A kind of iron-carbon slow-release material and its preparation method and application
By using silica to coat iron particles and activated carbon as a composite catalyst to restrain the iron active center and weaken the iron carbon reaction, the problem of difficult iron sludge generation and reaction rate control in the treatment of petroleum hydrocarbon pollutants is solved. A wider range of pH application and long-term catalytic oxidation activity are achieved.
Patent Information
- Application Number
- CN202111277404.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-30
AI Technical Summary
The existing iron-carbon catalytic materials have severe iron-carbon reactions when dealing with petroleum hydrocarbon pollutants, resulting in large quantities of iron sludge, blocking water flow channels and difficulty in replacing catalysts, and it is difficult to control the reaction rate.
Using a composite catalyst coated with silica with activated carbon as the support, the hydrophobic silica porous structure is formed by premixed cross-linking to constrain the iron active center, weaken the null microelectrolytic reaction between iron and carbon, and adsorption by porous structure Iron ions delay iron consumption and reaction rate.
It has achieved slow iron participation in the reaction, reduced iron sludge production, expanded the scope of pH application, improved catalytic oxidation activity and mechanical strength, and enhanced the long-term repair ability of petroleum hydrocarbon pollutants.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic materials, and in particular relates to a catalytic material for catalytic oxidation and a preparation method thereof. Background Art
[0002] Advanced oxidation techniques (AOPs) can utilize highly active, strong oxidizing free radical species activated by oxidants such as persulfate, percarbonate, hydrogen peroxide and ozone to efficiently oxidize and degrade organic pollutants. They have the advantages of fast reaction rate, strong oxidation ability, almost no selectivity for organic matter and high mineralization rate. In recent years, advanced oxidation techniques have developed rapidly in the field of organic pollutant wastewater treatment.
[0003] Iron-carbon material is a material for degrading organic pollutants. It has the characteristics of micro-electrolysis reaction and has been used in many occasions. However, the conventional iron-carbon oxidation reaction has the problem of violent iron-carbon reaction, large amount of iron sludge is produced, and it needs to be in acidic conditions to have good activity, so its application is limited.
[0004] Iron-carbon activated persulfate has broadened the pH application range, but there are still problems with violent reactions and the generation of a large amount of iron sludge. Therefore, two approaches, iron slow release and oxidant slow release, are considered. Researchers use nano zero-valent iron and porous Fe2O3 particles to activate persulfate for organic pollutant treatment, which can slowly release Fe 2+ , thereby controlling the activation speed of persulfate and ensuring that the system continuously and efficiently degrades pollutants. However, like the slow release of oxidants, it cannot solve the problem of iron consumption and large amounts of iron sludge produced by electrolysis of iron-carbon. The production of iron sludge will block the water flow channel and make it difficult to replace the catalyst, so the slow release material needs to have long-term activity.
[0005] The sustained-release technology was first used in the development of medicine in the medical field. Now, after receiving widespread attention, it has gradually been applied to the environmental field to treat soil and groundwater pollution, and has achieved good remediation effects. As a result, sustained-release agents for pollution remediation have been derived. However, most of them are for the sustained release of oxidants, and there are few studies on the sustained release of iron.
[0006] CN108675431A discloses a method for preparing a porous carbon-coated magnetic nano-iron water treatment composite material by low-temperature pyrolysis of a metal organic framework (MOF) and its application method in water treatment. The present invention first uses urea to prepare graphite phase carbon nitride (g-C3N4), then couples it with an iron-containing MOF in situ, and finally pyrolyzes it at low temperature in an inert atmosphere to obtain a porous carbon-coated magnetic nano-iron water treatment composite material. The iron element in the composite material obtained by the present invention is mainly present in the porous carbon in the form of zero-valent iron and γ-Fe2O3, and has excellent magnetic properties and is easy to be magnetically separated. However, the product prepared by this method has close contact between iron and carbon, which is easy to cause the loss of iron ions and is not suitable for iron-carbon reaction.
[0007] CN108690625A discloses a slow-release composite repair agent for treating persistent halogenated hydrocarbons in soil and its preparation method. The preparation method includes 1) preparing bacterial liquid saturated black carbon; 2) preparing a colloidal solution A containing locust bean gum and an organic carbon source; 3) preparing a colloidal suspension B containing locust bean gum, an organic carbon source, a nano-scale zero-valent metal and bacterial liquid saturated black carbon; 4) cross-linking reaction for 2 to 6 hours; 5) delaying the cross-linking reaction for 2 to 6 hours to obtain a slow-release composite repair agent for treating persistent halogenated hydrocarbons in soil. The invention does not involve iron-carbon reaction.
[0008] CN201910067630.3 Preparation and application of functional slow-release microcapsules for soil heavy metal treatment, discloses that under certain conditions, microcrystalline cellulose is used as raw material, sodium alginate is used as adhesive, CaCl2 is used as curing liquid, and nano zero-valent iron (nZVI) is used as core material to prepare slow-release microcapsules for soil heavy metal pollution treatment. The invention uses a slow-release agent to encapsulate nano zero-valent iron, and the reaction rate is difficult to control.
[0009] CN201910373586.9 discloses a novel biomass iron-carbon composite material based on cherry pits. Cherry pit powder is mixed evenly with anhydrous FeCl3 and calcined at high temperature under an inert atmosphere. 3+ Cherry pit powder can be activated by its oxidative property, and then reduced to iron nanoparticles loaded on cherry pit powder biomass activated carbon. This material can be used to catalyze the activation of sodium persulfate to produce active free radicals to degrade endocrine disruptor bisphenol A. This invention introduces iron in a conventional way and does not involve sustained release treatment.
[0010] CN202010346235.1 discloses a production process of nano-scale iron oxide, which is obtained by pre-activating the nano-scale iron oxide and then mixing it with a hydrophobic agent to obtain nano-scale hydrophobic iron oxide through a series of reactions. The nano-scale iron oxide of the present invention is first activated to make the contact effect between the nano-scale iron oxide and the hydrophobic agent better, thereby improving the hydrophobic ability of the nano-scale iron oxide. It can be used in the field of hydrophobic material preparation. Summary of the invention
[0011] In view of the shortcomings of the prior art, the main purpose of the present invention is to provide an iron-carbon slow-release material and a preparation method and application thereof. The provided iron-carbon slow-release material can enable iron to react slowly with carbon and protect the iron from being rapidly oxidized, thereby being combined with an in-situ catalytic oxidation method to carry out long-term repair of petroleum hydrocarbon pollutants.
[0012] The first aspect of the present invention provides an iron-carbon slow-release material, which includes an iron phase, silicon dioxide, carbon and an inorganic refractory oxide; the iron phase is dispersed particles of zero-valent iron and ferric oxide, the surface of the iron phase is coated with silicon dioxide, and the iron phase coated with silicon dioxide is distributed in the pores and / or on the surface of the carbon and the inorganic refractory oxide.
[0013] Furthermore, in the above-mentioned iron-carbon slow-release material, based on the total weight of the iron-carbon slow-release material, the iron phase content is 5wt%~35wt%, preferably 10wt%~30wt%; the silicon dioxide content is 0.5wt%~4.0wt%, preferably 1.0wt%~3.0wt%; the carbon content is 10wt%~55wt%, preferably 15wt%~45wt%; the inorganic refractory oxide content is 30wt%~70wt%, preferably 35wt%~60wt%.
[0014] Furthermore, in the above-mentioned iron-carbon sustained-release material, the pore size distribution of the iron-carbon sustained-release material is as follows, wherein the pore diameter of the first-level channel is less than 4nm, and the most probable pore diameter is 2.5nm; the pore diameter of the second-level channel is 4-9nm, and the most probable pore diameter is 7.5nm; the pore diameter of the third-level channel is greater than 9nm, preferably 9-20nm, and the most probable pore diameter is 13.5nm. Furthermore, the peak intensity ratio represented by the Y-axis coordinates corresponding to the most probable pore diameters of the first-level channel, the second-level channel and the third-level channel is 2:1~4:1~8.
[0015] Furthermore, in the above-mentioned iron-carbon slow-release material, the specific surface area of the iron-carbon slow-release material is 120 to 1200 m 2 / g.
[0016] The second aspect of the present invention provides a method for preparing an iron-carbon sustained-release material, the preparation method comprising the following contents:
[0017] (1) Mixing iron salt and stabilizer, and then adding alkaline substance to obtain iron-containing material;
[0018] (2) mixing the first silicon source, the second silicon source, and the organic solvent, and mixing them evenly to obtain a silicon-containing material;
[0019] (3) Mixing and reacting the iron-containing material, the silicon-containing material, formaldehyde, and the additive, and mixing them evenly to obtain material A;
[0020] (4) mixing a carbon source, an inorganic refractory oxide and a binder, and after uniform mixing, forming, drying and calcining to obtain a carrier precursor;
[0021] (5) The carrier precursor obtained in step (4) is mixed with the material A obtained in step (3) and reacted, and then dried and calcined to obtain an iron-carbon slow-release material.
[0022] Furthermore, in the preparation method of the above-mentioned iron-carbon sustained-release material, the iron salt in step (1) includes a trivalent iron salt and an optional divalent iron salt, preferably a trivalent iron salt; the trivalent iron salt is at least one of ferric nitrate, ferric chloride, ferric citrate, ferric acetate, and ferric sulfate, preferably ferric sulfate; the divalent iron salt is at least one of ferrous chloride, ferrous acetate, and ferrous sulfate, preferably ferrous sulfate.
[0023] Furthermore, in the preparation method of the above-mentioned iron-carbon sustained-release material, the stabilizer in step (1) is one or more of hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, octadecyltrimethylammonium bromide, polyamide, polyethyleneimine, and dimercaptosuccinic acid.
[0024] Furthermore, in the method for preparing the iron-carbon sustained-release material, the alkaline substance in step (1) is at least one of sodium hydroxide, potassium hydroxide, ammonia water, urea, and sodium bicarbonate. The molar amount of the alkaline substance added is 0.8 to 1.5 times that of the iron element.
[0025] Furthermore, in the preparation method of the above-mentioned iron-carbon slow-release material, the first silicon source in step (2) is at least one of silica sol, sodium silicate, and silicic acid, preferably silica sol; the silica sol is further preferably alkaline silica sol, the pH value of the alkaline silica sol is 9-12, and the concentration of the silica sol is 10wt% to 40wt%.
[0026] Furthermore, in the preparation method of the iron-carbon sustained-release material, the second silicon source in step (2) is an organic silicon ester and / or an organic siloxane, and the second silicon source can be selected from one or more of tetraethyl silicate, methyl orthosilicate, methyl trimethoxysilane, methyl triethoxysilane, trimethyl chlorosilane, and octyl trimethoxysilane; preferably tetraethyl silicate. The mass ratio of silicon dioxide contained in the second silicon source to the first silicon source is 1:2-6.
[0027] Furthermore, in the preparation method of the above-mentioned iron-carbon sustained-release material, the organic solvent in step (2) is an alcohol compound and / or an ether compound, and the alcohol compound can be selected from one or more of methanol, ethanol, n-propanol, n-butanol, n-pentanol, isopropanol, isobutanol and isopentanol, preferably ethanol; the ether compound can be specifically selected from one or more of diethyl ether, petroleum ether, tetrahydrofuran, 1,4-dioxane, preferably tetrahydrofuran.
[0028] Furthermore, in the preparation method of the above-mentioned integral slow-release iron-carbon catalytic material, the auxiliary agent in step (3) is at least one of phenol, cresol, xylenol, resorcinol, and urea, and the molar ratio of the auxiliary agent to formaldehyde is 1.2 to 2.5:1.
[0029] Furthermore, in the method for preparing the above-mentioned integral slow-release iron-carbon catalytic material, the reaction condition in step (3) is that the reaction temperature is 20 to 90°C.
[0030] Furthermore, in the method for preparing the above-mentioned integral slow-release iron-carbon catalytic material, the reaction condition in step (3) is that the pH value of the reaction system is 9-12.
[0031] Furthermore, in the preparation method of the above-mentioned iron-carbon slow-release material, the carbon source in step (4) can be one or more selected from biomass charcoal, petroleum-based charcoal, coal-based charcoal, etc., and the carbon element content of the carbon source is not less than 60wt%; further, the carbon source can specifically be one or more of activated carbon, fruit shell powder, wood powder, coconut shell powder, coal powder, coal tar, asphalt, organic polymers (polyethylene, polystyrene, polyvinyl chloride, polyacrylic acid, polyacrylonitrile, polymethyl methacrylate, polylactic acid, polycarbonate, phenolic resin, urea-formaldehyde resin), and cellulose.
[0032] Furthermore, in the preparation method of the above-mentioned iron-carbon slow-release material, the inorganic refractory oxide in step (4) can be one or more of alumina, molecular sieve, and clay; further, the molecular sieve can be one or more of ZSM-5 molecular sieve, A-type molecular sieve, Y-type molecular sieve, and β molecular sieve; the clay can be silica-alumina clay, with a particle size of 300 to 2000 mesh, the sum of the mass of SiO2 and Al2O3 in the component accounts for more than 80% of the total mass of the silica-alumina clay, and the specific surface area is 5 to 500 m 2 / g.
[0033] Furthermore, in the preparation method of the above-mentioned iron-carbon sustained-release material, the binder in step (4) is one or more of water, an inorganic binder and an organic binder, the inorganic binder can be selected from one or more of silica sol, aluminum sol, aluminum dihydrogen phosphate, and water glass, and the organic binder can be selected from one or more of hydroxymethyl cellulose, carboxymethyl cellulose, carboxyethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol, and polyethylene glycol.
[0034] Furthermore, in the above-mentioned method for preparing the iron-carbon sustained-release material, the drying temperature in step (4) is 50 to 120°C, preferably 60 to 110°C.
[0035] Furthermore, in the preparation method of the above-mentioned iron-carbon sustained-release material, the calcination in step (4) is carried out under oxygen-free conditions, such as in an inert atmosphere such as nitrogen, helium, neon, argon, etc., and the calcination temperature is 500-900°C, preferably 600-700°C; the calcination time is 1-8h, preferably 2-4h.
[0036] Furthermore, in the above-mentioned method for preparing the iron-carbon sustained-release material, the reaction temperature in step (5) is 20 to 80° C., the reaction time is 2 to 24 hours, and the pH value of the reaction system is preferably controlled to be 9 to 12.
[0037] Furthermore, in the above-mentioned method for preparing the iron-carbon sustained-release material, the drying temperature in step (5) is 50 to 120°C, preferably 60 to 110°C.
[0038] Furthermore, in the preparation method of the above-mentioned iron-carbon sustained-release material, the calcination in step (5) is carried out under oxygen-free conditions, such as in an inert atmosphere such as nitrogen, helium, neon, argon, etc., and the calcination temperature is 500-900°C, preferably 600-700°C; the calcination time is 1-8h, preferably 2-4h.
[0039] The third aspect of the present invention provides an iron-carbon slow-release material obtained by the above-mentioned preparation method.
[0040] Furthermore, in the above-mentioned iron-carbon slow-release material, the iron-carbon slow-release material includes an iron phase, silica, carbon and an inorganic refractory oxide; the iron phase is dispersed particles of zero-valent iron and ferric oxide, the surface of the iron phase is coated with silica, and the iron phase coated with silica is distributed in the pores and / or on the surface of the carbon and the inorganic refractory oxide.
[0041] Furthermore, in the above-mentioned iron-carbon slow-release material, based on the total weight of the iron-carbon slow-release material, the iron phase content is 5wt%~35wt%, preferably 10wt%~30wt%; the silicon dioxide content is 0.5wt%~4.0wt%, preferably 1.0wt%~3.0wt%; the carbon content is 10wt%~55wt%, preferably 15wt%~45wt%; the inorganic refractory oxide content is 30wt%~70wt%, preferably 35wt%~60wt%.
[0042] Furthermore, in the above-mentioned iron-carbon sustained-release material, the pore size distribution of the iron-carbon sustained-release material is as follows, wherein the pore diameter of the first-level channel is less than 4nm, and the most probable pore diameter is 2.5nm; the pore diameter of the second-level channel is 4-9nm, and the most probable pore diameter is 7.5nm; the pore diameter of the third-level channel is greater than 9nm, preferably 9-20nm, and the most probable pore diameter is 13.5nm. Furthermore, the ratio of the peak intensity (peak height) represented by the Y-axis coordinate corresponding to the most probable pore diameters of the first-level channel, the second-level channel and the third-level channel is 2:1~4:1~8.
[0043] Furthermore, in the above-mentioned iron-carbon slow-release material, the specific surface area of the iron-carbon slow-release material is 120 to 1200 m 2 / g.
[0044] A fourth aspect of the present invention provides an application of the above-mentioned iron-carbon slow-release material in the treatment of wastewater containing petroleum hydrocarbons.
[0045] Furthermore, in the above application, the specific application process is that the petroleum hydrocarbon-containing wastewater is contacted with an oxidant and reacts in the presence of the above iron-carbon slow-release material to obtain purified water after the reaction.
[0046] Furthermore, in the above application, the oxidant is one or more of ozone, hydrogen peroxide, sodium persulfate, and sodium percarbonate.
[0047] Furthermore, in the above application, the petroleum hydrocarbons contained in the petroleum hydrocarbon-containing wastewater are mainly C4-C40 hydrocarbons, and the hydrocarbons are generally one or more of alkanes, olefins, benzene series, halogenated hydrocarbons, etc.
[0048] Compared with the prior art, the iron-carbon slow-release material and its preparation method and application described in the present invention have the following advantages:
[0049] The present invention provides a composite catalyst formed by silica-coated iron particles and carrier materials such as activated carbon. Among them, iron and silica are pre-mixed and cross-linked together to prepare a hydrophobic silica porous structure to constrain the iron active center, weaken the ineffective micro-electrolysis reaction of iron and carbon, so that iron slowly participates in the reaction and is not easy to produce iron mud. During use, the reaction core iron is highly dispersed in the carrier, so the consumption of iron will not affect the integrity of the carrier structure, and the mechanical strength of the material is not easy to change. The catalyst is used in combination with an oxidant in an advanced oxidation mode, has a wider pH range of application, and has a wider application value.
[0050] At the same time, the carbon-containing composite material used as a carrier has a strong adsorption capacity for organic pollutant components, and can adsorb pollutant molecules to the catalyst surface, thereby increasing the probability of contact between active components and pollutant molecules, improving local concentration, and promoting the initial reaction rate, which is beneficial to the catalytic oxidation reaction. The content of activated carbon in the carbon-containing composite carrier is controlled at a reasonable ratio, and the unique contact mode with iron particles also significantly reduces the ineffective reaction of iron-carbon micro-electrolysis. The carbon-containing composite carrier has a porous structure and can also adsorb iron ions produced by the iron-carbon reaction, forming catalytic active centers in situ, and continuously maintaining good catalytic oxidation activity. DETAILED DESCRIPTION
[0051] The preparation method of the present invention is further described below in conjunction with specific examples, but the scope of the present invention is not limited to the scope of these examples.
[0052] The specific surface area and average pore size involved in the embodiments of the present invention and the comparative examples are measured by a nitrogen physical adsorption instrument. The ratio of the most probable pore size corresponding to the Y-axis value on the pore size distribution curve is recorded as the peak intensity ratio. The iron ion analysis method is microwave digestion / inductively coupled plasma mass spectrometry. The silica content involved in the present invention is the mass of silica combined with iron when added, excluding the mass of silica introduced in the inorganic refractory oxide and the binder.
[0053] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight and pressure is gauge pressure.
[0054] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0055] Herein, for convenience of description, spatially relative terms, such as “below,” “beneath,” “lower,” “above,” “over,” “upper,” etc., may be used to describe the relationship between one element or feature and another element or feature.
[0056] In this document, the terms "first", "second", etc. are used to distinguish two different elements or parts, and are not used to limit a specific position or relative relationship. In other words, in some embodiments, the terms "first", "second", etc. can also be interchangeable.
[0057]
[0043] All numerical values for parameters (eg, amounts or conditions) herein are to be understood as being modified in all instances by the term "about", whether or not "about" actually appears before the numerical value.
[0058] In the context of this specification, any two or more embodiments of the present invention may be arbitrarily combined, and the technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.
[0059] Example 1
[0060] Weigh 241g of ferric nitrate to make an iron salt solution, add 2.8g of hexadecyltrimethylammonium bromide, stir evenly, and then add 60.7g of ammonia water to form colloidal solution A. Weigh 13.3g of 30wt% silica sol, 5.6g of tetraethyl silicate and 25g of ethanol, mix them, stir evenly, and then add 1.8g of phenol. Then pour solution A into it, adjust the pH to 9.5 with ammonia water, add 1.2g of formaldehyde, and continue stirring for 30min to form solution B. Mix 290g of activated carbon, 186g of silica-alumina clay and 22.4g of water glass evenly, extrude them into strips according to the conventional method, dry them at 110℃ for 8h, and bake them at 600℃ in an oxygen-free state for 6h to obtain a carrier. Add the carrier to solution B, heat it to 65℃ in a water bath, react for 6h, take out the carrier and evaporate it to dryness. The dried material is baked at 550℃ in an oxygen-free state for 3h to obtain iron-carbon slow-release material A1. The specific surface area of the material is 523m 2 / g, the ratio of the most probable pore peak intensity of the first-order pore, the second-order pore and the third-order pore is 2:1.3:2.6.
[0061] Example 2
[0062] Weigh 245g of ferric citrate to make an iron salt solution, add 1.2g of polyacetimide and stir evenly. Add 40g of sodium hydroxide to form colloidal solution A. Weigh 5.1g of sodium silicate, 3.8g of methyltriethoxysilane and 40g of ether, mix them, stir evenly, then add 1.5g of urea, pour solution A into it, adjust the pH to 10 with sodium hydroxide, add 1.0g of formaldehyde, and continue stirring for 10min to form solution B. Mix 56g of activated carbon, 104g of silica-alumina clay, 50g of 4A molecular sieve and 20g of aluminum dihydrogen phosphate colloid evenly, extrude into strips according to conventional methods, dry at 100℃ for 12h, and calcine at 700℃ for 2h in an oxygen-free state to obtain a carrier. Immerse the carrier in solution B, react at room temperature for 6h, and evaporate to dryness by rotary evaporation. The dried material is calcined at 500℃ for 2h in an oxygen-free state to obtain iron-carbon sustained-release material A2. The specific surface area of the material is 387m 2 / g, the ratio of the most probable pore peak intensity of the first-order pore, the second-order pore and the third-order pore is 2:3.3:3.6.
[0063] Example 3
[0064] Weigh 152g of ferrous sulfate to make an iron salt solution, add 2.0g of octadecyltrimethylammonium bromide, and stir evenly. Then add 80g of sodium bicarbonate to form colloidal solution A. Weigh 5g of 40% alkaline silica sol, 2.8g of tetraethyl methyl silicate and 40g of methanol, mix them, stir evenly, add 2.0g of resorcinol, then pour solution A, adjust the pH to 9.5 with potassium hydroxide, add 0.8g of formaldehyde, and continue stirring for 20min to form solution B. Mix 74.6g of activated carbon, 87.6g of alumina and 5.6g of carboxymethyl cellulose evenly, extrude them into strips according to the conventional method, dry them at 95℃ for 7h, and roast them at 680℃ under argon protection for 6h to obtain the carrier. Add the carrier to solution B, heat it to 62℃ in a water bath, react for 6h, take out the carrier and evaporate it to dryness. The dried material is isolated from oxygen and roasted at 600℃ for 5h to obtain iron-carbon slow-release material A3. The specific surface area of the material is 611m 2 / g, the ratio of the most probable pore peak intensity of the first-order pore, the second-order pore and the third-order pore is 2:3.5:5.5.
[0065] Example 4
[0066] Weigh 400g of ferric sulfate to make an iron salt solution, add 1.6g of polyamide, and stir evenly. Then add 60g of urea to form colloidal solution A. Weigh 4.5g of silicic acid, 1.3g of trimethylchlorosilane and 25g of tetrahydrofuran, mix them, stir evenly, add 2.4g of phenol, adjust the pH to 9.5 with potassium hydroxide, add 1.6g of formaldehyde, and continue stirring for 20min to form solution B. Mix 286g of activated carbon, 240g of white carbon black and 36.4g of water glass evenly, extrude into strips according to the conventional method, dry at 100℃ for 12h, and roast at 700℃ for 2h to obtain a carrier. Mix solutions A and B, stir for 15min, add the carrier, heat to 75℃ in a water bath, react for 5h, take out the carrier and evaporate it to dryness. The dried material is roasted at 680℃ for 6h under nitrogen protection to obtain iron-carbon sustained-release material A4. The specific surface area of the material is 658m 2 / g, the ratio of the most probable pore peak intensity of the first-order pore, the second-order pore and the third-order pore is 2:1.2:1.8.
[0067] Example 5
[0068] Weigh 95.5g of ferric acetate and 63g of ferrous chloride to form an iron salt solution, add 2.5g of hexadecyltrimethylammonium chloride, and stir evenly. Then add 60g of potassium hydroxide to form colloidal solution A. Weigh 19.3g of 20wt% alkaline silica sol, 2.4g of tetraethyl silicate and 30g of ethanol, stir evenly, add 2.3g of urea, adjust the pH to 10 with ammonia water, add 1.7g of formaldehyde dropwise, and continue stirring for 20min to form solution B. Mix 28.4g of activated carbon, 78.8g of silica-alumina clay and 13.3g of hydroxypropyl methylcellulose evenly, extrude into strips according to the conventional method, dry at 90℃ for 12h, and calcine at 650℃ under nitrogen protection for 6h to obtain a carrier. Mix solutions A and B, stir for 20min, add the carrier, heat to 55℃ in a water bath, react for 6h, take out the carrier and evaporate to dryness. The dried material was calcined at 720℃ under nitrogen protection for 6h to obtain the iron-carbon slow-release material A5. The specific surface area of the material is 523m 2 / g, the ratio of the most probable pore peak intensity of the first-order pore, the second-order pore and the third-order pore is 2:3.6:6.2.
[0069] Example 6
[0070] 200 mL of iron-carbon slow-release material A1 was loaded into a cylindrical reaction tube. The gasoline simulated petroleum hydrocarbon wastewater with a COD of 150 mg / L was continuously treated under the action of 250 mg / L of sodium persulfate. The iron ion concentration in the effluent was 26 mg / L, and the COD removal rate was 93.1%.
[0071] Example 7
[0072] 1g of iron-carbon slow-release material A2 was measured and filled into a sealed bottle. 100g of gasoline-simulated petroleum hydrocarbon wastewater with an initial COD of 150 mg / L was poured into it. Then 0.2g of sodium persulfate was added. The mixture was continuously oscillated at 25°C in a constant temperature oscillator for 180min. The iron ion concentration in the water sample after the reaction was detected to be 55 mg / L, and the COD removal rate was 95.3%.
[0073] Example 8
[0074] 200 mL of iron-carbon slow-release material A3 was loaded into a cylindrical reaction tube. Diesel simulated petroleum hydrocarbon wastewater with a COD of 120 mg / L was continuously treated under the action of 125 mg / L of sodium persulfate. The iron ion concentration in the effluent was 21 mg / L, and the COD removal rate was 92.5%.
[0075] Example 9
[0076] 0.5g of iron-carbon slow-release material A4 was measured and filled into a sealed bottle. 100g of gasoline-simulated petroleum hydrocarbon wastewater with an initial COD of 100 mg / L was poured into it. 0.2g of sodium persulfate was added and the mixture was continuously oscillated at 35°C in a constant temperature oscillator for 120min. The iron ion concentration in the water sample after the reaction was detected to be 28 mg / L, and the COD removal rate was 94.2%.
[0077] Example 10
[0078] 500 mL of iron-carbon slow-release material A5 was loaded into a cylindrical reaction tube. The gasoline simulated petroleum hydrocarbon wastewater with a COD of 120 mg / L was continuously treated under the action of 300 mg / L of sodium persulfate. The iron ion concentration in the effluent was 59 mg / L, and the COD removal rate was 96.1%.
[0079] Comparative Example 1
[0080] 386.4g activated carbon, 140g silica-alumina clay and 22.4g water glass were mixed evenly, extruded into strips according to conventional methods, dried at 110°C for 8h, and calcined at 600°C in an oxygen-free state for 6h to obtain a carrier. 241g ferric nitrate was weighed to prepare an iron salt solution, and the carrier was added to the solution for impregnation, and then rotary evaporated to dryness. The dried material was calcined at 550°C in an oxygen-free state for 3h to obtain catalytic material B1.
[0081] Comparative Example 2
[0082] 45g and 25g of iron filings and activated carbon were weighed respectively, mixed and loaded in a cylindrical reaction tube, and continuously reacted to treat gasoline simulated petroleum hydrocarbon wastewater with a COD of 200 mg / L under the action of 300mg / L of sodium persulfate. There was obvious yellow precipitation in the effluent, and the contact between iron filings and activated carbon quickly hardened. The iron ion concentration was 7839 mg / L, and the COD removal rate was 88.1% after the iron ions were precipitated.
[0083] Comparative Example 3
[0084] Example 6 was repeated, except that the iron-carbon slow-release material A1 was replaced with the catalytic material B1. The iron ion concentration in the effluent was 1426 mg / L, and the COD removal rate was 79.2%.
[0085] Comparative Example 4
[0086] Using conventional iron-carbon reaction, 40g, 20g and 35g of iron filings, activated carbon and inert porcelain balls were weighed respectively, mixed and loaded into a cylindrical reaction tube, and toluene with a COD of 160 mg / L was introduced to simulate petroleum hydrocarbon wastewater. There was obvious yellow precipitation in the effluent, and the contact between iron filings and activated carbon quickly hardened. The iron ion concentration was 6621 mg / L, and the COD removal rate was 81.5% after the iron ions were precipitated.
[0087] Comparative Example 5
[0088] Weigh 50g of activated carbon and 50g of iron filings, mix and load them in a cylindrical reaction tube, use the raw water from a gas station with an average COD value of 140mg / L containing petroleum hydrocarbons, add 100 mg / L of sodium persulfate for continuous reaction, and there is obvious yellow precipitation in the effluent water, and the contact between the iron filings and the activated carbon quickly hardens. The iron ion concentration is 7351 mg / L, and the COD removal rate after the iron ions are precipitated is 87.2%.
Claims
1. An iron-carbon slow-release material, comprising an iron phase, silicon dioxide, carbon and an inorganic refractory oxide; the iron phase is dispersed particles of zero-valent iron and ferric oxide, the outer surface of the iron phase is coated with silicon dioxide, and the iron phase coated with silicon dioxide is distributed in the pores and / or on the surface of the carbon and the inorganic refractory oxide; The preparation method of the iron-carbon slow-release material comprises the following contents: (1) Mixing iron salt and stabilizer, and then adding alkaline substance to obtain iron-containing material; (2) mixing the first silicon source, the second silicon source, and the organic solvent, and mixing them evenly to obtain a silicon-containing material; (3) mixing and reacting the iron-containing material, the silicon-containing material, formaldehyde and the auxiliary agent, and obtaining material A after uniform mixing, wherein the auxiliary agent is at least one of phenol, cresol, xylenol, resorcinol and urea; (4) mixing a carbon source, an inorganic refractory oxide and a binder, and after uniform mixing, forming, drying and calcining, obtaining a carrier precursor; (5) mixing the carrier precursor obtained in step (4) and the material A obtained in step (3) and reacting them, and then drying and calcining them to obtain an iron-carbon slow-release material; In step 2), the first silicon source is at least one of silica sol, sodium silicate and silicic acid; the second silicon source is organic silicon ester and / or organic siloxane.
2. The iron-carbon slow-release material according to claim 1, wherein: Based on the total weight of the iron-carbon slow-release material, the iron phase content is 5wt% to 35wt%; the silicon dioxide content is 0.5wt% to 4.0wt%; the carbon content is 10wt% to 55wt%; and the inorganic refractory oxide content is 30wt% to 70wt%.
3. The iron-carbon slow-release material according to claim 2, wherein: Based on the total weight of the iron-carbon slow-release material, the iron phase content is 10wt% to 30wt%; the silicon dioxide content is 1.0wt% to 3.0wt%; the carbon content is 15wt% to 45wt%; and the inorganic refractory oxide content is 35wt% to 60wt%.
4. The iron-carbon slow-release material according to claim 1, wherein: The pore size distribution of the iron-carbon sustained-release material is as follows: the pore diameter of the first-level channel is less than 4nm, and the most probable pore diameter is 2.5nm; the pore diameter of the second-level channel is 4-9nm, and the most probable pore diameter is 7.5nm; the pore diameter of the third-level channel is greater than 9nm, and the most probable pore diameter is 13.5nm.
5. The iron-carbon slow-release material according to claim 4, wherein: The pore diameter of the third-level channel is 9 to 20 nm.
6. The iron-carbon slow-release material according to claim 1, wherein: The peak intensity ratios represented by the Y-axis coordinates of the most probable apertures of the first-order pores, the second-order pores and the third-order pores are 2:1-4:1-8.
7. The iron-carbon slow-release material according to claim 1, wherein: The specific surface area of the iron-carbon slow-release material is 120 to 1200 m 2 / g.
8. A method for preparing an iron-carbon sustained-release material, the method comprising the following contents: (1) Mixing iron salt and stabilizer, and then adding alkaline substance to obtain iron-containing material; (2) mixing the first silicon source, the second silicon source, and the organic solvent, and mixing them evenly to obtain a silicon-containing material; (3) mixing and reacting the iron-containing material, the silicon-containing material, formaldehyde and the auxiliary agent, and obtaining material A after uniform mixing, wherein the auxiliary agent is at least one of phenol, cresol, xylenol, resorcinol and urea; (4) mixing a carbon source, an inorganic refractory oxide and a binder, and after uniform mixing, forming, drying and calcining, obtaining a carrier precursor; (5) mixing the carrier precursor obtained in step (4) and the material A obtained in step (3) and reacting them, and then drying and calcining them to obtain an iron-carbon slow-release material; In step 2), the first silicon source is at least one of silica sol, sodium silicate and silicic acid; the second silicon source is organic silicon ester and / or organic siloxane.
9. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: The iron salt in step (1) includes a ferric salt and an optional ferrous salt; the ferric salt is at least one of ferric nitrate, ferric chloride, ferric citrate, ferric acetate, and ferrous sulfate; the ferrous salt is at least one of ferrous chloride, ferrous acetate, and ferrous sulfate.
10. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: In step (1), the stabilizer is one or more of hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, octadecyltrimethylammonium bromide, polyamide, polyethyleneimine, and dimercaptosuccinic acid.
11. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: In step (1), the alkaline substance is at least one of sodium hydroxide, potassium hydroxide, aqueous ammonia, urea, and sodium bicarbonate.
12. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: The molar amount of the alkaline substance added is 0.8 to 1.5 times that of the iron element.
13. The method for preparing the iron-carbon slow-release material according to claim 8, wherein: In step (2), the first silicon source is silica sol.
14. The method for preparing the iron-carbon slow-release material according to claim 13, wherein: The silica sol is alkaline silica sol, the pH value of the alkaline silica sol is 9-12, and the concentration of the silica sol is 10wt%-40wt%.
15. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: In step (2), the second silicon source is selected from one or more of tetraethyl silicate, methyl orthosilicate, methyltrimethoxysilane, methyltriethoxysilane, trimethylchlorosilane, and octyltrimethoxysilane; the mass ratio of silicon dioxide contained in the second silicon source to the first silicon source is 1:2-6.
16. The method for preparing the iron-carbon slow-release material according to claim 8, wherein: In step (2), the organic solvent is an alcohol compound and / or an ether compound, wherein the alcohol compound is selected from one or more of methanol, ethanol, n-propanol, n-butanol, n-pentanol, isopropanol, isobutanol and isopentanol; and the ether compound is selected from one or more of diethyl ether, petroleum ether, tetrahydrofuran and 1,4-dioxane.
17. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: In step (3), the molar ratio of the auxiliary agent to formaldehyde is 1.2 to 2.5:
1.
18. The method for preparing the iron-carbon slow-release material according to claim 8, wherein: In step (4), the carbon source is one or more selected from biomass charcoal, petroleum-based charcoal, and coal-based charcoal, and the carbon element content of the carbon source is not less than 60wt%.
19. The method for preparing the iron-carbon slow-release material according to claim 8, wherein: The carbon source is one or more of activated carbon, fruit shell powder, wood powder, coconut shell powder, coal powder, coal tar, asphalt, high molecular organic polymer with a polymerization degree greater than 3000, and cellulose.
20. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: In step (4), the inorganic refractory oxide is one or more of alumina, molecular sieve, and clay.
21. The method for preparing the iron-carbon slow-release material according to claim 8, wherein: The binder in step (4) is one or more of water, an inorganic binder and an organic binder, wherein the inorganic binder is selected from one or more of silica sol, alumina sol, aluminum dihydrogen phosphate and water glass, and the organic binder is selected from one or more of hydroxymethyl cellulose, carboxymethyl cellulose, carboxyethyl cellulose, hydroxypropyl methyl cellulose, polyvinyl alcohol and polyethylene glycol.
22. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: The drying temperature in step (4) and step (5) is 50 to 120°C.
23. The method for preparing the iron-carbon slow-release material according to claim 22, wherein: The drying temperature in step (4) and step (5) is 60 to 110°C.
24. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: The calcination in step (4) and step (5) is carried out under oxygen-free conditions at a calcination temperature of 500 to 900°C.
25. The method for preparing the iron-carbon slow-release material according to claim 24, wherein: The calcination temperature in step (4) and step (5) is 600-700°C.
26. The method for preparing the iron-carbon sustained-release material according to claim 8, wherein: The reaction temperature in step (5) is 20-80° C., and the pH value of the reaction system is controlled to be 9-12.
27. An iron-carbon sustained-release material obtained by the preparation method described in any one of claims 8 to 26.
28. An application of the iron-carbon slow-release material described in any one of claims 1-8 and 27 in the treatment of wastewater containing petroleum hydrocarbons, wherein the application process is that the wastewater containing petroleum hydrocarbons is contacted with an oxidant and reacts in the presence of the iron-carbon slow-release material to obtain purified water after the reaction.
29. The use according to claim 28, wherein: The oxidant is one or more of ozone, hydrogen peroxide, sodium persulfate and sodium percarbonate.