hole transport layer or interface modification materials can not only change the work function of indium tin oxide (ITO) and inhibit the recombination loss at the interface, but also significantly improve the NiO x Energy level matching with perovskite promotes carrier transport and improves the photovoltaic performance of the device.

[0006] At present, the introduction of interface layer materials that interact with inorganic metal oxides (electron / hole transport layer components) has been proven to be an effective strategy to improve the efficiency and stability of perovskite optoelectronic devices. However, it is still necessary to develop new interface modification materials to have dual-functional organic molecules that can modify the carrier transport layer and passivate the surface defects of perovskite films, so as to further improve the efficiency and stability of perovskite optoelectronic devices. Summary of the invention

[0007] The technical problem solved by the present invention is a compound containing a phosphate group, a preparation method thereof and an application in a perovskite photoelectric device. The compound containing a phosphate group provided in the present application can improve the comprehensive performance of the perovskite photoelectric device.

[0008] The present application provides a compound containing a phosphate group as an interface modification material, wherein the phosphate group can interact with an inorganic metal oxide, adjust the energy level arrangement of an electron or hole transport layer, and facilitate carrier transport. At the same time, the phosphate group in the triaryl phosphate oxygen fragment can passivate surface defects of the perovskite film and reduce the non-radiative recombination of carriers at the interface. The synergistic effect of the two can effectively improve the comprehensive performance of perovskite optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 The H NMR spectrum of the compound I-7a containing a phosphate group prepared in Example 8 of the present invention;

[0010] Figure 2 This is the H NMR spectrum of the intermediate N-7c containing a phosphate group prepared in Example 10 of the present invention;

[0011] Figure 3 This is the H NMR spectrum of the intermediate L-7c containing a phosphate group prepared in Example 10 of the present invention;

[0012] Figure 4 The H NMR spectrum of the compound I-7c containing a phosphate group prepared in Example 10 of the present invention;

[0013] Figure 5 This is a graph showing the relationship between the external quantum efficiency and the current density of the electroluminescent device using compound I-7c as the interface modification layer in Example 55 of the present invention;

[0014] Figure 6 This is a current-voltage relationship diagram of a solar cell device using compound I-7c as an interface modification layer in Example 100 of the present invention. DETAILED DESCRIPTION

[0015] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0016] In order to further improve the performance of perovskite optoelectronic devices, the present application provides a compound containing a phosphate group, which, as an interface modification material, helps carrier transport and can also reduce the non-radiative recombination of carriers at the interface, thereby improving the comprehensive performance of the perovskite optoelectronic device. Specifically, the embodiment of the present invention discloses a compound containing a phosphate group as shown in formula (I),

[0017]

[0018] Wherein, X1, X2 and Y are each independently selected from O or S;

[0019] and Each is independently selected from a substituted C5-C60 aromatic ring group, an unsubstituted C5-C60 aromatic ring group, a substituted C3-C60 aromatic heterocyclic group or an unsubstituted C3-C60 aromatic heterocyclic group; the heteroatom in the aromatic heterocyclic group is selected from one or more of Si, Ge, N, P, O, S and Se;

[0020] n is an integer from 0 to 20.

[0021] In the present application, the compound containing a phosphate group has a structure shown in formula (II) to formula (IV):

[0022]

[0023] and Each is independently selected from a substituted or unsubstituted C5-C60 aromatic ring group, or a substituted or unsubstituted C3-C60 aromatic heterocyclic group;

[0024] The heteroatom in the heteroaromatic group is selected from one or more of Si, Ge, N, P, O, S and Se;

[0025] n is an integer from 0 to 20.

[0026] In the present application, the substituents in the substituted C5-C60 aromatic ring group and the substituted C3-C60 aromatic heterocyclic group are each independently selected from H, D, F, Cl, Br, I, CF3, -CN, -OR 1 、-SR 1 、-Se-R 1 ,-Te-R 1 , A C1-C30 straight-chain hydrocarbon group, a C3-C30 branched hydrocarbon group, a C1-C30 halogenated alkyl group, a C3-C30 cycloalkyl group, a C6-C60 aromatic group, or a C5-C60 heteroaromatic group;

[0027] Among them, the R 1 , R 2 and R 3 Each is independently selected from a C1-C30 straight-chain hydrocarbon group, a C3-C30 branched hydrocarbon group, a C1-C30 halogenated alkyl group, a C3-C30 cycloalkyl group, a C6-C60 aromatic group or a C5-C60 heteroaromatic group; the heteroatom in the heteroaromatic group is selected from one or more of Si, Ge, N, P, O, S and Se; R 1 , R 2 and R 3They can also be connected to each other via a single bond, -CC-, -C=C-, -C=N-, -O-, -S-, -Se-, or -Te-.

[0028] In the above technical solution, preferably, the and Each is independently selected from one of the groups represented by formula 1 to 29:

[0029]

[0030]

[0031] Among them, L3~L5 are each independently selected from a C1~C30 straight chain hydrocarbon group, a C3~C30 branched hydrocarbon group, a C1~C30 halogenated alkyl group, a C3~C30 cycloalkyl group, a C6~C60 aromatic group, or a C5~C60 heteroaromatic group; the heteroatom in the heteroaromatic group is selected from one or more of Si, Ge, N, P, O, S and Se.

[0032] In the above technical solution, it is further preferred that: and A substituted or unsubstituted C5-C48 aromatic ring group, or a substituted or unsubstituted C4-C45 aromatic heterocyclic group;

[0033] More preferably, Select one of the following structures:

[0034]

[0035]

[0036] More preferably, Select one of the following structures:

[0037]

[0038] Above and In the structure, the dotted lines represent the connections.

[0039] In the above technical solution, further, the compound containing a phosphate group has one of the structures shown in Formula I-1 to Formula I-90;

[0040]

[0041]

[0042]

[0043]

[0044]

[0045] In the above structure, the value of n is an integer of 0 to 4.

[0046] The present invention also provides a method for preparing a compound containing a phosphate group, comprising the following steps:

[0047] (A) subjecting a Grignard reagent or lithium salt represented by formula (Z) to a nucleophilic substitution reaction with diethyl phosphite or diethyl thiophosphite represented by formula (P1) to obtain an intermediate represented by formula (M);

[0048] (B) reacting the dihalide represented by formula (S) with the phosphate represented by formula (P2) through Michaelis-Arbuzov reaction to obtain an intermediate of a brominated aryl phosphonate represented by formula (N);

[0049] Or, a dihalide represented by formula (S) is reacted with a phosphate represented by formula (P3) through a phosphitylation reaction to obtain an intermediate of a brominated aryl phosphonate represented by formula (N);

[0050] (C) the intermediate represented by formula (M) is subjected to a phosphorylation reaction with the intermediate of the brominated aryl phosphonate represented by formula (N) to obtain the intermediate represented by formula (L);

[0051] (D) reacting the intermediate represented by formula (L) to obtain a compound containing a phosphate group represented by formula (I);

[0052]

[0053]

[0054] Wherein, the aryl group Ar1- corresponds to unit;

[0055] The aryl group Ar2- corresponds to unit;

[0056] More specifically, the aromatic group Ar1- corresponds to unit;

[0057] The aryl group Ar2- corresponds to the following in formula (II), (III) and (IV): unit;

[0058] The definitions of each substituent group and n are consistent with those in the above formula (I) and are not repeated here.

[0059] In the process of preparing a compound containing a phosphoric acid group, the present application first performs a nucleophilic substitution reaction between an Ar1 Grignard reagent or a lithium salt represented by formula (Z) and diethyl phosphite or diethyl thiophosphite represented by formula (P1) to form a diaryl phosphorus oxide or diaryl phosphorus sulfide intermediate represented by (Formula M). In this process, the reaction temperature is 0 to 25°C and the reaction time is 1.5 to 12 hours; more specifically, the reaction temperature is 15 to 25°C and the reaction time is 5 to 10 hours. Formula (Z) represents an Ar1 Grignard reagent or a lithium salt.

[0060] The present application then prepares an intermediate of a brominated aryl phosphate, that is, a dihalide represented by formula (S) and a phosphate represented by formula (P2) are subjected to a Michaelis-Arbuzov reaction to obtain an intermediate of a brominated aryl phosphonate represented by formula (N) (when n=1 to 4); or, a dihalide represented by formula (S) and a phosphate represented by formula (P3) are subjected to a phosphorylation reaction to obtain an intermediate of a brominated aryl phosphonate represented by formula (N) (when n=0); the right-side substituent in the dihalide represented by formula (S) can be Br or I. In this process, the temperature of the Michaelis-Arbuzov reaction is 100-150°C, and the time is 10-20 hours. Specifically, the temperature of the Michaelis-Arbuzov reaction is 110-140°C, and the time is 10-16 hours. The temperature of the phosphorylation reaction is 50-150°C, and the temperature of the reaction is 64-115°C, and the time is 5-20 hours. Specifically, the time is 8-16 hours. The catalytic system of the phosphorylation is palladium acetate / dppf / potassium acetate / triethylamine / THF or Pd(PPh3)4 / N-methylmorpholine / toluene.

[0061] According to the present invention, a diaryl phosphorus oxide or diaryl phosphorus sulfide intermediate as shown in formula (M) is then subjected to a phosphorylation reaction with an intermediate of a bromoaryl phosphonate as shown in formula (N) to obtain an intermediate containing P=X1 / phosphate group as shown in formula (L). In the above steps, the temperature of the phosphorylation reaction is 50-150°C, specifically, the temperature of the reaction is 64-115°C; the time is 5-20h, specifically, the time is 8-16h; the catalytic system of the phosphorylation reaction is palladium acetate / dppf / potassium acetate / triethylamine / THF or Pd(PPh3)4 / N-methylmorpholine / toluene.

[0062] Finally, the intermediate of P=X1 / phosphate group as shown in formula (L) is cracked by trimethylsilane bromide to generate a compound containing a phosphoric acid group. In this process, the reaction temperature is 20-50°C, specifically, the reaction temperature is 25°C; the cracking conditions are trimethylsilane bromide and methanol, and the time is 5-20h.

[0063] The present invention also provides the use of the compound containing a phosphate group shown in the above formula (I) as a perovskite interface modification material or additive; the interface modification layer is preferably prepared by a solution spin coating or immersion process, and the obtained film is annealed after the spin coating or immersion to obtain the interface modification layer; specifically, the compound containing a phosphate group described in the present invention can be used between the hole transport layer and the perovskite active layer, and can also be used between the perovskite active layer and the electron transport layer; it can also be added as an additive to the perovskite precursor solution to prepare the perovskite active layer by a spin coating process.

[0064] The present invention also provides a perovskite light-emitting device, comprising an anode, a cathode, and a carrier transport layer, an interface modification layer and a perovskite photoactive layer located between the anode and the cathode; the interface modification layer and / or the perovskite layer are prepared from the compound containing a phosphate group as described in the above technical solution.

[0065] In addition, the present invention also provides a perovskite solar cell device, comprising an anode, a cathode, and a carrier transport layer, an interface modification layer and a perovskite photoactive layer located between the anode and the cathode; the interface modification layer and / or the perovskite layer are prepared from the compound containing a phosphate group as described in the above technical solution.

[0066] The present invention has no particular limitation on the structure of the perovskite photoelectric device, and conventional perovskite light-emitting devices and solar cell devices familiar to those skilled in the art may be used. Those skilled in the art may select and adjust the structure according to application conditions, quality requirements and product requirements.

[0067] The present invention provides a compound containing a phosphoric acid group, which is applied to an interface modification layer material for use in a perovskite photoelectric device, and the structure is shown in formula (I). Compared with the prior art, the present invention can utilize the phosphoric acid group to interact with the carrier transport layer to form a self-assembled layer, effectively improve the wettability, and adjust the perovskite film structure; the phosphorus oxygen group in the compound structure can passivate the unsaturated coordinated lead defects in the perovskite lattice, reduce non-radiative energy loss, and improve the fluorescence quantum yield and carrier transport performance of the perovskite film; by introducing different substituents, the defect passivation effect can be further adjusted, and the interface energy level can be more matched.

[0068] The experimental results show that the use of the compound containing a phosphate group as the interface modification layer of the perovskite optoelectronic device can improve the carrier transport performance and achieve high device external quantum efficiency or photoelectric conversion efficiency, while substantially not affecting the structure and luminescence characteristics of the perovskite itself. The present invention can provide a structural design idea for the development of interface modification materials for high-performance perovskite optoelectronic devices.

[0069] In order to further understand the present invention, the compounds containing phosphate groups, preparation methods and applications thereof provided by the present invention are described in detail below in conjunction with examples. The protection scope of the present invention is not limited by the following examples.

[0070] Example 1

[0071] The reaction formula is as follows:

[0072]

[0073] The phosphate-substituted triphenylphosphine intermediate L-1a (2.07 g, 5.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (3.96 mL, 30 mmol) was added dropwise under argon protection. The reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol. The mixture was stirred at room temperature for 3 hours, and the methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-1a (1.29 g, yield 72%).

[0074] Example 2

[0075] The reaction formula is as follows:

[0076]

[0077] Diethyl phosphite (0.85 mL, 6.5 mmol) was dissolved in 10 mL of ether. After the reaction solution was cooled to 0°C, a phenylmagnesium bromide Grignard reagent ether solution (5.2 mL, 15.6 mmol) was added dropwise to the reaction flask, and the reaction solution was stirred at room temperature for 5 hours; the reaction solution was poured into 100 mL of NH4Cl aqueous solution, the mixture was extracted three times with ether, the combined organic phase was dried over Na2SO4, and after the solvent was completely removed, it was purified by silica gel column chromatography (petroleum ether / ethyl acetate = 2:1 as eluent) to obtain the product diphenylphosphine oxide M-1b (1.03 g, yield 78%) as a white solid; 1 HNMR (500MHz, CDCl3) δ: 8.03 (d, J=480.7Hz, 1H), 7.81-7.73 (m, 4H), 7.57-7.7.52 (m, 2H), 7.47-7.40 (m, 4H);

[0078] Add p-bromobenzyl bromide (12.5 g, 50 mmol) and triethyl phosphite (9.5 mL, 55 mmol) into a Schlenk reaction tube, evacuate the air three times, react at 125 degrees overnight, and complete the reaction of the raw materials on the plate. Slowly cool to 50 degrees, remove excess triethyl phosphite under reduced pressure, and separate and purify by silica gel column chromatography to obtain N-1b (14.6 g, yield 94%) as a light yellow liquid. 1H NMR (500MHz, CDCl3) δ: 7.44 (d, J=8.1Hz, 2H), 7.17 (d, J=8.2Hz, 2H), 3.96-4.08 (q, 4H), 3.09 (d, J=8.1Hz, 2H), 1.25 (t, J=7.1Hz, 6H);

[0079] Under argon atmosphere, (4-bromobenzyl) phosphonic acid diethyl ester N-1b (1.69g, 5.5mmol), bisphenylphosphine oxide M-1b (1.0g, 5.0mmol), N-methylmorpholine (0.75g, 7.5mmol) and tetrakis(triphenylphosphine) palladium (0.29g, 0.25mmol) were dissolved in 35mL of anhydrous toluene, heated to 100°C and stirred for 8 hours. After the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 2 / 1). Using n-hexane and dichloromethane as solvents, further purification by recrystallization gave L-1b as a pure white solid 1.6g, yield: 75%;

[0080] The phosphate derivative L-1b (1.6 g, 3.6 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (2.85 mL, 21.6 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was ultrasonically washed and recrystallized from methanol / ether to obtain a white solid I-1b (1.0 g, yield 75%).

[0081] Example 3

[0082] The reaction formula is as follows:

[0083]

[0084] Add p-bromophenylethyl bromide (2.64 g, 10 mmol) and triethyl phosphite (1.9 mL, 11 mmol) into a Schlenk reaction tube, evacuate the air three times, react at 125 degrees overnight, and complete the reaction of the raw materials on the plate. Slowly cool to 50 degrees, remove excess triethyl phosphite under reduced pressure, and separate and purify by silica gel column chromatography to obtain (4-bromophenylethyl) diethyl phosphonate N-1c (3.0 g, yield 92%) as a light yellow liquid. 1 H NMR (500MHz, DMSO) δ7.47 (d, J=8.3Hz, 2H), 7.24 (d, J=8.4Hz, 2H), 3.98 (dd, J=11.2, 4.1Hz, 4H), 2.75 (td, J=11.3, 8.3Hz, 2H), 2.16–1.96 (m, 2H), 1.21 (t, J=7.1Hz, 6H);

[0085] Under argon atmosphere, diethyl (4-bromophenylethyl)phosphonate N-1c (1.76 g, 5.5 mmol), bisphenylphosphine oxide (1.0 g, 5.0 mmol), N-methylmorpholine (0.75 g, 7.5 mmol) and tetrakis(triphenylphosphine)palladium (0.29 g, 0.25 mmol) were dissolved in 35 mL of anhydrous toluene, heated to 100 ° C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 2 / 1) to obtain 1.7 g of L-1c as a colorless liquid, with a yield of 78%;

[0086] The phosphate derivative L-1c (1.6 g, 3.6 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (2.85 mL, 21.6 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid (0.9 g, yield 68%).

[0087] Example 4

[0088] The reaction formula is as follows:

[0089]

[0090] The phosphate derivative L-6a (2.07 g, 5.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (3.2 mL, 30 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-6a (1.29 g, yield 72%).

[0091] Example 5

[0092] The reaction formula is as follows:

[0093]

[0094] Under an argon atmosphere, magnesium chips (0.53 g, 21.0 mmol) and a small particle of iodine were placed in a dry three-necked flask, p-fluorobromobenzene (3.50 g, 20.0 mmol) was dissolved in dry THF (100 mL) and placed in a constant pressure dropping funnel, about 15 mL of p-fluorobromobenzene THF solution was added to the three-necked flask, and the remaining solution was slowly dripped in after the brown-yellow color faded. After the dropwise addition was completed, it was heated to reflux for 2 hours, and the reaction solution was cooled to 0°C, and diethyl phosphite (1.19 mL, 9.1 mmol) was added dropwise; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried over Na2SO4 to completely remove the solvent, and then separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 2:1) to obtain the product bis(4-fluorophenyl)phosphine oxide M-6a (3.19 g, yield 67%) as a white solid;

[0095] Under argon atmosphere, (4-bromobenzyl) diethyl phosphonate N-6b (1.33 g, 4.4 mmol), bis(4-fluorophenyl)phosphine oxide M-6a (0.96 g, 4.0 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine) palladium (0.24 g, 0.20 mmol) were dissolved in 30 mL of anhydrous toluene, heated to 100°C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (eluent: petroleum ether / ethyl acetate = 1 / 1). Using n-hexane and dichloromethane as solvents, further purification was obtained by recrystallization to obtain 1.3 g of pure white solid L-6b, with a yield of 77%;

[0096] The phosphate derivative L-6b (1.32 g, 3.0 mmol) was dissolved in 12 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-6a (1.2 g, yield 67%).

[0097] Example 6

[0098] The reaction formula is as follows:

[0099]

[0100] Under argon atmosphere, diethyl (4-bromophenylethyl)phosphonate N-6c (1.41 g, 4.4 mmol), bis(4-fluorophenyl)phosphine oxide (0.96 g, 4.0 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine)palladium (0.24 g, 0.20 mmol) were dissolved in 30 mL of anhydrous toluene, heated to 100 ° C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1 / 1) to obtain L-6c (1.6 g, yield: 83%), which was a colorless liquid;

[0101] The phosphate derivative L-6c (1.43 g, 3.0 mmol) was dissolved in 12 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-6c (0.96 g, yield 76%).

[0102] Example 7

[0103] The reaction formula is as follows:

[0104]

[0105] Add p-bromophenylbutyl bromide (2.92 g, 10 mmol) and triethyl phosphite (1.9 mL, 11 mmol) into a Schlenk reaction tube, evacuate the air three times, react at 125 degrees overnight, and when the reaction of the raw material on the plate is complete, slowly cool to 50 degrees, remove the excess triethyl phosphite under reduced pressure, and separate and purify by silica gel column chromatography to obtain N-6d (3.14 g, yield 90%) as a colorless liquid;

[0106] Under argon atmosphere, diethyl (4-bromophenylbutyl)phosphonate N-6d (1.53 g, 4.4 mmol), bis(4-fluorophenyl)phosphine oxide (0.96 g, 4.0 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine)palladium (0.24 g, 0.20 mmol) were dissolved in 30 mL of anhydrous toluene, heated to 100°C and stirred overnight. After the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1 / 1) to obtain L-6d (1.7 g, yield: 86%), which was a colorless liquid;

[0107] The phosphate derivative L-6d (1.52 g, 3.0 mmol) was dissolved in 12 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 5 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-6d (0.90 g, yield 67%).

[0108] Example 8

[0109] The reaction formula is as follows:

[0110]

[0111] The phosphate derivative L-7a (1.45 g, 3.0 mmol) was dissolved in 15 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 4 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-7a (0.99 g, yield 77%). 1 HNMR (500 MHz, DMSO) δ: 11.34 (br, 2H, OH), 7.85-7.64 (m, 12H, ArH); Figure 1 As shown, Figure 1 This is the H NMR spectrum of I-7a prepared in this example.

[0112] Example 9

[0113] The reaction formula is as follows:

[0114]

[0115] Under an argon atmosphere, magnesium chips (0.37 g, 15.0 mmol) and a small particle of iodine were added to a dry three-necked flask, p-bromochlorobenzene (2.49 g, 13.0 mmol) was dissolved in dry tetrahydrofuran (80 mL) and placed in a constant pressure dropping funnel, about 10 mL of p-bromochlorobenzene in THF solution was added to the three-necked flask, and the remaining solution was slowly dripped in after the brown-yellow color faded. After the addition was complete, it was heated to reflux for 2 hours, and the reaction solution was cooled to 0°C, and diethyl phosphite (0.56 mL, 4.3 mmol) was added dropwise; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried over Na2SO4; after the solvent was completely removed, it was purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain the product bis(4-chlorophenyl)phosphine oxide M-7b as a white solid (2.1 g, yield 60%). 1 HNMR (500MHz, CDCl3) δ: 8.07 (d, J=486.6Hz, 1H), 7.63 (dd, J=13.3, 8.4Hz, 4H), 7.50 (dd, J=13.5, 2.2Hz, 4H);

[0116] Under argon atmosphere, diethyl (4-bromobenzyl)phosphonate N-7b (1.35 g, 4.4 mmol), bis(4-chlorophenyl)phosphine oxide M-7b (1.08 g, 4.0 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine)palladium (0.24 g, 0.20 mmol) were dissolved in 30 mL of anhydrous toluene, heated to 100 ° C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1 / 1); using n-hexane and dichloromethane as solvents, further purified by recrystallization to obtain 1.7 g of pure white solid L-7b, yield: 84%;

[0117] The phosphate derivative L-7b (1.49 g, 3.0 mmol) was dissolved in 12 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was ultrasonically washed and recrystallized from methanol / ether to obtain a white solid I-7b (0.9 g, yield 71%).

[0118] Example 10

[0119] The reaction formula is as follows:

[0120]

[0121] Under argon atmosphere, diethyl (4-bromophenylethyl)phosphonate N-7c (1.41 g, 4.4 mmol), bis(4-chlorophenyl)phosphine oxide (1.08 g, 4.0 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine)palladium (0.24 g, 0.20 mmol) were dissolved in 30 mL of anhydrous toluene, heated to 100 ° C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1 / 1) to obtain L-7c (1.5 g, yield: 74%), which was a colorless liquid; 1 H NMR (400MHz, CDCl3) δ7.57 (dt, J=12.4, 7.2Hz, 6H), 7.45 (dd, J=8.4, 2.0Hz, 4H), 7.33 (dd, J=8.0, 2.2 Hz, 2H), 4.26-3.97 (m, 4H), 2.98 (dd, J=16.8, 10.5Hz, 2H), 2.22-1.96 (m, 2H), 1.31 (t, J=7.1Hz, 6H); such as Figure 2 As shown, Figure 2 is the H NMR spectrum of N-7c in this example, Figure 3 As shown, Figure 3 This is the H NMR spectrum of L-7c prepared in this example;

[0122] The phosphate derivative L-7c (1.5 g, 3.0 mmol) was dissolved in 12 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-7c (0.86 g, yield 63%). 1 H NMR (400 MHz, DMSO) δ 7.87-7.32 (m, 12H), 3.00-2.75 (m, 2H), 1.98-1.75 (m, 2H); Figure 4 As shown, Figure 4 This is the H NMR spectrum of I-7c prepared in this example.

[0123] Embodiment 11

[0124] The reaction formula is as follows:

[0125]

[0126] Under argon atmosphere, diethyl (4-bromophenylbutyl)phosphonate N-7d (1.53 g, 4.4 mmol), bis(4-chlorophenyl)phosphine oxide (1.08 g, 4.0 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine)palladium (0.24 g, 0.20 mmol) were dissolved in 30 mL of anhydrous toluene, heated to 100 ° C and stirred overnight; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1 / 1) to obtain L-7d (1.6 g, yield: 76%), which was a colorless liquid;

[0127] The phosphate derivative L-7d (1.6 g, 3.0 mmol) was dissolved in 12 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 5 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain a white solid I-7d (0.9 g, yield 62%).

[0128] Example 12

[0129] The reaction formula is as follows:

[0130]

[0131] The phosphate derivative L-8a (2.86 g, 5.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (3.2 mL, 30 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-8a (1.7 g, yield 66%).

[0132] Embodiment 13

[0133] The reaction formula is as follows:

[0134]

[0135] Under argon atmosphere, magnesium chips (0.53 g, 21.0 mmol) and a small particle of iodine were placed in a dry three-necked flask, p-dibromobenzene (4.72 g, 20.0 mmol) was dissolved in dry THF (100 mL) and placed in a constant pressure dropping funnel, about 15 mL of p-dibromobenzene THF solution was added to the three-necked flask, and the remaining solution was slowly dripped into the three-necked flask after the brown-yellow color faded. After the addition was completed, it was heated to reflux for 2 hours, and the reaction solution was cooled to 0°C, and diethyl phosphite (1.19 mL, 9.1 mmol) was added dropwise; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried over Na2SO4; after the solvent was completely removed, column chromatography was performed on a silica gel column with petroleum ether / ethyl acetate = 2:1 eluent to obtain the product bis(4-bromophenyl)phosphine oxide M-8b as a white solid (5.1 g, yield 71%);

[0136] Dissolve bis(4-bromophenyl)phosphine oxide M-8b (1.44 g, 4.0 mmol), diethyl (4-bromobenzyl)phosphonate N-8b (1.35 g, 4.4 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine)palladium (0.24 g, 0.20 mmol) in 30 mL of anhydrous toluene, heat to 100 °C and stir overnight. After the reaction is cooled to room temperature, the solvent is removed under reduced pressure, and the product L-8b is separated and purified by silica gel column chromatography to obtain 2.1 g of the product, with a yield of 88%;

[0137] The phosphate derivative L-8b (1.76 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-8b (1.2 g, yield 79%).

[0138] Embodiment 14

[0139] The reaction formula is as follows:

[0140]

[0141] Dissolve bis(4-bromophenyl)phosphine oxide (1.44 g, 4.0 mmol) and diethyl(4-bromophenylethyl)phosphonate N-8c (1.41 g, 4.4 mmol), N-methylmorpholine (0.60 g, 6.0 mmol) and tetrakis(triphenylphosphine)palladium (0.24 g, 0.20 mmol) in 30 mL of anhydrous toluene, heat to 100° C. and stir overnight; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography to obtain 1.6 g of L-8c product as a colorless liquid with a yield of 67%;

[0142] The phosphate derivative L-8c (1.6 g, 2.7 mmol) was dissolved in 18 mL of dry dichloromethane, and trimethylsilyl bromide (1.71 mL, 16.2 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was ultrasonically washed and recrystallized from methanol / ether to obtain a white solid I-8c (1.1 g, yield 75%).

[0143] Embodiment 15

[0144] The reaction formula is as follows:

[0145]

[0146] The phosphate derivative L-13a (2.25 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was ultrasonically washed and recrystallized from methanol / ether to obtain a light yellow solid I-13a (1.6 g, yield 76%).

[0147] Example 16

[0148] The reaction formula is as follows:

[0149]

[0150] Under argon atmosphere, magnesium chips (0.27g, 10.5mmol) and a small particle of iodine were placed in a dry three-necked flask, 4-bromotriphenylamine (3.24g, 10.0mmol) was dissolved in dry ether (60mL) and placed in a constant pressure dropping funnel, about 8mL of 4-bromotriphenylamine ether solution was added to the three-necked flask, and the remaining solution was slowly dripped into the three-necked flask after the brown-yellow color faded. After the addition was completed, it was heated to reflux for 2 hours, and the reaction solution was cooled to 0°C, and diethyl phosphite (0.6mL, 4.6mmol) was added dropwise. After stirring at room temperature for 8 hours, the reaction solution was poured into 60mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried over Na2SO4. After the solvent was completely removed, column chromatography was performed on a silica gel column with petroleum ether / ethyl acetate = 1:1 as eluent to obtain the product bis(4-diphenylaminophenyl)phosphine oxide M-13c as a white solid (3.27 g, yield 61%);

[0151] Under argon atmosphere, diethyl (4-bromophenylethyl)phosphonate (1.41 g, 4.4 mmol), bis(4-diphenylaminophenyl)phosphine oxide M-13c (2.16 g, 4.0 mmol) were dissolved in anhydrous THF (15 mL), evacuated three times, palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (84 mg, 0.88 mmol) and triethylamine (0.84 mL, 13.2 mmol) were added, and the mixture was heated to 74 ° C and stirred for 12 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1); using n-hexane and dichloromethane as solvents, further purified by recrystallization to obtain 2.27 g of L-13c as a light yellow solid, with a yield of 73%;

[0152] The phosphate derivative L-13c (2.10 g, 2.7 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.71 mL, 16.2 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was ultrasonically washed with water and recrystallized from methanol / diethyl ether to obtain a light yellow solid I-13c (1.3 g, yield 65%).

[0153] Embodiment 17

[0154] The reaction formula is as follows:

[0155]

[0156] The phosphate derivative L-15a (2.45 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain I-15a as a light yellow solid (1.3 g, yield 58%).

[0157] Embodiment 18

[0158] The reaction formula is as follows:

[0159]

[0160] Under argon atmosphere, the phosphate derivative L-8c (2.64 g, 4.4 mmol) and bisphenylphosphine oxide (0.81 g, 4.0 mmol) were dissolved in anhydrous THF (15 mL), evacuated three times, palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (84 mg, 0.88 mmol) and triethylamine (0.84 mL, 13.2 mmol) were added, and the temperature was raised to 74 ° C. and stirred for 16 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (dichloromethane / methanol=100:1); using n-hexane and dichloromethane as solvents, it was further purified by recrystallization to obtain 1.89 g of L-15c as a light yellow solid, with a yield of 56%;

[0161] The phosphate derivative L-15c (1.72 g, 2.1 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.33 mL, 12.6 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure, ultrasonically washed, and recrystallized from tetrahydrofuran / n-hexane to obtain a light yellow solid I-15c (0.88 g, yield 53%).

[0162] Embodiment 19

[0163] The reaction formula is as follows:

[0164]

[0165] The phosphate derivative L-29a (1.46 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain I-29a as a white solid (0.85 g, yield 66%).

[0166] Embodiment 20

[0167] The reaction formula is as follows:

[0168]

[0169] Under argon atmosphere, magnesium chips (0.53 g, 21.0 mmol) and a small particle of iodine were placed in a dry three-necked flask. 3,4-difluorobromobenzene (3.86 g, 20.0 mmol) was dissolved in dry THF (100 mL) and placed in a constant pressure dropping funnel. About 15 mL of 3,4-difluorobromobenzene in THF solution was added to the three-necked flask. After the brown-yellow color faded, the remaining solution was slowly dripped in. After the addition was completed, it was heated to reflux for 2 hours. After the reaction solution was cooled to 0°C, diethyl phosphite (1.19 mL, 9.1 mmol) was added dropwise. After stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried over Na2SO4; after the solvent was completely removed, column chromatography was performed on a silica gel column with petroleum ether / ethyl acetate = 2:1 eluent to obtain the product bis(3,4-difluorophenyl)phosphine oxide as a white solid (3.4 g, yield 63%);

[0170] Dissolve bis(3,4-difluorophenyl)phosphine oxide (1.09 g, 4.0 mmol) and diethyl(4-bromophenylethyl)phosphonate (1.41 g, 4.4 mmol) in anhydrous THF (15 mL), evacuate and purify for three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (84 mg, 0.88 mmol) and triethylamine (0.84 mL, 13.2 mmol), heat to 74° C. and stir for 16 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, and the crude product is separated and purified by silica gel column chromatography (eluent: petroleum ether / ethyl acetate=4:1); use n-hexane and dichloromethane as solvents, and further purify by recrystallization to obtain 1.5 g of L-29c as a white solid, with a yield of 74%;

[0171] The phosphate derivative L-29c (1.39 g, 2.7 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.71 mL, 16.2 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-29c (0.73 g, yield 59%).

[0172] Embodiment 21

[0173] The reaction formula is as follows:

[0174]

[0175] The phosphate derivative L-30a (1.65 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.1 g of I-30a as a white solid with a yield of 72%.

[0176] Embodiment 22

[0177] The reaction formula is as follows:

[0178]

[0179] Under argon atmosphere, magnesium chips (0.53 g, 21.0 mmol) and a small particle of iodine were placed in a dry three-necked flask. 3,4-dichlorobromobenzene (4.52 g, 20.0 mmol) was dissolved in dry THF (100 mL) and placed in a constant pressure dropping funnel. About 15 mL of 3,4-dichlorobromobenzene in THF solution was added to the three-necked flask. After the brown-yellow color faded, the remaining solution was slowly dripped in. After the addition was completed, it was heated to reflux for 2 hours. After the reaction solution was cooled to 0°C, diethyl phosphite (1.19 mL, 9.1 mmol) was added dropwise. After stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried over Na2SO4; after the solvent was completely removed, column chromatography was performed on a silica gel column with petroleum ether / ethyl acetate = 4:1 eluent to obtain the product bis(3,4-dichlorophenyl)phosphine oxide as a white solid (4.5 g, yield 66%);

[0180] Dissolve bis(3,4-difluorophenyl)phosphine oxide (1.36 g, 4.0 mmol) and diethyl(4-bromophenylethyl)phosphonate (1.41 g, 4.4 mmol) in anhydrous THF (15 mL), evacuate and purify three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (84 mg, 0.88 mmol) and triethylamine (0.84 mL, 13.2 mmol), heat to 74 °C and stir for 16 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, and the crude product is separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 4:1). Using n-hexane and dichloromethane as solvents, further purification by recrystallization gives 1.8 g of L-30c as a white solid with a yield of 77%;

[0181] The phosphate derivative L-30c (1.74 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.1 g of I-30c as a white solid with a yield of 67%.

[0182] Embodiment 23

[0183] The reaction formula is as follows:

[0184]

[0185] The phosphate derivative L-39a (1.29 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.88 g of I-39a as a white solid with a yield of 78%.

[0186] Embodiment 24

[0187] The reaction formula is as follows:

[0188]

[0189] Diethyl thiophosphite (1.0 g, 6.5 mmol) was dissolved in 10 mL of ether. After the reaction solution was cooled to 0°C, a solution of phenylmagnesium bromide Grignard reagent in ether (5.2 mL, 15.6 mmol) was added dropwise to the reaction flask, and the reaction solution was stirred at room temperature for 7 hours; the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with ether, and the combined organic phase was dried over Na2SO4; after the solvent was completely removed, the product was purified by silica gel column chromatography (petroleum ether / ethyl acetate = 2:1 as eluent) to obtain the product diphenylphosphonium sulfide (0.95 g, yield 67%) as a white solid;

[0190] Under argon atmosphere, diethyl (4-bromophenylethyl)phosphonate (1.41 g, 4.4 mmol), diphenylphosphine sulfide (0.88 g, 4.0 mmol), N-methylmorpholine (0.30 g, 3.0 mmol) and tetrakis(triphenylphosphine)palladium (0.12 g, 0.10 mmol) were dissolved in 15 mL of anhydrous toluene, heated to 100 ° C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (eluent: petroleum ether / ethyl acetate = 1 / 1) to obtain 1.5 g of L-39c colorless liquid, yield: 79%;

[0191] The phosphate derivative L-39c (1.37 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.74 g of I-39c as a white solid with a yield of 61%.

[0192] Embodiment 25

[0193] The reaction formula is as follows:

[0194]

[0195] The phosphate derivative L-51a (1.44 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.91 g of I-51a as a white solid with a yield of 72%.

[0196] Embodiment 26

[0197] The reaction formula is as follows:

[0198]

[0199] 4-Bromophenylethyl bromide (2.16 g, 8 mmol) and triethyl trithiophosphite (1.64 g, 8.8 mmol) were added to a Schlenk reaction tube, ventilated three times, reacted at 125 degrees overnight, and the reaction of the raw materials on the plate was completed. The reaction was slowly cooled to 50 degrees, and the excess triethyl trithiophosphite was removed under reduced pressure. The mixture was separated and purified by silica gel column chromatography to obtain (4-bromophenylethyl) diethyl trithiophosphorate N-51c (2.77 g, yield 94%) as a light yellow liquid;

[0200] Under argon atmosphere, diethyl (4-bromophenylethyl) trithiophosphate (1.62 g, 4.4 mmol), diphenylphosphine sulfide (1.46 g, 4.0 mmol), N-methylmorpholine (0.30 g, 3.0 mmol) and tetrakis(triphenylphosphine)palladium (0.12 g, 0.10 mmol) were dissolved in 15 mL of anhydrous toluene, heated to 100 ° C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 2 / 1) to obtain 1.32 g of L-51c as a light yellow liquid, with a yield of 65%;

[0201] The phosphate derivative L-51c (1.15 g, 2.4 mmol) was dissolved in 16 mL of dry dichloromethane, and trimethylsilyl bromide (1.52 mL, 14.4 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.65 g of I-51c as a white solid with a yield of 60%.

[0202] Embodiment 27

[0203] The reaction formula is as follows:

[0204]

[0205] The phosphate derivative L-63a (1.24 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 6 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.68 g of I-63a as a white solid with a yield of 63%.

[0206] Embodiment 28

[0207] The reaction formula is as follows:

[0208]

[0209] m-Bromophenylethyl bromide (2.64 g, 10 mmol) and triethyl phosphite (1.9 mL, 11 mmol) were added to a Schlenk reaction tube, ventilated three times, reacted at 125 degrees overnight, and the reaction of the raw materials on the plate was completed. The reaction was slowly cooled to 50 degrees, and the excess triethyl phosphite was removed under reduced pressure. The mixture was separated and purified by silica gel column chromatography to obtain N-63c (3.1 g, yield 94%) as a colorless liquid;

[0210] Under argon atmosphere, diethyl (3-bromophenylethyl)phosphonate N-63c (1.76 g, 5.5 mmol), bisphenylphosphine oxide (1.0 g, 5.0 mmol), N-methylmorpholine (0.75 g, 7.5 mmol) and tetrakis(triphenylphosphine)palladium (0.29 g, 0.25 mmol) were dissolved in 35 mL of anhydrous toluene, heated to 100 ° C and stirred for 8 hours; after the reaction was cooled to room temperature, the solvent was removed under reduced pressure, and the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 2 / 1) to obtain 1.8 g of L-63c as a colorless liquid, with a yield of 83%;

[0211] The phosphate derivative L-63c (1.33 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.74 g of white solid I-63c with a yield of 64%.

[0212] Embodiment 29

[0213] The reaction formula is as follows:

[0214]

[0215] The phosphate derivative L-75a (2.04 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.29 g of white solid I-75a with a yield of 69%.

[0216] Embodiment 30

[0217] The reaction formula is as follows:

[0218]

[0219] At -78°C, n-butyl lithium (4.4 mL, 2.5 M) was added dropwise to a solution of 3-bromo-5,5-dimethyldibenzosilylene (3.18 g, 11 mmol) in anhydrous THF (100 mL), stirred at -78°C for 30 minutes, and then diethyl phosphite (0.69 g, 5.0 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phases were dried over Na2SO4; after the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain bis(9,9-dimethyl-9-silafluorene-2-yl)phosphine oxide M-75c 1.42 g, white solid, yield: 61%;

[0220] Dissolve bis(9,9-dimethyl-9-silafluorene-2-yl)M-75c (1.4 g, 3.0 mmol) and diethyl (4-bromophenylethyl) phosphate (1.06 g, 3.3 mmol) in anhydrous THF (15 mL), evacuate the air three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74°C and stir for 15 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate=1:1) to obtain 1.82 g of L-75c as a white solid, yield: 86%;

[0221] The phosphate derivative L-75c (1.69 g, 2.4 mmol) was dissolved in 16 mL of dry dichloromethane, and trimethylsilyl bromide (1.52 mL, 14.4 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.1 g of I-75c as a white solid with a yield of 73%.

[0222] Embodiment 31

[0223] The reaction formula is as follows:

[0224]

[0225] The phosphate derivative L-76a (1.48 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.93 g of white solid I-76a with a yield of 71%.

[0226] Embodiment 32

[0227] The reaction formula is as follows:

[0228]

[0229] At -78 ° C, n-butyl lithium (4.4 mL, 2.5 M) was added dropwise to a solution of 2-bromobenzofuran (2.17 g, 11 mmol) in anhydrous THF (100 mL), stirred at -78 ° C for 30 minutes, and then diethyl phosphite (0.69 g, 5.0 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phases were dried over Na2SO4; after the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain bis(benzofuran-2-yl)phosphine oxide M-76c1.04 g, white solid, yield: 74%;

[0230] Dissolve bis(benzofuran-2-yl)phosphine oxide M-76c (1.02 g, 3.6 mmol) and diethyl (4-bromophenylethyl) phosphate (1.28 g, 4 mmol) in anhydrous THF (25 mL), evacuate the air three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74°C and stir for 8 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate=1:1) to obtain L-76c 1.42 g as a white solid, yield: 76%;

[0231] The phosphate derivative L-76c (1.41 g, 2.7 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.7 mL, 16.2 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.83 g of white solid I-76c with a yield of 66%.

[0232] Embodiment 33

[0233] The reaction formula is as follows:

[0234]

[0235] The phosphate derivative L-77a (1.58 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.03 g of white solid I-77a with a yield of 73%.

[0236] Embodiment 34

[0237] The reaction formula is as follows:

[0238]

[0239] At -78 ° C, n-butyl lithium (4.4 mL, 2.5 M) was added dropwise to a solution of 2-bromobenzothiophene (2.34 g, 11 mmol) in anhydrous THF (100 mL), stirred at -78 ° C for 30 minutes, and then diethyl phosphite (0.69 g, 5.0 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution. The mixture was extracted three times with dichloromethane, and the combined organic phase was dried with Na2SO4; after the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain bis (benzothiophene-2-yl) phosphorus oxide M-77c 1.05 g, white solid, yield 67%;

[0240] Dissolve bis(benzothiophene-2-yl)phosphine oxide M-77c (0.94 g, 3.0 mmol) and diethyl (4-bromophenylethyl) phosphate (1.02 g, 3.2 mmol) in anhydrous THF (18 mL), evacuate the air three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74 ° C and stir for 12 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain L-77c 1.33 g, white solid, yield: 80%;

[0241] The phosphate derivative L-77c (1.33 g, 2.4 mmol) was dissolved in 15 mL of dry dichloromethane, and trimethylsilyl bromide (1.2 mL, 10.8 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.82 g of white solid I-77c with a yield of 69%.

[0242] Embodiment 35

[0243] The reaction formula is as follows:

[0244]

[0245] The phosphate derivative L-79a (1.78 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.27 g of white solid I-79a with a yield of 79%.

[0246] Embodiment 36

[0247] The reaction formula is as follows:

[0248]

[0249] At -78 ° C, n-butyl lithium (8.8 mL, 2.5 M) was added dropwise to a solution of 3-bromodibenzofuran (5.44 g, 22 mmol) in anhydrous THF (150 mL), and the mixture was stirred at -78 ° C for 30 minutes, and then diethyl phosphite (1.38 g, 10 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phases were dried over Na2SO4; after the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate=1:1) to obtain bis(dibenzofuran-3-yl)phosphine oxide M-79c2.21 g as a white solid with a yield of 58%;

[0250] Dissolve bis(dibenzofuran-3-yl)phosphine oxide M-79c (2.14 g, 4.0 mmol) and diethyl (4-bromophenylethyl) phosphate (1.41 g, 4.4 mmol) in anhydrous THF (25 mL), evacuate and purify for three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74°C and stir for 15 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate=1:1) to obtain 1.62 g of L-79c product as a white solid, with a yield of 65%;

[0251] The phosphate derivative L-79c (1.50 g, 2.4 mmol) was dissolved in 15 mL of dry dichloromethane, and trimethylsilyl bromide (1.2 mL, 10.8 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.96 g of I-79c as a white solid with a yield of 71%.

[0252] Embodiment 37

[0253] The reaction formula is as follows:

[0254]

[0255] The phosphate derivative L-80a (1.88 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.2 g of white solid I-80a with a yield of 70%.

[0256] Embodiment 38

[0257] The reaction formula is as follows:

[0258]

[0259] At -78 ° C, n-butyl lithium (8.8 mL, 2.5 M) was added dropwise to a solution of 3-bromodibenzothiophene (2.63 g, 10 mmol) in anhydrous THF (150 mL), stirred at -78 ° C for 30 minutes, and then diethyl phosphite (1.38 g, 10 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour. After stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried with Na2SO4; after the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain bis (dibenzothiophene-3-yl) phosphorus oxide M-80c2.5g, white solid, yield: 60%.

[0260] Dissolve bis(dibenzothiophene-3-yl)phosphine oxide (1.66 g, 4.0 mmol) and diethyl (4-bromophenylethyl) phosphate (1.41 g, 4.4 mmol) in anhydrous THF (25 mL), evacuate the air three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74 ° C and stir for 8 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate=1:1) to obtain 1.89 g of white solid L-80c, with a yield of 72%.

[0261] The phosphate derivative L-80c (1.77 g, 2.7 mmol) was dissolved in 18 mL of dry dichloromethane, and trimethylsilyl bromide (1.71 mL, 16.2 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 10 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / ether to obtain 0.95 g of I-80c as a white solid with a yield of 59%.

[0262] Embodiment 39

[0263] The reaction formula is as follows:

[0264]

[0265] The phosphate derivative L-81a (1.95 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.26 g of yellow solid I-81a with a yield of 71%.

[0266] Embodiment 40

[0267] The reaction formula is as follows:

[0268]

[0269] At -78 ° C, n-butyl lithium (8.8 mL, 2.5 M) was added dropwise to a solution of 2-bromo-N-ethylcarbazole (2.74 g, 10 mmol) in anhydrous THF (150 mL), stirred at -78 ° C for 30 minutes, and then diethyl phosphite (1.38 g, 10 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour. After stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried with Na2SO4. After the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain bis (N-ethylcarbazole-2-yl) phosphorus oxide M-81c2.75 g, light yellow solid, yield 63%.

[0270] Dissolve bis(N-ethylcarbazole-2-yl)phosphine oxide M-81c (1.74 g, 4.0 mmol) and diethyl (4-bromophenylethyl) phosphate (1.41 g, 4.4 mmol) in anhydrous THF (25 mL), evacuate the air three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74 ° C and stir for 8 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain L-81c 2.17 g, yellow solid, yield 80%;

[0271] The phosphate derivative L-81c (2.03 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.25 g of yellow solid I-81c with a yield of 67%.

[0272] Embodiment 41

[0273] The reaction formula is as follows:

[0274]

[0275] The phosphate derivative L-83a (2.04 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.24 g of white solid I-83a with a yield of 66%.

[0276] Embodiment 42

[0277] The reaction formula is as follows:

[0278]

[0279] At -78 ° C, n-butyl lithium (8.8 mL, 2.5 M) was added dropwise to a solution of 3-bromo-10-ethyl-10H-phenoxazine (2.90 g, 10 mmol) in anhydrous THF (150 mL), stirred at -78 ° C for 30 minutes, and then diethyl phosphite (1.38 g, 10 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour; after stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried with Na2SO4. After the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain bis (10-ethyl-10H-phenoxazine-3-yl) phosphorus oxide M-83c3.13 g, yellow solid, yield 67%;

[0280] Dissolve bis(10-ethyl-10H-phenoxazine-3-yl)phosphine oxide (1.87 g, 4.0 mmol) and diethyl (4-bromophenylethyl) phosphate (1.41 g, 4.4 mmol) in anhydrous THF (25 mL), evacuate the air three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74°C and stir for 8 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate=1:1) to obtain L-832.1 g as a yellow solid with a yield of 73%;

[0281] The phosphate derivative L-83c (1.91 g, 2.7 mmol) was dissolved in 18 mL of dry dichloromethane, and trimethylsilyl bromide (1.71 mL, 16.2 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / ether to obtain 1.1 g of yellow solid I-80c with a yield of 64%.

[0282] Embodiment 43

[0283] The reaction formula is as follows:

[0284]

[0285] The phosphate derivative L-84a (2.14 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The product was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain 1.24 g of yellow solid I-84a with a yield of 63%.

[0286] Embodiment 44

[0287] The reaction formula is as follows:

[0288]

[0289] At -78 ° C, n-butyl lithium (8.8 mL, 2.5 M) was added dropwise to a solution of 3-bromo-10-ethyl-10H-phenothiazine (3.06 g, 10 mmol) in anhydrous THF (150 mL), stirred at -78 ° C for 30 minutes, and then diethyl phosphite (1.38 g, 10 mmol) was slowly added; the mixture was slowly warmed to room temperature within 1 hour. After stirring at room temperature for 8 hours, the reaction solution was poured into 100 mL of NH4Cl aqueous solution; the mixture was extracted three times with dichloromethane, and the combined organic phase was dried with Na2SO4. After the solvent was completely removed, the crude product was separated and purified by silica gel column chromatography (petroleum ether / ethyl acetate = 1:1) to obtain bis (10-ethyl-10H-phenothiazine-3-yl) phosphorus oxide M-84c2.76 g, light yellow solid, yield 55%;

[0290] Dissolve bis(10-ethyl-10H-phenothiazine-3-yl)phosphine oxide (2.00 g, 4.0 mmol) and diethyl (4-bromophenylethyl) phosphate (1.41 g, 4.4 mmol) in anhydrous THF (25 mL), evacuate the air three times, add palladium acetate (27 mg, 0.12 mmol), 1,1'-bis(diphenylphosphino)ferrocene (0.14 g, 0.24 mmol), potassium acetate (64 mg, 0.66 mmol) and triethylamine (1 mL), heat to 74°C and stir for 13 hours; after the reaction is cooled to room temperature, remove the solvent under reduced pressure, separate and purify by silica gel column chromatography (petroleum ether / ethyl acetate=1:1) to obtain 2.25 g of L-84c as a yellow solid with a yield of 76%;

[0291] The phosphate derivative L-84c (2.22 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain 1.34 g of yellow solid I-84c with a yield of 65%.

[0292] Embodiment 45

[0293] The reaction formula is as follows:

[0294]

[0295] The phosphate derivative L-89a (1.59 g, 3.0 mmol) was dissolved in 20 mL of dry dichloromethane, and trimethylsilyl bromide (1.9 mL, 18 mmol) was added dropwise under argon protection, and the reaction was carried out at room temperature for 8 hours. After the reaction, dichloromethane and excess trimethylsilyl bromide were removed under reduced pressure, and the residual material was dissolved in 20 mL of methanol, stirred at room temperature for 3 hours, and methanol was removed under reduced pressure. The mixture was washed with ultrasonic water and recrystallized from methanol / diethyl ether to obtain a white solid I-89a (0.97 g, yield 68%).

[0296] Device Examples

[0297] 1. Preparation of perovskite light-emitting device precursor solution and NiOx solution

[0298] Phenethylammonium bromide (PEABr):formamidine bromide (FABr):lead bromide (PbBr2):ammonium chloride (MACl) were dissolved in a mixed solvent of DMF:DMSO with a volume ratio of 1:1 according to the molar ratio of 2:4:5:0.05, where Pb 2+ The molar concentration was 0.2 mol / L, the solution was stirred for 2 hours, allowed to stand, and filtered before use;

[0299] 0.4977 g of nickel acetate tetrahydrate was dissolved in 10 ml of anhydrous ethanol, stirred at 70° C. for half an hour, and then 120 ul of ethanolamine was added, and stirring was continued at 70° C. for 4 hours to obtain a precursor solution.

[0300] 2. Preparation of perovskite light-emitting devices by solution spin coating + vacuum evaporation process

[0301] ① First, the ITO glass was ultrasonically cleaned with alkali solution, and then ultrasonically cleaned with deionized water, acetone and isopropanol for 20 minutes in sequence, and finally dried with nitrogen; ② The ITO glass was treated with ultraviolet ozone for 30 minutes, and then the nickel oxide precursor solution was spin-coated on the ITO in an atmospheric environment (the speed was 4000 rpm, the time was 30 seconds), annealed at 350°C for 1 hour, and cooled; ③ The anhydrous ethanol solution containing the invented compound was spin-coated (the speed was 4000 rpm, the time was 30 seconds), 100 ℃ anneal for 1 hour, cool; ④ transfer to a nitrogen-protected glove box, spin-coat the perovskite precursor solution (rotation speed is 7000 rpm, anti-solvent ethyl acetate is added in the 15th second), and anneal at 85℃ for 30 minutes; ⑤ send the prepared perovskite film into the evaporation chamber, evaporate a 55nm electron transport layer TPBI and LiF (1.5nm) / Al (100nm) electrode to obtain a perovskite electroluminescent device, in which NiOx and TPBi are used as hole transport layer and electron transport layer, respectively;

[0302] The specific device structure (device structure 1) is: ITO / NiOx / phosphoric acid modification layer / perovskite active layer (~50nm) / TPBi (55nm) / LiF (1.5nm) / Al (100nm).

[0303] Embodiment 46

[0304] Taking Formula I-1a in Example 1 as the implementation object, Formula I-1a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0305] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0306] Implementation 47

[0307] Taking Formula I-1b in Example 2 as the implementation object, Formula I-1b was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0308] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0309] Embodiment 48

[0310] Taking Formula I-1c in Example 3 as the implementation object, Formula I-1c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0311] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0312] Embodiment 49

[0313] Taking Formula I-6a in Example 4 as the implementation object, Formula I-6a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0314] The device prepared in the above embodiment was tested, and the results are shown in Table 1, which provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention. Figure 4 .

[0315] Embodiment 50

[0316] Taking Formula I-6b in Example 5 as the implementation object, Formula I-6b was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0317] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0318] Embodiment 51

[0319] Taking Formula I-6c in Example 6 as the implementation object, Formula I-6c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. A perovskite electroluminescent device was prepared using the structure described in "Device Structure 1", and the obtained device was tested.

[0320] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0321] Embodiment 52

[0322] Taking Formula I-6d in Example 7 as the implementation object, Formula I-6d was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. A perovskite electroluminescent device was prepared using the structure described in "Device Structure 1", and the obtained device was tested.

[0323] See Table 1, which provides performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0324] Embodiment 53

[0325] Formula I-7a in Example 8 was used as an implementation object, and Formula I-7a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml, and was spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer. The nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. The perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0326] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0327] Embodiment 54

[0328] Taking Formula I-7b in Example 9 as the implementation object, Formula I-7b was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0329] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0330] Embodiment 55

[0331] Formula I-7c in Example 10 was used as an implementation object, and Formula I-7c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml, and was spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer. The nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. The perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0332] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0333] Embodiment 56

[0334] Formula I-7d in Example 11 was used as an implementation object, and Formula I-7d was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml, and was spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer. The nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. The perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0335] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0336] Embodiment 57

[0337] Formula I-8a in Example 12 was used as an implementation object, and Formula I-8a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml, and was spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer. The nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. The perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0338] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0339] Embodiment 58

[0340] Taking Formula I-8b in Example 13 as the implementation object, Formula I-8b was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0341] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0342] Embodiment 59

[0343] Taking Formula I-8c in Example 14 as the implementation object, Formula I-8c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0344] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0345] Embodiment 60

[0346] Formula I-13a in Example 15 was used as an implementation object, and Formula I-13a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml, and was spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer. The nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. The perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0347] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0348] Embodiment 61

[0349] Formula I-13c in Example 16 was used as an implementation object, and Formula I-13c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml, and was spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer. The nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process. The perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0350] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0351] Embodiment 62

[0352] Taking Formula I-15a in Example 17 as the implementation object, Formula I-15a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0353] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0354] Embodiment 63

[0355] Taking Formula I-15c in Example 18 as the implementation object, Formula I-15c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0356] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0357] Embodiment 64

[0358] Taking Formula I-29a in Example 19 as the implementation object, Formula I-29a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0359] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0360] Embodiment 65

[0361] Taking Formula I-29c in Example 20 as the implementation object, Formula I-29c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0362] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0363] Embodiment 66

[0364] Taking Formula I-30a in Example 21 as the implementation object, Formula I-30a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0365] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0366] Embodiment 67

[0367] Taking Formula I-30c in Example 22 as the implementation object, Formula I-30c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0368] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0369] Embodiment 68

[0370] Taking Formula I-39a in Example 23 as the implementation object, Formula I-39a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0371] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0372] Embodiment 69

[0373] Taking Formula I-39c in Example 24 as the implementation object, Formula I-39c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0374] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0375] Embodiment 70

[0376] Formula I-51a in Example 25 was used as an implementation object. Formula I-51a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by solution spin coating, and the organic electron transport layer was prepared by vacuum evaporation.

[0377] Preparation, using the structure described in "Device Structure 1" to prepare a perovskite electroluminescent device.

[0378] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0379] Embodiment 71

[0380] Taking Formula I-51c in Example 26 as the implementation object, Formula I-51c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0381] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0382] Embodiment 72

[0383] Taking Formula I-63a in Example 27 as the implementation object, Formula I-63a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0384] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0385] Embodiment 73

[0386] Taking Formula I-63c in Example 28 as the implementation object, Formula I-63c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0387] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0388] Embodiment 74

[0389] Taking Formula I-75a in Example 29 as the implementation object, Formula I-75a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0390] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0391] Embodiment 75

[0392] Taking Formula I-75c in Example 30 as the implementation object, Formula I-75c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0393] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0394] Embodiment 76

[0395] Taking Formula I-76a in Example 31 as the implementation object, Formula I-76a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0396] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0397] Embodiment 77

[0398] Taking Formula I-76c in Example 32 as the implementation object, Formula I-76c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0399] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0400] Embodiment 78

[0401] Taking Formula I-77a in Example 33 as the implementation object, Formula I-77a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0402] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0403] Embodiment 79

[0404] Taking Formula I-77c in Example 34 as the implementation object, Formula I-77c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0405] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0406] Embodiment 80

[0407] Taking Formula I-79a in Example 35 as the implementation object, Formula I-79a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0408] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0409] Embodiment 81

[0410] Taking Formula I-79c in Example 36 as the implementation object, Formula I-79c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0411] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0412] Embodiment 82

[0413] Taking Formula I-80a in Example 37 as the implementation object, Formula I-80a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0414] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0415] Embodiment 83

[0416] Formula I-80c in Example 38 was used as an implementation object. Formula I-80c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite luminescent layer.

[0417] Between the layers; the nickel oxide hole transport layer is prepared by a solution spin coating process, the organic electron transport layer is prepared by a vacuum evaporation process, and the perovskite electroluminescent device is prepared using the structure described in "Device Structure 1".

[0418] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0419] Embodiment 84

[0420] Taking Formula I-81a in Example 39 as the implementation object, Formula I-81a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0421] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0422] Embodiment 85

[0423] Taking Formula I-81c in Example 40 as the implementation object, Formula I-81c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0424] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0425] Embodiment 86

[0426] Taking Formula I-83a in Example 41 as the implementation object, Formula I-83a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0427] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0428] Embodiment 87

[0429] Taking Formula I-83c in Example 42 as the implementation object, Formula I-83c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0430] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0431] Embodiment 88

[0432] Taking Formula I-84a in Example 43 as the implementation object, Formula I-84a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0433] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0434] Embodiment 89

[0435] Taking Formula I-84c in Example 44 as the implementation object, Formula I-84c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0436] The devices prepared in the above embodiments were tested, and the results are shown in Table 1. Table 1 provides the devices prepared in the embodiments of the present invention.

[0437] Performance parameters of perovskite electroluminescent devices.

[0438] Embodiment 90

[0439] Taking Formula I-89a in Example 45 as the implementation object, Formula I-89a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on the nickel oxide layer as an interface modification layer, located between the NiOx hole transport layer and the perovskite light-emitting layer; the nickel oxide hole transport layer was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite electroluminescent device was prepared using the structure described in "Device Structure 1".

[0440] The device prepared in the above embodiment was tested, and the results are shown in Table 1. Table 1 provides the performance parameters of the perovskite electroluminescent device prepared in the embodiment of the present invention.

[0441] Comparative Example 1

[0442] The perovskite device without the phosphate compound of the present invention as the interface modification layer was used as the implementation object, the perovskite active layer was directly spin-coated on the hole transport layer NiOx, and the organic electron transport layer was prepared by vacuum evaporation process. The device structure was ITO / NiOx / EML (~50nm) / TPBi (55nm) / LiF (1.5nm) / Al (100nm), and the obtained light-emitting device was tested; the performance parameters are shown in Table 1;

[0443] Table 1 Performance parameters of the light emitting devices provided in the embodiments of the present invention and the comparative examples

[0444]

[0445]

[0446] Note: The start voltage in the table is for a brightness of 1cd m -2 The driving voltage of the device.

[0447] 3. Preparation of precursor solution for perovskite battery devices

[0448] Preparation of PTAA precursor solution: Dissolve 1.5 mg of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) in 1 mL of toluene, shake, and use after dissolution;

[0449] Preparation of FAPbI3 precursor solution: iodoformamidine (FAI), lead iodide (PbI2), and chloromethylamine (MACl) were dissolved in a mixed solvent of N-N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) with a volume ratio of 8:1 at a molar ratio of 1:1:0.15. 2+ The molar concentration was 1.4 mol / L. The solution was stirred for 8 hours, allowed to stand, and filtered before use.

[0450] 4. Preparation of perovskite light-emitting devices by solution spin coating + vacuum evaporation process

[0451] The indium-doped tin oxide (ITO) patterned glass substrate was cleaned and ultrasonically treated in an ultrasonic bath with deionized water, acetone, and isopropanol for 30 minutes, respectively. After the ITO glass was treated with UV ozone for 30 minutes, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) dissolved in toluene solvent at a mass concentration of 1.5 mg / mL was spin-coated on the indium tin oxide supported on the glass substrate at a speed of 2000 rpm in an air atmosphere, and annealed at 100° C. for 10 minutes. Subsequently, an anhydrous ethanol solution containing the compound of the invention was spin-coated at a speed of 4000 rpm (time for 30 seconds), and annealed at 100° C. for 1 hour. Then, the perovskite layer was spin-coated at a speed of 5000 rpm in a nitrogen atmosphere. At the 10th second of the spin coating of the perovskite precursor solution, the anti-solvent ethyl acetate (EA) was added dropwise, and the solution was annealed at 150° C. for 15 minutes. Then, the substrate was transferred to a 5×10 -4 Pa, 25nm C60, 10nm bathocuproin (BCP), and 100nm silver (Ag) electrodes were deposited in sequence to obtain a perovskite battery device; PTAA, C60, and BCP were the hole transport layer, electron transport layer, and cathode buffer layer, respectively;

[0452] The specific device structure (device structure 2) is: ITO / PTAA / phosphoric acid modification layer / perovskite active layer (~50nm) / C60 (25nm) / BCP (10nm) / Ag (100nm).

[0453] Embodiment 91

[0454] Taking Formula I-1a in Example 1 as the implementation object, Formula I-1a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0455] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0456] Implementation 92

[0457] Taking Formula I-1b in Example 2 as the implementation object, Formula I-1b was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0458] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0459] Embodiment 93

[0460] Taking Formula I-1c in Example 3 as the implementation object, Formula I-1c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0461] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0462] Embodiment 94

[0463] Taking Formula I-6a in Example 4 as the implementation object, Formula I-6a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0464] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0465] Embodiment 95

[0466] Taking Formula I-6b in Example 5 as the implementation object, Formula I-6b was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0467] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0468] Embodiment 96

[0469] Taking Formula I-6c in Example 6 as the implementation object, Formula I-6c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0470] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0471] Embodiment 97

[0472] Taking Formula I-6d in Example 7 as the implementation object, Formula I-6d was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0473] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0474] Embodiment 98

[0475] Formula I-7a in Example 8 was used as an implementation object. Formula I-7a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by solution spin coating, and the organic electron transport layer was prepared by vacuum evaporation.

[0476] The structure described in “Device Structure 2” is used to prepare a perovskite battery device.

[0477] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0478] Embodiment 99

[0479] Taking Formula I-7b in Example 9 as the implementation object, Formula I-7b was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0480] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0481] Embodiment 100

[0482] Taking Formula I-7c in Example 10 as the implementation object, Formula I-7c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0483] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0484] Embodiment 101

[0485] Taking Formula I-7d in Example 11 as the implementation object, Formula I-7d was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0486] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0487] Embodiment 102

[0488] Taking Formula I-8a in Example 12 as the implementation object, Formula I-8a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0489] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0490] Embodiment 103

[0491] Taking Formula I-8b in Example 13 as the implementation object, Formula I-8b was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0492] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0493] Embodiment 104

[0494] Taking Formula I-8c in Example 14 as the implementation object, Formula I-8c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0495] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0496] Embodiment 105

[0497] Taking Formula I-13a in Example 15 as the implementation object, Formula I-13a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0498] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0499] Embodiment 106

[0500] Taking Formula I-13c in Example 16 as the implementation object, Formula I-13c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0501] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0502] Embodiment 107

[0503] Taking Formula I-15a in Example 17 as the implementation object, Formula I-15a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0504] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0505] Embodiment 108

[0506] Taking Formula I-15c in Example 18 as the implementation object, Formula I-15c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0507] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0508] Embodiment 109

[0509] Taking Formula I-29a in Example 19 as the implementation object, Formula I-29a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0510] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0511] Embodiment 110

[0512] Taking Formula I-29c in Example 20 as the implementation object, Formula I-29c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0513] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0514] Embodiment 111

[0515] Formula I-30a in Example 21 was used as an implementation object. Formula I-30a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer.

[0516] Between; the hole transport layer PTAA is prepared by a solution spin coating process, the organic electron transport layer is prepared by a vacuum evaporation process, and the perovskite battery device is prepared using the structure described in "Device Structure 2".

[0517] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0518] Embodiment 112

[0519] Taking Formula I-30c in Example 22 as the implementation object, Formula I-30c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0520] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0521] Embodiment 113

[0522] Taking Formula I-39a in Example 23 as the implementation object, Formula I-39a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0523] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0524] Embodiment 114

[0525] Taking Formula I-39c in Example 24 as the implementation object, Formula I-39c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0526] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0527] Embodiment 115

[0528] Taking Formula I-51a in Example 25 as the implementation object, Formula I-51a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0529] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0530] Embodiment 116

[0531] Taking Formula I-51c in Example 26 as the implementation object, Formula I-51c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0532] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0533] Embodiment 117

[0534] Taking Formula I-63a in Example 27 as the implementation object, Formula I-63a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0535] The devices prepared in the above embodiments were tested, and the results are shown in Table 2. Table 2 provides the devices prepared in the embodiments of the present invention.

[0536] Performance parameters of perovskite cell devices.

[0537] Embodiment 118

[0538] Taking Formula I-63c in Example 28 as the implementation object, Formula I-63c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0539] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0540] Embodiment 119

[0541] Taking Formula I-75a in Example 29 as the implementation object, Formula I-75a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0542] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0543] Embodiment 120

[0544] Taking Formula I-75c in Example 30 as the implementation object, Formula I-75c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0545] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0546] Embodiment 121

[0547] Taking Formula I-76a in Example 31 as the implementation object, Formula I-76a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0548] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0549] Embodiment 122

[0550] Taking Formula I-76c in Example 32 as the implementation object, Formula I-76c was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0551] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0552] Embodiment 123

[0553] Taking Formula I-77a in Example 33 as the implementation object, Formula I-77a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0554] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0555] Embodiment 124

[0556] Formula I-77c in Example 34 was used as the implementation object, and Formula I-77c was dissolved in an aqueous solution at a concentration of 1.0 mg / ml.

[0557] In water and ethanol, it is spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA is prepared by a solution spin coating process, and the organic electron transport layer is prepared by a vacuum evaporation process, and the perovskite battery device is prepared using the structure described in "Device Structure 2".

[0558] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0559] Embodiment 125

[0560] Taking Formula I-79a in Example 35 as the implementation object, Formula I-79a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0561] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0562] Embodiment 126

[0563] Taking Formula I-79c in Example 36 as the implementation object, Formula I-79c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0564] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0565] Embodiment 127

[0566] Taking Formula I-80a in Example 37 as the implementation object, Formula I-80a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0567] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0568] Embodiment 128

[0569] Taking Formula I-80c in Example 38 as the implementation object, Formula I-80c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0570] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0571] Embodiment 129

[0572] Taking Formula I-81a in Example 39 as the implementation object, Formula I-81a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0573] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0574] Embodiment 130

[0575] Taking Formula I-81c in Example 40 as the implementation object, Formula I-81c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0576] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0577] Embodiment 131

[0578] Taking Formula I-83a in Example 41 as the implementation object, Formula I-83a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0579] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0580] Embodiment 132

[0581] Taking Formula I-83c in Example 42 as the implementation object, Formula I-83c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0582] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0583] Embodiment 133

[0584] Taking Formula I-84a in Example 43 as the implementation object, Formula I-84a was dissolved in anhydrous ethanol at a concentration of 1.0 mg per milliliter, and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0585] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0586] Embodiment 134

[0587] Taking Formula I-84c in Example 44 as the implementation object, Formula I-84c was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0588] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0589] Embodiment 135

[0590] Taking Formula I-89a in Example 45 as the implementation object, Formula I-89a was dissolved in anhydrous ethanol at a concentration of 1.0 mg / ml and spin-coated on PTAA as an interface modification layer, located between the hole transport layer PTAA and the perovskite active layer; the hole transport layer PTAA was prepared by a solution spin coating process, and the organic electron transport layer was prepared by a vacuum evaporation process, and the perovskite battery device was prepared using the structure described in "Device Structure 2".

[0591] The device prepared in the above embodiment was tested, and the results are shown in Table 2. Table 2 provides the performance parameters of the perovskite battery device prepared in the embodiment of the present invention.

[0592] Comparative Example 2

[0593] Taking the battery device without adding the interface modification layer as the implementation object, the perovskite film is directly spin-coated on the organic hole transport layer PTAA, the PTAA is prepared by solution spin coating process, and the organic electron transport layer is prepared by vacuum evaporation process. The device structure is ITO / PTAA / perovskite active layer (~50nm) / C60 (25nm) / BCP (10nm) / Ag (100nm), and the photoelectric conversion performance of the obtained device is tested; the specific performance parameters are shown in Table 2;

[0594] Table 2 Performance parameter data of battery devices provided by the embodiments of the present invention and comparative examples

[0595]

[0596]

[0597]

[0598] As can be seen from Table 1, compared with the device without the phosphoric acid compound interface modification layer (Comparative Example 1), the perovskite electroluminescent device prepared by the compound containing the phosphonic acid group provided by the present invention generally has a high device efficiency, and the peak value of the electroluminescent spectrum is almost unchanged (less than 2nm), and the change in the luminescent properties of the device can be ignored; by reasonably selecting the substituent to improve the defect passivation effect of the phosphorus oxygen group, the appropriate alkyl chain length is conducive to regulating the self-assembly behavior between molecules, improving the film quality and improving the charge transfer ability, and achieving a perovskite electroluminescent device with a maximum external quantum efficiency of 7.23% (see Figure 5 ).

[0599] As can be seen from Table 2, compared with the device without the phosphoric acid compound interface modification layer (Comparative Example 2), the efficiency of the perovskite battery device prepared by the compound containing the phosphonic acid group provided by the present invention is significantly improved; through the regulation of the substituent and the alkyl chain, the problem of poor wettability of the hole transport layer is effectively improved, the formation of defects is reduced, and thus better carrier transport performance is obtained, so that the photoelectric conversion efficiency is increased to 16.74% (see Figure 5 ).

[0600] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0601] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A compound containing a phosphate group having one of the structures shown below: In the above structure, the value of n is an integer of 2 to 4.

2. Use of the compound containing a phosphate group according to claim 1 as an interface modification layer material or additive.

3. A perovskite light-emitting device, comprising an anode, a cathode, and a carrier transport layer, an interface modification layer and a perovskite light-emitting layer located between the anode and the cathode, characterized in that: The interface modification material of the interface modification layer comprises the compound containing a phosphate group according to claim 1.

4. A perovskite solar cell device, comprising an anode, a cathode, and a carrier transport layer, an interface modification layer and a perovskite photoactive layer located between the anode and the cathode, characterized in that: The interface modification material of the interface modification layer comprises the compound containing a phosphate group according to claim 1.