A composite metal oxide catalyst and its preparation method and application
By encapsulating manganese oxide and cerium oxide in all-silica molecular sieves, the problem of simultaneous improvement of low-temperature catalytic activity, water resistance and adsorption performance of composite metal oxide catalysts is solved, and efficient catalytic oxidation of volatile organic compounds is achieved. and excellent water resistance.
Patent Information
- Application Number
- CN202310077484.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-01-17
AI Technical Summary
Existing composite metal oxide catalysts cannot simultaneously take into account the defects and deficiencies of low-temperature catalytic activity, water resistance and adsorption performance, especially when dealing with volatile organic compounds.
By encapsulating manganese oxide and cerium oxide in all-silica molecular sieves, and controlling the content and proportion of active components, the high specific surface area and hydrophobicity of all-silica molecular sieves are used to improve the dispersion and water resistance of the catalyst to form manganese-cerium Metal complex oxides to improve catalytic activity and adsorption performance.
It achieves efficient catalytic oxidation of volatile organic compounds under low temperature conditions, improves the water resistance and adsorption performance of the catalyst, ensures that the catalytic activity is not reduced, and performs well under conditions containing water vapor.
Smart Images

Figure CN116060080B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal catalytic treatment of organic pollutants, and more specifically, to a composite metal oxide catalyst and a preparation method and application thereof. Background Art
[0002] Volatile organic compounds (VOCs) are toxic and are one of the most important sources of air pollution and excessive ozone. Catalytic oxidation technology can directly degrade VOCs into pollution-free CO2 and water. It has the advantages of energy saving, high efficiency and no secondary pollutants. It is considered to be one of the most effective and cost-effective technologies for removing VOCs.
[0003] The main technical core of the catalytic oxidation method is to design and prepare efficient catalysts. At present, the catalyst used in the catalytic oxidation method is mainly commercial Pd / Al2O3, but the water resistance of the catalyst is poor, the catalytic activity is reduced under water conditions, and the adsorption performance is also weak. Moreover, the catalyst needs to be at a higher temperature to show the corresponding activity. Long-term exposure to high temperature conditions will cause the catalyst to sinter and the active metal center to aggregate, resulting in reduced catalytic activity. Moreover, Pd is a precious metal and has high cost. Using composite metal oxide catalysts instead of precious metal catalysts can reduce the temperature and cost of catalytic oxidation to a certain extent. However, the existing composite metal oxide catalysts have poor water resistance, and the active sites are easily combined with water molecules, resulting in reduced catalytic ability of the catalyst to VOCs, and poor adsorption performance.
[0004] The prior art discloses a low-temperature SCR catalyst, the carrier of which is a composite of titanium dioxide and silicon dioxide, and the active components include manganese oxide and pre-sulfurized cerium trioxide, which has certain water resistance, but its specific surface area is low and cannot take into account the adsorption performance of the composite metal oxide catalyst at the same time. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing composite metal oxide catalysts that cannot simultaneously take into account low-temperature catalytic activity, water resistance and adsorption performance, and to provide a composite metal oxide catalyst, in which manganese oxide and cerium oxide are encapsulated in an all-silicon molecular sieve, and the content of the active component is controlled, while the ratio of manganese element to cerium element is adjusted, so as to achieve the simultaneous improvement of low-temperature catalytic activity, water resistance and adsorption performance.
[0006] Another object of the present invention is to provide a method for preparing the composite metal oxide catalyst.
[0007] Another object of the present invention is to provide use of the composite metal oxide catalyst in treating volatile organic compounds.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A composite metal oxide catalyst comprises an active component and a carrier, wherein the active components of the composite metal oxide catalyst are manganese oxide and cerium oxide, and the carrier is an all-silicon molecular sieve;
[0010] The manganese oxide and cerium oxide are encapsulated in an all-silicon molecular sieve;
[0011] The mass content of active components in the composite metal oxide catalyst is 6-15%, wherein the mass ratio of manganese element to cerium element is (1-2):(2-1).
[0012] It should be noted that:
[0013] The carrier of the composite metal oxide catalyst of the present invention is an all-silicon molecular sieve, which is obtained by crystallization of silica balls. Its rich pore structure and high specific surface area improve the dispersibility of the active components, so that the active components are highly dispersed, and at the same time improve the adsorption performance of the composite metal oxide catalyst. After the active components manganese oxide and cerium oxide are highly dispersed in the all-silicon molecular sieve, the active sites of the composite metal oxide catalyst are increased, and the control of the content of the active components makes the competitive adsorption of water vapor have less effect on the adsorption performance of the catalyst, and the catalytic activity is increased. The all-silicon molecular sieve is a hydrophobic molecular sieve. The present invention encapsulates the active components manganese oxide and cerium oxide in the all-silicon molecular sieve, which can also reduce the adsorption of water vapor by the active components and improve water resistance.
[0014] Specifically, among the active components, the total mass content of manganese oxide and cerium oxide encapsulated in the all-silicon molecular sieve is ≥50%.
[0015] When the content of active components in the composite metal oxide catalyst is too low, the active sites are reduced, and when it is too high, metal aggregation will occur, both of which will reduce the catalytic activity and water resistance. Specifically, the content of the carrier all-silicon molecular sieve in the composite metal oxide catalyst is 85-94%.
[0016] In addition, the active components of the composite metal oxide catalyst, manganese oxide and cerium oxide, will form a manganese-cerium metal composite oxide, such as a manganese-cerium solid solution, and redox coupling will occur between manganese and cerium, such as tetravalent manganese is reduced to trivalent manganese, and trivalent cerium is oxidized to tetravalent cerium. This process will form oxygen vacancies, provide gaseous oxygen adsorption and activation, and then promote the degradation of VOCs, so that the composite metal oxide catalyst still has good catalytic oxidation performance under low temperature conditions. In addition, a small amount of water vapor adsorbed on the composite metal oxide catalyst will produce active hydroxyl oxygen species, further promoting catalytic oxidation efficiency. Therefore, controlling the molar ratio of manganese element to cerium element in the active component can improve the low-temperature catalytic performance of the composite metal oxide catalyst and further improve the catalytic activity.
[0017] Specifically, the mass ratio of the manganese element to the cerium element can be 1:1, 2:1, 1:2, and preferably 1:1.
[0018] More than half of the manganese oxide and cerium oxide in the composite metal oxide catalyst of the present invention are encapsulated inside the all-silicon molecular sieve, and the rest are loaded on the surface of the all-silicon molecular sieve, thereby achieving a highly dispersed effect. At the same time, the pore structure of the all-silicon molecular sieve can expose more active sites, and the adsorption of VOCs by the all-silicon molecular sieve can directly cause in-situ catalytic oxidation reaction, thereby improving the catalytic activity and catalytic efficiency of the catalyst.
[0019] Specifically, the mass content of the active components in the composite metal oxide catalyst may be 6%, 10%, 12%, 14%, or 15%.
[0020] Preferably, the mass content of the active component in the composite metal oxide catalyst is 10-14%, more preferably 10-12%, and even more preferably 12%.
[0021] Specifically, the specific surface area of the all-silicon molecular sieve is 300 to 450 m 2 / g, for example, 300m 2 / g, 350m 2 / g, 400m 2 / g, 420m 2 / g, 430m 2 / g, 450m 2 / g.
[0022] Preferably, the specific surface area of the all-silicon molecular sieve is 400-430 m 2 / g, more preferably 420m 2 / g.
[0023] By controlling the specific surface area of the all-silicon molecular sieve, it is beneficial to highly disperse the active components manganese oxide and cerium oxide in the all-silicon molecular sieve, while further improving the adsorption of the catalyst.
[0024] The present invention specifically protects a method for preparing the composite metal oxide catalyst, comprising the following steps:
[0025] S1. Adding lower alcohol and ammonia water to a mixed solution of manganese salt and cerium salt, mixing evenly to obtain a suspension; the volume ratio of the mixed solution of lower alcohol, manganese salt and cerium salt to ammonia water is (70-80):3:4; the total concentration of manganese ions and cerium ions in the mixed solution is 0.1 mol / L-0.8 mol / L;
[0026] S2. Add a silicon source to the suspension obtained in S1. After the silicon source is completely hydrolyzed, the obtained suspension is dried to obtain a precursor;
[0027] S3. Add tetrapropylammonium hydroxide to the precursor obtained in S2, mix well and then crystallize; the mass ratio of tetrapropylammonium hydroxide to the precursor is (0.5 to 1.5):1; the crystallization temperature is 100 to 200°C;
[0028] S4. calcining the product obtained by crystallization in S3 to obtain a composite metal oxide catalyst; the calcination temperature is 500-800°C.
[0029] The lower alcohol in step S1 of the present invention is a solvent, specifically one of methanol, ethanol, n-propanol and n-butanol. The choice of solvent will affect the particle size of the silica spheres obtained in step S2.
[0030] The silicon source in step S2 undergoes two reactions, hydrolysis and polycondensation, in the suspension, and the silica spheres formed by the polycondensation are used in the subsequent transformation of silica into an all-silicon molecular sieve; the hydrolysis and polycondensation reactions are the processes in which the silicon source and water react to generate silica. In this process, increasing the water / silicon source ratio (i.e., the water-silicon ratio) can promote hydrolysis, but too large a water-silicon ratio will cause the already generated silicon-oxygen bonds to break, making it impossible to form silica spheres, encapsulate manganese ions and cerium ions, and even more impossible to transform into an all-silicon molecular sieve. Therefore, it is necessary to control the balance between the hydrolysis reaction and the polycondensation reaction in this process.
[0031] The ammonia water in step S1 acts as an alkaline catalyst. In addition to being able to control the particle size of the formed silicon dioxide, it can also inhibit the hydrolysis of the silicon source during the reaction, which is beneficial to the occurrence of the polycondensation reaction and the formation of silicon dioxide particles with regular shapes.
[0032] Specifically, the mass fraction of the ammonia water is 5 to 25%.
[0033] The mass fraction of ammonia water will affect the hydrolysis and condensation rate of the silicon source, thereby affecting the morphology of silica.
[0034] The volume ratio of the mixed solution of low-level alcohol, manganese salt and cerium salt to ammonia water in step S1 will affect the morphology and pore structure of the silicon dioxide generated by the reaction. If the ratio of manganese salt to cerium salt is too large, the all-silicon molecular sieve structure cannot be successfully formed, thereby affecting the catalytic activity and adsorption performance of the composite metal oxide catalyst. Controlling the concentration of manganese ions and cerium ions in the mixed solution is the key to controlling the content of active components in the composite metal oxide catalyst. If the concentration is too low, the content of active components is insufficient. If the concentration is too high, the silicon dioxide will be incompletely transformed or even fail to transform, and the all-silicon molecular sieve carrier cannot be formed.
[0035] Specifically, the volume ratio of the mixed solution of the lower alcohol, manganese salt and cerium salt to the ammonia water can be 70:3:4, 75:3:4, or 80:3:4.
[0036] In step S2, whether the silicon source is completely hydrolyzed and polycondensed will directly affect the structure of the catalyst; the drying process is to remove the residual low-grade alcohol solution and ammonia water to make the precursor a dry solid.
[0037] Specifically, the volume ratio of the silicon source to the lower alcohol in S1 is 3:(70-80).
[0038] Specifically, the silicon source is one of tetraethyl orthosilicate, silica sol and water glass.
[0039] The conditions of the silicon source hydrolysis process are: stirring at 20-95° C. and hydrolyzing for 0.5-48 hours.
[0040] Specifically, the drying temperature is 80-100° C. and the drying time is 0.2-12 hours.
[0041] Specifically, the silicon dioxide obtained by polycondensation of the silicon source has a spherical structure.
[0042] The manganese ions and cerium ions need to be encapsulated in silicon dioxide first, and then crystallized and calcined. This encapsulation belongs to core-shell encapsulation. The use of spherical silicon dioxide is conducive to the core-shell encapsulation of manganese oxide and cerium oxide in all-silicon molecular sieves.
[0043] The tetrapropylammonium hydroxide added in step S3 acts as a guiding agent and a template agent, guiding the silicon dioxide to be crystallized into a full silicon molecular sieve during the crystallization process, and the mass ratio of the tetrapropylammonium hydroxide to the precursor directly affects whether the silicon dioxide can be crystallized into a full silicon molecular sieve. In addition, the crystallization in step S3 adopts a steam dry gel crystallization method, and the crystallization temperature is also a key factor in whether the silicon dioxide can be recrystallized into a full silicon molecular sieve. Too high or too low a temperature will lead to incomplete crystallization or even crystallization failure, and the pore structure and packaging morphology of the full silicon molecular sieve will be affected, reducing the dispersion and adsorption performance of manganese oxide and cerium oxide; specifically, the mass ratio of the tetrapropylammonium hydroxide to the precursor can be 0.5:1, 0.75:1, 1:1, 1.33:1, 1.5:1.
[0044] Preferably, the mass ratio of tetrapropylammonium hydroxide to the precursor is (1-1.5):1, more preferably 1.33:1.
[0045] The tetrapropylammonium hydroxide and the precursor are mixed by grinding for a total of 10 to 20 minutes.
[0046] Specifically, the crystallization temperature may be 100°C, 110°C, 120°C, 130°C, 150°C, 160°C, or 200°C.
[0047] The calcination time and temperature in step S4 will affect the oxidation of manganese ions and cerium ions, as well as the dispersibility of the obtained manganese oxide and cerium oxide and the removal of tetrapropylammonium hydroxide. Too high a temperature will cause the active components to aggregate, reduce the active sites, and reduce the catalytic activity; too low a temperature will not completely remove tetrapropylammonium hydroxide, resulting in impurities on the surface of the all-silicon molecular sieve, and even the inability to completely oxidize manganese ions and cerium ions, reducing the catalytic efficiency of the composite metal oxide catalyst.
[0048] Specifically, the calcination temperature may be 500°C, 600°C, 650°C, 700°C, 750°C, or 800°C, preferably 650-750°C, and more preferably 700°C.
[0049] Specifically, the manganese salt in step S1 is one or more of manganese nitrate, manganese chloride and manganese sulfate.
[0050] Specifically, the cerium salt in step S1 is cerium nitrate or cerium sulfate.
[0051] Specifically, the preparation method of the mixed solution of manganese salt and cerium salt can be referred to as follows:
[0052] Add manganese salt and cerium salt into deionized water and dissolve them at 20-80°C.
[0053] Specifically, the total concentration of manganese ions and cerium ions in the mixed solution of step S1 is 0.2 mol / L to 0.6 mol / L, preferably 0.4 mol / L to 0.5 mol / L.
[0054] Further controlling the total concentration of manganese ions and cerium ions can control the content of metal ions, which is beneficial to the encapsulation of metal ions by silica balls.
[0055] Specifically, the crystallization time in step S3 is 12 to 72 hours, preferably 40 to 50 hours, and more preferably 48 hours.
[0056] By combining the crystallization time and the crystallization temperature, the structure of the silica all-silicon molecular sieve can be better controlled.
[0057] Preferably, the crystallization temperature in step S3 is 110-130° C., more preferably 120 h.
[0058] Specifically, the calcination time in step S4 is 0.2 to 12 hours, preferably 3 to 5 hours, and more preferably 4 hours.
[0059] By adjusting the calcination time and temperature, the removal of tetrapropylammonium hydroxide can be better controlled while ensuring that the active components do not aggregate.
[0060] The present invention particularly protects the use of the composite metal oxide catalyst in treating volatile organic compounds.
[0061] The active components in the composite metal oxide catalyst of the present invention are highly dispersed, and the redox coupling between manganese and cerium forms oxygen vacancies, which promotes the in-situ catalytic oxidation degradation of VOCs, and the catalyst has good low-temperature catalytic oxidation performance, which can further prevent the active components from aggregating during the catalytic process and causing the catalyst to deactivate. In addition, the composite metal oxide catalyst of the present invention has excellent water resistance, and the catalytic activity does not decrease or even increases under conditions containing water vapor.
[0062] Specifically, the composite metal oxide catalyst is assembled in a regenerative catalytic combustion device or a catalytic oxidation combustion device for VOCs to be treated for use.
[0063] Compared with the prior art, the present invention has at least the following beneficial effects:
[0064] The present invention provides a composite metal oxide catalyst and a preparation method and application thereof. Manganese oxide and cerium oxide are encapsulated in silicon dioxide balls by a modified Stober process, and a full silicon molecular sieve is formed by crystallization. The contents of manganese oxide and cerium oxide, as well as the ratio of manganese element to cerium element are controlled, so that the low-temperature thermal catalytic activity, water resistance and adsorption performance of the composite metal oxide catalyst are simultaneously improved, so that the composite metal oxide catalyst has the functions of adsorption enrichment and in-situ catalytic degradation of VOCs.
[0065] The composite metal oxide catalyst of the present invention catalyzes the oxidation of VOCs in the presence of 10 vol.% H2O(g) of water vapor. When the conversion rate of VOCs reaches 90%, the temperature does not exceed 250°C, and the water resistance and low-temperature catalytic performance are good. In addition, the composite metal oxide catalyst adsorbs VOCs, and the time for VOCs to penetrate the catalyst and be released again is not less than 30 minutes, and the adsorption performance is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 This is a scanning electron microscope image of the entire composite metal oxide catalyst of Example 1.
[0067] Figure 2 This is a local scanning electron microscope image of the composite metal oxide catalyst of Example 1.
[0068] Figure 3 The figure is a comparison chart of the acetone degradation efficiency of the catalysts of Example 1 and Comparative Example 1.
[0069] Figure 4 It is a comparison diagram of the adsorption curves of acetone by the catalysts of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0070] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0071] Example 1
[0072] A composite metal oxide catalyst comprises an active component and a carrier, wherein the active components of the composite metal oxide catalyst are manganese oxide and cerium oxide, and the carrier is an all-silicon molecular sieve;
[0073] The specific surface area of the all-silicon molecular sieve is 420m 2 / g;
[0074] The manganese oxide and cerium oxide are encapsulated in an all-silicon molecular sieve;
[0075] In the composite metal oxide catalyst, the mass content of active components is 12%, wherein the mass ratio of manganese element to cerium element is 1:1; and the mass content of all-silicon molecular sieve is 88%.
[0076] The preparation method of the composite metal oxide catalyst can refer to the following steps:
[0077] S1. adding anhydrous ethanol and ammonia water to a mixed solution of manganese nitrate and cerium nitrate hexahydrate, and stirring for 2 hours at 35° C. to completely precipitate manganese ions and cerium ions in the mixed solution to obtain a suspension; wherein the volume ratio of the anhydrous ethanol, manganese salt and cerium salt mixed solution to ammonia water is 80:3:4;
[0078] S2. Slowly add 6 mL of tetraethyl orthosilicate to the suspension obtained in S1, and continue stirring at 35°C for 24 hours to hydrolyze the tetraethyl orthosilicate to obtain a silicon dioxide precipitate to obtain a suspension, and place the suspension in an oven at 100°C and dry for 12 hours to obtain a precursor; the volume ratio of the anhydrous ethanol in S1 to the tetraethyl orthosilicate in S2 is 80:3;
[0079] S3. Tetrapropylammonium hydroxide was added to the precursor obtained in S2, and after grinding in a mortar for 15 minutes, it was added to a polytetrafluoroethylene reactor for crystallization; the mass ratio of tetrapropylammonium hydroxide to the precursor was 1.33:1; the crystallization temperature was 120°C; and the crystallization time was 48 hours;
[0080] S4. The product obtained by crystallization in S3 is calcined to obtain a composite metal oxide catalyst; the calcination temperature is 700°C and the calcination time is 4h;
[0081] The steps of mixing manganese nitrate and cerium nitrate hexahydrate in S1 are:
[0082] Manganese nitrate and cerium nitrate hexahydrate were added to 6 mL of deionized water and stirred to dissolve at 35° C. to obtain a mixed solution with a total concentration of manganese ions and cerium ions of 0.467 mol / L.
[0083] Embodiments 2 to 8
[0084] A composite metal oxide catalyst, the structure and composition are the same as those in Example 1, and the differences are shown in Table 1.
[0085] Table 1. Structural parameters of composite metal oxide catalysts
[0086]
[0087]
[0088] Note: The mass content of all-silicon molecular sieve in the catalyst of each example in Table 1 above = 1 - the mass content of active component.
[0089] The preparation steps of the composite metal oxide catalysts in the above-mentioned embodiments in Table 1 are the same as those in Embodiment 1, and the differences are shown in Table 2.
[0090] Table 2. Preparation parameters of composite metal oxide catalysts
[0091]
[0092] Example 9
[0093] A method for preparing a composite metal oxide catalyst, the steps are the same as those in Example 1, except that the manganese nitrate in step S1 is replaced by manganese sulfate.
[0094] Example 10
[0095] A method for preparing a composite metal oxide catalyst, the steps are the same as those of Example 1, except that the cerium nitrate hexahydrate in step S1 is replaced by cerium sulfate tetrahydrate.
[0096] Embodiment 11
[0097] A method for preparing the composite metal oxide catalyst described in Example 1 has the same steps as Example 1, except that in step S3, the crystallization temperature is 100°C and the time is 72h; the calcination temperature is 500°C and the time is 12h.
[0098] Example 12
[0099] A method for preparing the composite metal oxide catalyst described in Example 1 has the same steps as Example 1, except that in step S3, the crystallization temperature is 110° C. and the time is 50 h; the calcination temperature is 650° C. and the time is 5 h.
[0100] Example 13
[0101] A method for preparing the composite metal oxide catalyst described in Example 1 has the same steps as Example 1, except that in step S3, the crystallization temperature is 130° C. and the time is 40 h; the calcination temperature is 750° C. and the time is 3 h.
[0102] Embodiment 14
[0103] A method for preparing the composite metal oxide catalyst described in Example 1 has the same steps as Example 1, except that in step S3, the crystallization temperature is 200°C and the time is 24h; the calcination temperature is 800°C and the time is 1h.
[0104] Comparative Example 1
[0105] A carrier-free manganese-cerium composite metal oxide catalyst has a plate aggregation structure.
[0106] The preparation method of the above manganese-cerium composite metal oxide catalyst can refer to the following steps:
[0107] S1. Dissolve cerium nitrate hexahydrate and manganese nitrate in 50 ml of deionized water, wherein the ratio of manganese ions to cerium ions is 1:1, and then add citric acid monohydrate (CA) to the solution, wherein the molar ratio of CA / (Mn+Ce) is maintained at 1.2;
[0108] S2. After the citric acid monohydrate is completely dissolved, the mixture is heated to 80°C in a water bath and maintained at this temperature with stirring until a gel is formed;
[0109] S3. The gel obtained in S2 was dried in an oven at 120°C overnight to obtain a sponge-like material, which was calcined in a muffle furnace at 200°C for 2 hours, and then raised to 700°C at a rate of 2°C / min and calcined for 2 hours to obtain an unsupported manganese-cerium composite metal oxide catalyst.
[0110] Comparative Example 2
[0111] A method for preparing a composite metal oxide catalyst, the steps are the same as those of Example 1, except that cerium nitrate hexahydrate is not added in step S1.
[0112] Comparative Example 3
[0113] A method for preparing a composite metal oxide catalyst, the steps are the same as those of Example 1, except that manganese nitrate is not added in step S1.
[0114] Comparative Example 4
[0115] A composite metal oxide catalyst has the same structure and components as those in Example 1, except that, in the active components of the composite metal oxide catalyst, the mass ratio of manganese element to cerium element is 1:3.
[0116] The preparation method of the above catalyst is the same as that of Example 1.
[0117] Comparative Example 5
[0118] A composite metal oxide catalyst, the components of which are the same as those of Example 1, except that the carrier of the composite metal oxide catalyst is silicon dioxide.
[0119] The preparation method of the above catalyst is the same as that of Example 1, except that step S3 is not performed and the calcination temperature in step S4 is 550°C.
[0120] Results
[0121] (1) Low temperature catalytic performance test:
[0122] 80 mg of the catalysts of the above-mentioned embodiments and comparative examples were taken and tested in a fixed-bed continuous flow quartz reactor. Before the test, the catalysts were purged with air at 300°C for 2 hours to dry and activate the catalysts. The composition of the reaction gas was: acetone was bubbled with air, and air was used as a diluent to obtain 1000 ppm acetone gas. The mass space velocity during the reaction was 60000 mL / min. cat. -1 h -1 .
[0123] The above catalytic reaction was carried out at 100-300°C, with a heating rate of 1°C / min, and the temperature T of the catalyst when the acetone conversion rate reached 90% was recorded. 90-1 The lower the temperature, the better the low-temperature catalytic performance.
[0124] (2) Water resistance test:
[0125] The specific test method is the same as (1) low temperature catalytic performance test, except that 10 vol.% H2O (g) water vapor is introduced into the reaction gas, and the temperature T when the catalyst reaches 90% conversion rate of acetone is recorded. 90 -2. The lower the temperature, the higher the catalytic activity of the catalyst in the presence of water vapor, that is, the better the water resistance.
[0126] In addition, the catalyst of Example 1 was taken to carry out water resistance test at different water vapor contents. The specific test method was the same as above, except that water vapor with contents of 3 vol.% H2O(g), 5 vol.% H2O(g), 7 vol.% H2O(g), and 10 vol.% H2O(g) were introduced into the reaction gas, respectively.
[0127] (3) Adsorption performance test:
[0128] 80 mg of each catalyst of the above embodiments and comparative examples were taken and placed in a reaction tube filled with 1000 ppm acetone at a flow rate of 70 ml / min. At 30° C., the reaction tube was switched from an empty state to a reaction tube filled with catalyst and timing was started. At the same time, the acetone concentration at the tail end of the reaction tube was collected online until the acetone concentration returned to the initial concentration. Timing was stopped to obtain the adsorption penetration time from the catalyst adsorbing acetone to the release of acetone. The mass space velocity during the reaction was 60000 mL / g cat. -1 h -1 The longer the adsorption penetration time is, the better the adsorption performance of the catalyst is.
[0129] The results are shown in Table 3.
[0130] Table 3. Catalytic performance of composite metal oxide catalysts
[0131] <![CDATA[T 90-1 (℃)]]> <![CDATA[T 90-2 (℃)]]> Adsorption penetration time (min) Example 1 179 178 45 Example 2 225 220 30 Example 3 195 197 35 Example 4 185 182 40 Example 5 202 206 35 Example 6 210 212 32 Example 7 205 205 42 Example 8 198 198 42 Example 9 186 188 45 Example 10 180 182 45 Embodiment 11 185 183 40 Example 12 182 184 42 Example 13 192 190 42 Embodiment 14 204 208 42 Comparative Example 1 209 240 15 Comparative Example 2 255 250 30 Comparative Example 3 272 270 32 Comparative Example 4 240 242 34 Comparative Example 5 342 354 22
[0132] As can be seen from Table 3, the temperature of the composite metal oxide catalyst of the present invention is lower than 250°C when the conversion rate reaches 90%, and it has low-temperature thermal catalytic performance. After introducing 10 vol.% H2O (g) of water vapor into the reaction gas, the temperature corresponding to the 90% conversion rate remains basically unchanged, indicating that the composite metal oxide catalyst of the present invention also has excellent water resistance. At the same time, in the adsorption performance test, the penetration time of acetone on the catalyst of the present invention is more than 30 minutes, and the adsorption performance of the catalyst is good. In Examples 11 to 14, the crystallization conditions and calcination conditions of the composite metal oxide catalyst described in Example 1 are changed. Since the change of the crystallization temperature will lead to different crystallinity of the final all-silicon molecular sieve, different pore structures, and different numbers of exposed active sites, and the calcination temperature will affect the dispersibility of the active components, the final composite metal oxide catalyst has different activities. That is, there are differences in low-temperature catalytic performance and water resistance; in Comparative Example 2, a single manganese oxide is used, and in Comparative Example 3, the active component is a single cerium oxide, and the catalytic activity of the obtained catalyst is reduced. In the low-temperature performance test and the water resistance test, the temperature corresponding to 90% conversion rate is above 250°C; in Comparative Example 4, the mass ratio of manganese to cerium exceeds the scope of the technical solution of the present invention, and the catalytic activity of the catalyst is also reduced; the manganese-cerium composite metal oxide catalyst in Comparative Example 1 is a carrier-free manganese-cerium composite metal oxide catalyst, and the addition of CA is only to adjust the structure of the catalyst so that it has gaps and will not aggregate into stone-like shapes, but has plate-like shapes, but its water resistance and adsorption properties are worse than those of the composite metal oxide catalyst of the present invention; the carrier of the catalyst described in Comparative Example 5 is silicon dioxide, which is not crystallized into all-silicon molecular sieve, and the low-temperature catalytic performance, water resistance and adsorption performance of the final catalyst are all low.
[0133] The catalytic efficiency of the composite metal oxide catalyst of Example 1 at different water vapor contents and different temperatures is as follows: When the water vapor content is 3 vol.% H2O (g), T 90 Temperature is 169℃, 5vol.%H2O(g) 90 Temperature is 172℃, 7vol.%H2O(g) 90 Temperature 175℃, 10vol.%H2O(g) 90 The temperature is 178℃. As the water vapor content increases, T 90 Although it increased, the amplitude did not exceed 10°C, which further illustrates that the composite metal oxide catalyst of the present invention has good water resistance.
[0134] Figure 1 This is a scanning electron microscope image of the composite metal oxide catalyst of Example 1. Figure 2is a stacked scanning electron microscope image of the composite metal oxide catalyst of Example 1, from Figure 1 and Figure 2 It can be seen that the catalyst has the characteristic morphology of silicon-1 (all-silicon molecular sieve), indicating that the silicon dioxide is successfully transformed into an all-silicon molecular sieve. At the same time, the manganese-cerium composite metal oxide on the outer surface of the molecular sieve is evenly distributed without aggregation, indicating that the metal is well dispersed.
[0135] Figure 3 1 is a comparison chart of the acetone degradation efficiency of the catalysts of Example 1 and Comparative Example 1. It can be seen from the figure that the catalyst of Example 1 (black curve) has a T of 90% conversion rate. 90 The temperature is 179°C, while the catalyst of Comparative Example 1 (gray curve) T 90 The temperature is 209° C., indicating that the catalyst of Example 1 of the present invention has better low-temperature catalytic activity than that of Comparative Example 1.
[0136] Figure 4 It is a comparison diagram of the adsorption curves of acetone by the catalysts of Example 1 and Comparative Example 1. It can be seen from the figure that the adsorption penetration time of the catalyst of Experimental Example 1 (black line) is 45 minutes, which is much longer than the adsorption time of 15 minutes of the catalyst of Comparative Example 1 (gray line), indicating that the composite metal oxide catalyst of Example 1 of the present invention contains an all-silicon molecular sieve structure, and has better adsorption performance than the catalyst of Comparative Example 1 that does not contain an all-silicon molecular sieve structure.
[0137] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a composite metal oxide catalyst, characterized in that: The steps include: S1. Adding lower alcohol and ammonia water to a mixed solution of manganese salt and cerium salt, and mixing them evenly to obtain a suspension; the volume ratio of the mixed solution of lower alcohol, manganese salt and cerium salt to ammonia water is (70-80):3:4; the total concentration of manganese ions and cerium ions in the mixed solution is 0.1 mol / L-0.8 mol / L; the mass fraction of ammonia water is 5-25%; the manganese salt is one or more of manganese nitrate, manganese chloride and manganese sulfate; the cerium salt is cerium nitrate or cerium sulfate; S2. Add a silicon source to the suspension obtained in S1. After the silicon source is completely hydrolyzed, dry the obtained suspension to obtain a precursor; the volume ratio of the silicon source to the lower alcohol in S1 is 3:(70-80); the silicon source is one of tetraethyl orthosilicate, silica sol, and water glass; S3. Add tetrapropylammonium hydroxide to the precursor obtained in S2, mix well and then crystallize; the mass ratio of tetrapropylammonium hydroxide to the precursor is (0.5~1.5):1; the crystallization temperature is 100~200°C; S4. The crystallized product obtained in S3 is calcined to obtain a composite metal oxide catalyst; the calcination temperature is 500 to 800 ° C; The active components of the composite metal oxide catalyst are manganese oxide and cerium oxide, and the carrier is an all-silicon molecular sieve; The manganese oxide and cerium oxide are encapsulated in an all-silicon molecular sieve; The mass content of active components in the composite metal oxide catalyst is 6-15%, wherein the mass ratio of manganese element to cerium element is (1-2):(2-1).
2. The preparation method according to claim 1, characterized in that: The mass content of active components in the composite metal oxide catalyst is 10-14%.
3. The preparation method according to claim 1, characterized in that: The specific surface area of the all-silicon molecular sieve is 300-450 m 2 / g.
4. The preparation method according to claim 1, characterized in that: The specific surface area of the all-silicon molecular sieve silicon is 400-430m 2 / g.
5. The preparation method according to claim 1, characterized in that: The total concentration of manganese ions and cerium ions in the mixed solution of step S1 is 0.2 mol / L to 0.6 mol / L.
6. The preparation method according to claim 1, characterized in that: The crystallization time in step S3 is 12 to 72 hours.
7. The preparation method according to claim 1, characterized in that: The crystallization temperature in step S3 is 110-130°C.
8. The preparation method according to claim 1, characterized in that: The calcination time in step S4 is 0.2 to 12 hours.
9. Use of the composite metal oxide catalyst prepared by the preparation method according to any one of claims 1 to 4 in treating volatile organic compounds.