A GH4169 high temperature alloy and its smelting process
Through vacuum induction smelting technology and multiple refining and electromagnetic stirring control, combined with the use of magnesium-magnesium alloy, the problems of low utilization efficiency and safety hazards of return materials during smelting of high-temperature alloy GH4169 are solved, and efficient and low-cost GH4169 alloy production is achieved. Improve product quality and lining life.
Patent Information
- Application Number
- CN202310072102.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-31
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-01-31
AI Technical Summary
The existing high-temperature alloy GH4169 smelting process is costly and difficult to fully utilize the return material, resulting in low recycling efficiency of GH4169 alloy, inclusion and oxide contamination, risk of furnace lining drilling steel and safety hazards.
Using vacuum induction smelting technology, through multiple refining and electromagnetic stirring control, combined with the use of magnesium-magnesium alloy, the precise control of the composition and temperature of the steel is achieved, the nitrogen content is reduced, and the raw material ratio is adjusted through pretreatment and multiple sampling, which improves the Return material utilization and product quality.
It realizes efficient recycling and utilization of high-temperature alloy GH4169, reduces production costs, improves product quality, reduces inclusions and oxide content, extends the service life of the furnace lining, and reduces safety risks.
Smart Images

Figure CN116043068B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of steel smelting, and in particular to a GH4169 high-temperature alloy and a smelting process thereof. Background Art
[0002] The high-temperature alloy GH4169 has excellent yield strength below 650°C, and has good oxidation resistance, fatigue resistance, creep resistance, processing performance and welding performance. It can be used for a long time under 650°C working conditions. Therefore, GH4169 alloy is widely used in aerospace, nuclear power and petrochemical industries. It is one of the most widely used and largest-volume steel grades in high-temperature alloy products.
[0003] In the production, processing and use of high-temperature alloy GH4169, various GH4169 return materials are inevitably generated every year. If not utilized, it will cause the loss and waste of precious metals such as Ni, Cr, Mo, Nb in GH4169 alloy. In this regard, the current conventional practice of domestic manufacturers is to recycle the return materials, mainly for the smelting of GH4169 alloy. In order to prevent impurity elements, oxide scale, slag inclusions, etc. in the return materials from entering the molten steel and causing excessive pollution, the current domestic manufacturers usually control the proportion of return materials to be less than 60% when smelting high-temperature alloy GH4169 containing return materials to obtain qualified product performance.
[0004] Since the recycling rate of high-temperature alloy GH4169 return materials in the industrial production process has not kept up with the production rate of return materials, it is difficult to achieve efficient and timely recycling and utilization of GH4169 alloy return materials. Chinese patent document CN114369736A "A high-temperature alloy and smelting process for increasing the utilization ratio of return materials" has a final return material addition ratio of 40% to 60%. The process in this patent includes the following 6 control steps: return material melting period, return material heating period, inclusion denaturation and removal period, new material addition period, oxidizable element addition period and casting period. The patent introduces the process control process, but does not clearly specify the corresponding steel grade composition (different steel grades will have different compositions, and different compositions will have different characteristics, including melting points). It is not appropriate to talk about specific process parameters without considering the composition.
[0005] In addition, the patent still has the following disadvantages:
[0006] 1. One of the purposes of the patent is to achieve a 40% to 60% return material ratio in the vacuum induction melting of high-temperature alloys, while not affecting the quality of ingots or castings. However, there are many sources of high-temperature alloy return materials, involving complex working conditions. Before recycling and melting, the return materials must be inspected and processed, but the patent does not mention this aspect, that is, the process of the patent fails to achieve effective control of the state of the return materials, and there is a risk that each furnace will bring different amounts of refractory inclusions and oil stains into the molten steel due to the addition of return materials, resulting in inconsistent experimental conditions in each comparative example. The input end cannot achieve effective control, and the rigor of the data obtained at the output end is problematic and not convincing.
[0007] 2. This patent uses high power to melt the returned material after it turns completely red. However, the temperature at which the charge turns red is only about 600°C, which makes it difficult to fully and effectively preheat the lining. In addition, the cracks on the lining in this patent have not been well healed, greatly increasing the risk of the lining drilling into the steel during the smelting process. At the same time, this patent uses a high power of nearly 1000kW to heat and melt the charge. The greater the power, the faster the charge melts, which means that the effective degassing time during the melting period is shorter. Many gases remain in the molten steel because they cannot be overflowed in time, which brings great difficulties to the later deep deoxidation.
[0008] 3. The patent believes that raising the temperature of the return molten steel to 1650-1700°C can destroy the stability of carbonitrides and convert them into atomic state, while nitrogen atoms are discharged in the form of nitrogen gas under vacuum conditions, thereby achieving the removal of carbonitrides. However, referring to the relationship between the solid solubility of nitrogen in iron and temperature, it can be seen that as the temperature of the molten steel increases, the solubility of the gas in the molten steel increases, and when the temperature of the molten steel rises from 1600°C to 1750°C, the solubility of nitrogen in the molten steel increases sharply, and the solubility of nitrogen in the molten steel (measured in mass percentage) increases from about 0.013wt% to 0.044wt%. Therefore, refining at this temperature cannot achieve the effect of denitrification of the molten steel. In addition, because the melting point of most high-temperature alloys is in the range of 1300-1450℃, and the comparative documents raise the return molten steel to a high temperature of 1650-1700℃, the superheat of the molten steel reaches 200-400℃, which will cause many negative effects: such as higher smelting energy consumption and increased steelmaking costs; the reaction between the crucible material and the active elements in the molten steel will be more intense, and while the crucible will be corroded and its service life will be shortened, it will also cause oxygenation in the molten steel; the fluidity of the molten steel will be greatly enhanced. If there are cracks in the crucible that have not been healed in the early stage, it is extremely easy to cause the crucible to drill into the steel or leak steel, and even cause personal safety accidents.
[0009] 4. This patent directly adds the remaining stable elements and carbon elements in the new material to the returned molten steel. Because the melting chamber of the vacuum induction melting furnace is in a vacuum-sealed state, the material needs to be added under vacuum. A large amount of solid furnace charge (especially the furnace with large tonnage) is directly added to the molten steel. As the charge enters the molten steel, there is also a large amount of water vapor adsorbed on the surface of the solid furnace charge. Therefore, in addition to the splashing caused by the solid furnace charge falling into the molten steel, there is also the water vapor that instantly enters the molten steel, causing serious splashing of the molten steel. In addition, the carbon element is added at this time, and it reacts violently with the gas in the molten steel. These problems occur at the same time, and in a vacuum environment, it is easy to cause the molten steel to boil, that is, under the condition of evacuation, the suction force on the surface of the molten steel will cause a large amount of molten steel to rise along the churning bubbles, and finally overflow the crucible and damage the equipment. This phenomenon is like boiling porridge overflowing from the lid. Therefore, in this operation link, not only will the gas adsorbed on the surface of the solid charge enter the molten steel (because after the solid charge is added, it is instantly submerged in the molten steel, and the gas adsorbed on the surface does not have time to be baked and extracted), but it will also cause serious splashing of the molten steel, and even cause the molten steel to boil violently, causing safety accidents. Because the refractory lining is wrapped from the outside by the copper energized water-cooling coil, because the temperature of the molten steel is 1650-1700℃ at this time, and the melting point of the copper coil is only 1083℃, if the crucible overflows with molten steel, it is likely to damage the coil. The cooling water sprayed from the damaged coil will instantly vaporize when it encounters the high-temperature molten steel, and the volume will instantly increase by 1600 times. And because it is in a closed chamber, when the pressure in the chamber exceeds its equipment limit, the equipment will be blown up, that is, an explosion will occur. Summary of the invention
[0010] Therefore, the technical problem to be solved by the present invention is that the existing high-temperature alloy GH4169 smelting process has the defects of high cost and inability to fully utilize the returned materials, thereby providing a GH4169 high-temperature alloy and a smelting process thereof.
[0011] To this end, the present invention adopts the following technical solutions:
[0012] The present invention provides a GH4169 high temperature alloy, the raw materials of which include return material, carbon particles, industrial pure iron, electrolytic nickel, metal chromium, molybdenum, niobium, and nickel-magnesium alloy;
[0013] In terms of mass percentage, the returned material accounts for 70-98% of the total raw materials;
[0014] The returned materials include GH4169 high temperature alloy returned materials and / or other steel grades with similar compositions, wherein the other steel grades with similar compositions include GH3039 alloy and GH4080A alloy;
[0015] The mass percentage of oxygen in the GH4169 alloy is not higher than 10×10 -6 %.
[0016] Furthermore, the chemical composition of the GH4169 high-temperature alloy, measured in mass percentage, includes: C≤0.08%, Si≤0.35%, Mn≤0.35%, Ni 50.0-55.0%, Cr 17.0-21.0%, Fe15.0-21.0%, Al 0.2-0.8%, Ti 0.65-1.15%, Mo 2.8-3.3%, Nb 4.75-5.5%, Mg 0.003-0.009%, Cu≤0.3%, B≤0.006%, Co≤0.3%, S≤0.002%, P≤0.005%, O≤0.001%, N≤0.004%, and the rest are unavoidable impurities.
[0017] The present invention also provides a smelting process of the above-mentioned GH4169 high temperature alloy, which adopts a vacuum induction smelting process and includes the following steps:
[0018] S1: first feeding and preheating;
[0019] S2: heating until the charge is melted, adding niobium and heating until the charge is melted again (the purpose of adding metallic niobium after the charge is melted is to remove nitrogen in the molten steel as much as possible, to prevent metallic niobium from being added too early and nitrogen from being completely removed, and niobium and nitrogen combining to form niobium nitride, resulting in incomplete removal of nitrogen in the molten steel);
[0020] S3: first refining;
[0021] S4: second refining;
[0022] S5: third refining;
[0023] S6: Adding nickel-magnesium alloy with argon filling (to make inclusions fully float up, so as to achieve the purpose of reducing inclusions in molten steel. Adding nickel-magnesium alloy under protective atmosphere is beneficial to reducing magnesium burning loss; and the addition of magnesium is beneficial to further deoxidation of molten steel, and the trace magnesium element contained in steel is helpful to improve subsequent hot working performance);
[0024] S7: heating and casting to obtain the GH4169 alloy;
[0025] Wherein, electromagnetic stirring is also included after steps S2, S3, S4 and S6;
[0026] The first refining includes the first sampling at the beginning, the second refining includes the second sampling at the beginning, and the third refining includes the third sampling at the end. The third sampling is carried out just before casting. The operation after taking this furnace sample is to adjust the steel temperature and cast. The composition of the furnace sample will be used as the composition data of the cast ingot to determine whether the composition of the ingot meets the process requirements.
[0027] Furthermore, after the first sampling result comes out, the content of each element is compared with the control range and target value of the element. When the amount of a certain element is insufficient, the amount of the element to be added is calculated, and the second addition is performed. The calculation formula is: the weight of the element to be added = [(theoretical total weight of the furnace * target content value of the element) - (real-time molten steel weight * component value of the element analyzed in the furnace)] / (element yield * metal purity); after the second addition, the power is turned off and the film is formed for 5 to 10 minutes, and the second addition is heated to melt it;
[0028] After the second sampling results come out, compare the content of each element with the control range and target value of the element. When the amount of a certain element is lacking, calculate the amount of the element to be added, and carry out the third addition. The calculation formula is: the weight of the element to be added = [(theoretical total weight of the furnace * target content value of the element) - (real-time weight of molten steel * component value of the element analyzed in the furnace)] / (element recovery rate * metal purity). Heat to melt the third addition.
[0029] In step S1, the first feeding is to place 5-15wt% of the return material flat on the bottom of the crucible, then add carbon particles, electrolytic nickel, industrial pure iron, chromium and molybdenum, and finally add the return material to the slag line of the crucible;
[0030] The remaining return material is added when the material added in step S2 is completely melted;
[0031] The preheating in step S1 is to adjust the power of the smelting chamber to 200 kW and preheat for 0.5 to 1 hour when the vacuum value of the smelting chamber is ≤10 Pa.
[0032] In step S2, before heating and melting, the power supply is increased to 300 kW, heated for 1 to 1.5 hours, the power is reduced to 240 to 280 kW, and the temperature is kept for 30 to 40 minutes;
[0033] The power transmitted during the heating and melting in step S2 is 500 to 800 kW.
[0034] The electromagnetic stirring is three-phase electromagnetic stirring, with a voltage of 110-130V, a current of 5500-7500A, and a stirring time of 2-5min;
[0035] The first refining time is 30 to 50 minutes, and the refining temperature is 1480±20°C;
[0036] The second refining time is 20 to 30 minutes, and the refining temperature is 1480±20°C;
[0037] The third refining time is 10 to 20 minutes, and the refining temperature is 1480±20°C.
[0038] In step S6, the smelting chamber is filled with argon to 25000-30000 Pa, and the nickel-magnesium alloy is added and stirred for 2-5 minutes, and then allowed to stand for 3-5 minutes at a power supply of 240-280 kW.
[0039] In step S7, the tapping temperature is 1520±20°C, the power supply is 300-400kW, and the casting speed is 300-400kg / min.
[0040] Preferably, the step S1 further includes pretreatment of the returned material, wherein the pretreatment is to first control the size of the returned material: the side length or diameter of the cross section of the returned material is ≤150mm, and the length is ≤300mm. If it exceeds this range, it should be sawed to ensure that the furnace loading or barrel loading is not affected; secondly, the surface quality of the returned material is visually inspected. If the surface of the returned material is obviously oily, or if the finger is touched and a distance of 30 to 50mm is drawn on the surface of the returned material, if obvious black oil stains are adhered to the touched surface of the finger, it means that there is too much oil stain on the surface of the returned material. It is recommended to use acid washing + alkali washing + water washing + baking + shot blasting to remove the surface oil and rust. If there is only a small amount or no oil stain, baking + shot blasting can be used to remove it. It is ensured that the harmful substances involved in the surface of the returned material are fully removed before use.
[0041] The technical solution of the present invention has the following advantages:
[0042] (1) In the early stage of material processing, the smelting process of the present invention adopts a control process of increasing the power to 300 kW, heating for 1 to 1.5 hours, reducing the power to a heat preservation power of 240 to 280 kW, and keeping warm for 30 to 40 minutes. This can effectively bridge the cracks in the furnace lining, reduce the drilling of the furnace lining during smelting, and increase the service life of the furnace lining.
[0043] (2) Through the process control in the smelting process of the present invention:
[0044] When nitrogen combines with niobium, it will generate niobium nitride with stable performance, which is not conducive to the denitrification of molten steel. In this smelting process, the nitrogen in the molten steel is removed as much as possible by using the operation of smelting and vacuuming until the molten steel is melted and clear, and then adding metallic niobium can greatly reduce the probability of nitrogen in the molten steel combining with niobium;
[0045] The three-phase electromagnetic stirring at four different melting stages, with the electromagnetic stirring voltage controlled at 110-130V, the current at 5500-7500A, and the stirring time at 2-5min, can effectively achieve the homogenization of the composition and temperature of the molten steel. Then, three times of in-furnace sampling and analysis and multiple molten steel temperature monitoring operations are used to finally achieve precise control of the composition and temperature of the molten steel. In addition, the stirring control under this parameter plays a key role in the floating of inclusions and gases in the molten steel.
[0046] The high vacuum refining in three different melting stages, at a temperature of 1480±20℃, lasted for 30-50min, 20-30min and 10-20min respectively, made the inclusions in the molten steel float further. At the same time, the melting chamber was continuously evacuated during the refining period to further remove harmful elements and gases in the molten steel, achieving the purpose of deep inclusion removal and deoxidation, thus producing high-quality GH4169 alloy ingots with low oxygen content and inclusions, of which the mass percentage of oxygen can reach 10×10 -6 %the following.
[0047] (3) The smelting control process of the present invention can use a vacuum induction melting furnace to melt the high-temperature alloy GH4169 with a return material ratio of up to 70-98%, which is much higher than the current industry level of only less than 60wt% return material ratio, and plays a great role in reducing costs and increasing efficiency of enterprises in the smelting process. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0049] Figure 1 It is a graph of power and time in the smelting process of the present invention. DETAILED DESCRIPTION
[0050] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0051] If no specific experimental steps or conditions are specified, the conventional experimental steps or conditions described in the literature in this field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be purchased commercially.
[0052] The returned materials include the cut ends and scraps of GH3039, GH4080A and GH4169 high temperature alloys, and the relevant components are as follows:
[0053] GH3039 high temperature alloy return material composition: (unit: wt%)
[0054] element C Si Cr Ni Al Ti Mo content 0.03 0.21 19.8 74.07 0.42 0.51 1.86 element Nb Fe Mn Cu O content 1.05 1.62 0.21 0.2 0.0027
[0055] GH4080A high temperature alloy return material composition: (unit: wt%)
[0056] element C Si Mn Cr Fe Mo Cu content 0.061 0.074 0.0005 19.26 0.26 0.008 0.009 element Co Nb Al Ti Ni O content 0.62 0.042 1.13 2.72 75.8 0.0042
[0057] GH4169 high temperature alloy return material composition: (unit: wt%)
[0058] element C Si Mn Ni Cr Fe Mo content 0.041 0.42 0.34 54.35 15.49 22.57 2.80 element Nb Al Ti Co Cu O content 3.01 0.19 0.51 0.16 0.07 0.0035
[0059] The remaining components are unavoidable impurities, and the composition of the alloy return material will fluctuate slightly.
[0060] The dimensions and surface quality control standards and methods of the returned materials: the side length or diameter of the cross section of the returned materials is ≤150mm, and the length is ≤300mm. If it exceeds this range, it should be cut and sawed to ensure that the loading into the furnace or barrel is not affected; secondly, the surface quality of the returned materials is visually inspected. If the surface of the returned materials is obviously oily, or if you touch the surface of the returned materials with your fingers, and scratch the surface of the returned materials for 30 to 50mm, if the surface of the touched fingers is obviously adhered to black oil stains, it means that there is too much oil on the surface of the returned materials. In this case, acid washing + alkali washing + water washing + baking + shot blasting are used to remove the surface oil and rust. If there is only a small amount or no oil, baking + shot blasting can be used to remove it. Ensure that the harmful substances on the surface of the returned materials are fully removed before use.
[0061] Example 1
[0062] This embodiment provides a specific vacuum induction melting process of GH4169 high temperature alloy containing a high return material addition ratio, including process steps and key control parameters. The relationship between power and time in the melting process of the present invention is as follows: Figure 1 As shown, the details are as follows:
[0063] The present embodiment aims to obtain a GH4169 high temperature alloy having the composition shown in the following table (unit: wt%):
[0064] element C Si Mn Ni Cr Mo Nb Fe content 0.03 0.09 0.07 53 18.5 3.0 5.3 18.0 element Co Cu Mg O B Al Ti content 0.2 0.04 0.007 ≤0.001 0.003 0.72 1.0
[0065] 1) After the return material is processed, the first feeding is carried out, with a total of 3922kg of return material (including 237kg of GH3039 alloy return material, 3185kg of GH4169 alloy return material, and 500kg of GH4080A alloy return material). After 10wt% of the return material is laid flat on the bottom of the crucible, 0.17kg of carbon particles, 116.38kg of electrolytic nickel, 203.85kg of industrial pure iron, 131.42kg of chromium and 36.98kg of molybdenum are added successively, and finally the return material is added to the crucible slag line position. When the vacuum value of the smelting chamber is ≤10Pa, the crucible is powered, first 200kW, for 0.5h, mainly to preheat the refractory crucible and the charge in the crucible, and at the same time, the smelting chamber is evacuated by the evacuation system to remove the gas attached to the surface of the crucible and the charge.
[0066] 2) Increase the power to 300kW for 1 hour. When the color of the lower half of the charge in the crucible turns white from the observation window, reduce the power to 250kW for 30 minutes. This is mainly to ensure that the cracks on the refractory lining have a high enough temperature and long enough time to heal.
[0067] 3) After the insulation is finished, the power is increased to 500kW, and the charge in the crucible begins to melt. As the amount of molten steel in the crucible gradually increases, the power supply is gradually increased to 700kW. If there is any return material that has not been fully added to the crucible, at this time, as the melting of the material proceeds, the remaining return material is added to the crucible from the feeding bin under vacuum through a feeding bucket in a timely manner. This process is repeated until all the return material has been added and melted.
[0068] 4) After melting, 72.29 kg of metallic niobium was added into the crucible using the above-mentioned feeding method. After the molten steel was melted again, the steel temperature was adjusted to 1500° C., the medium frequency melting power was turned off, and the three-phase electromagnetic stirring was started. The voltage during electromagnetic stirring was set to 115 V, the current was set to 6500 A, and the stirring time was set to 5 min. The powerful stirring force of the three-phase electromagnetic stirring function was used to homogenize the temperature and composition of the molten steel in the crucible, and to promote the discharge of gas in the molten steel and the floating and removal of inclusions.
[0069] 5) After stirring is completed, switch back to the medium frequency melting power, maintain the insulation power of 250kW, perform infrared optical temperature measurement on the molten steel, control the temperature of the molten steel at 1500℃, and enter the first refining period, which lasts for 40 minutes. At the same time, maintain the vacuum degree of the melting chamber, and continue to evacuate the melting chamber to make the molten steel degassing more thoroughly.
[0070] 6) After the refining period begins, the first sampling and analysis of the molten steel in the crucible is carried out to detect the composition of the molten steel in the furnace.
[0071] 7) After the first sampling and analysis results come out, compare the content of each element analyzed in the furnace with the control range and target value of the element on the process sheet. If the amount of a certain element is lacking, it is necessary to calculate the amount of the element to be added. The calculation formula is: weight of the element to be added = [(theoretical total weight of the furnace * target content value of the element) - (real-time weight of molten steel * composition value of the element analyzed in the furnace)] / (element recovery rate * metal purity). After calculation, 5.8kg of metallic nickel, 2.5kg of metallic molybdenum, 6.32kg of aluminum, and 2.26kg of titanium need to be added. The power is turned off for 8 minutes, which is the second feeding. That is, the surface of the molten steel is observed after the power is turned off. When the surface of the molten steel is filmed, the charge (5.8kg of metallic nickel, 2.5kg of metallic molybdenum, 6.32kg of aluminum, and 2.26kg of titanium) to be added is added into the crucible under vacuum through the charging barrel, and the power is supplied for melting. After the added charge is melted, the medium frequency melting power is turned off, and the three-phase electromagnetic stirring is started (control stirring parameters: voltage 120V, current 7000A) for 4 minutes. After that, the melting power is switched back, the steel temperature is adjusted to 1495℃, the power supply is 250kW, and the second sampling analysis is carried out to detect the composition of the molten steel in the furnace. Then the second refining period begins, and the refining is kept warm for 30 minutes.
[0072] 8) After the second sampling test results come out, refer to the calculation method of step 7, and fine-tune the composition by adding 0.5kg of aluminum, 0.3kg of titanium and 0.27kg of ferroboron (boron content 17wt%), i.e. the third feeding. The feeding operation is the same as that described in step 7. After the power is increased to melt, start the three-phase electromagnetic stirring (control stirring parameters: voltage 118V, current 6800A) for 2 minutes, then switch back to the melting power for temperature measurement, control the steel temperature at 1495°C, send 250kW of power for heat preservation and refining, and enter the third refining period, which lasts for 10 minutes.
[0073] 9) After the third refining period is over, stop evacuating the melting chamber, fill the melting chamber with argon to 28000Pa, add 4.5kg nickel-magnesium alloy (magnesium content 20wt%), start three-phase electromagnetic stirring (control stirring parameters: voltage 120V, current 7000A) for 5min, take the third sample after stirring, and then keep it at 280kW for 3min to make the inclusions float fully, so as to reduce the inclusions in the molten steel. Adding nickel-magnesium alloy under protective atmosphere is conducive to reducing the burning loss of magnesium; and the addition of magnesium is conducive to further deoxidation of the molten steel, and the trace magnesium element contained in the steel is conducive to improving the subsequent hot working performance.
[0074] 10) Adjust the steel temperature to the tapping temperature of 1520℃, maintain the power supply at 350kW, and cast. In the argon protective atmosphere, cast the molten steel into the mold, and control the casting speed at 350kg / min. After casting, turn off the power.
[0075] 11) The argon gas in the ingot mold chamber is evacuated, and the evacuation is stopped when the vacuum value reaches 100 Pa. The pressure is maintained until the next day and then demolding is performed to obtain a GH4169 high-temperature alloy steel ingot.
[0076] Test example
[0077] The composition of the GH4169 high temperature alloy steel ingot obtained in Example 1 is as follows: (unit: wt%)
[0078] element C Si Mn Ni Cr Mo Nb Fe content 0.03 0.09 0.07 52.83 18.48 3.04 5.31 18.01 element Co Cu Mg S P O N B content 0.19 0.04 0.0074 0.0005 0.0039 0.0004 0.0028 0.0029 element Al Ti content 0.70 1.00
[0079] The composition of the GH4169 high-temperature alloy ingot produced by the vacuum induction melting process of the present invention is precisely controlled, and the mass percentage of oxygen is controlled within 4×10 -6 %, which is in an extremely low range, reducing the formation of oxide inclusions in the steel ingot. The actual furnace load was 4491kg, and 3931kg of returned materials were used, accounting for 87.53wt%, which greatly reduced the cost of raw materials.
[0080] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A GH4169 high temperature alloy, characterized in that: Raw materials include return materials, carbon particles, industrial pure iron, electrolytic nickel, metallic chromium, molybdenum, niobium, and nickel-magnesium alloy; In terms of mass percentage, the return material accounts for 70-98% of the total raw materials; The returned materials include GH4169 high temperature alloy returned materials and / or other steel grades with similar compositions, wherein the other steel grades with similar compositions include GH3039 alloy and GH4080A alloy; The mass percentage of oxygen in the GH4169 high temperature alloy is not higher than 4×10 -4 %; GH4169 high temperature alloy adopts vacuum induction melting process, which includes the following steps: S1: first feeding and preheating; S2: heating until the charge is melted, adding niobium and heating until the charge is melted again; S3: first refining; S4: second refining; S5: third refining; S6: filling with argon and adding nickel-magnesium alloy; S7: heating and casting to obtain the GH4169 high temperature alloy; Wherein, electromagnetic stirring is also included after steps S2, S3, S4 and S6; The first sampling is included at the beginning of the first refining, the second sampling is included at the beginning of the second refining, and the third sampling is included at the end of the third refining; In step S1, the first feeding is to place 5-15wt% of the return material flat on the bottom of the crucible, then add carbon particles, electrolytic nickel, industrial pure iron, metal chromium and molybdenum, and finally add the return material to the slag line of the crucible; The remaining return material is added when the material added in step S2 is completely melted; The preheating in step S1 is to adjust the power of the smelting chamber to 200 kW and preheat for 0.5 to 1 hour when the vacuum value of the smelting chamber is ≤10 Pa. In step S2, before heating and melting, the power supply is increased to 300 kW, heated for 1 to 1.5 hours, the power is reduced to 240 to 280 kW, and the temperature is kept for 30 to 40 minutes; The power supply during heating and melting in step S2 is 500~800kW. The electromagnetic stirring is three-phase electromagnetic stirring, with a voltage of 110-130V, a current of 5500-7500A, and a stirring time of 2-5min; The first refining time is 30-50 minutes, and the refining temperature is 1480±20°C; The second refining time is 20-30 minutes, and the refining temperature is 1480±20°C; The third refining time is 10 minutes, and the refining temperature is 1480±20°C.
2. The GH4169 high temperature alloy according to claim 1, characterized in that: The chemical composition of the GH4169 high-temperature alloy, measured in percentage by mass, includes: C≤0.08%, Si≤0.35%, Mn≤0.35%, Ni 50.0~55.0%, Cr 17.0~21.0%, Fe 15.0~21.0%, Al 0.2~0.8%, Ti 0.65~1.15%, Mo 2.8~3.3%, Nb 4.75~5.5%, Mg0.003~0.009%, Cu≤0.3%, B≤0.006%, Co≤0.3%, S≤0.002%, P≤0.005%, O≤0.001%, N≤0.004%, and the rest are unavoidable impurities.
3. A smelting process for the GH4169 high temperature alloy according to any one of claims 1 to 2, characterized in that: The vacuum induction melting process is characterized by comprising the following steps: S1: first feeding and preheating; S2: heating until the charge is melted, adding niobium and heating until the charge is melted again; S3: first refining; S4: second refining; S5: third refining; S6: filling with argon and adding nickel-magnesium alloy; S7: heating and casting to obtain the GH4169 high temperature alloy; Wherein, electromagnetic stirring is also included after steps S2, S3, S4 and S6; The first sampling is included at the beginning of the first refining, the second sampling is included at the beginning of the second refining, and the third sampling is included at the end of the third refining. After the first sampling results come out, compare the content of each element with the control range and target value of the element. When the amount of a certain element is insufficient, calculate the amount of the element to be added and carry out the second addition. The calculation formula is: the weight of the element to be added = [(theoretical total weight of the furnace * target content value of the element) - (real-time molten steel weight * component value of the element analyzed in the furnace)] / (element yield * metal purity); after the second addition, turn off the power and conjunctiva for 5~10 minutes, and heat to melt the second addition; After the second sampling results come out, compare the content of each element with the control range and target value of the element. When the amount of a certain element is lacking, calculate the amount of the element to be added and make the third addition. The calculation formula is: weight of the element to be added = [(theoretical total weight of the furnace * target content value of the element) - (real-time weight of molten steel * component value of the element analyzed in the furnace)] / (element recovery rate * metal purity). Heat to melt the third addition.
4. The smelting process according to claim 3, characterized in that: In step S6, the smelting chamber is filled with argon to 25000-30000 Pa, and the nickel-magnesium alloy is added and stirred for 2-5 minutes, and then allowed to stand for 3-5 minutes at a power supply of 240-280 kW.
5. The smelting process according to claim 4, characterized in that: In step S7, the tapping temperature is 1520±20°C, the power supply is 300-400kW, and the casting speed is 300-400kg / min.