Ortho-cresol isomerization catalyst and preparation method thereof and ortho-cresol isomerization method
By using modified catalysts prepared by composite molecular sieve and alumina, the problems of poor catalytic performance and complex equipment are solved, and efficient catalytic performance and long-life catalysts are achieved, which are suitable for industrial applications.
Patent Information
- Application Number
- CN202111280371.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The existing o-cresol isomerization catalysts have poor catalytic performance, poor product selectivity, insufficient stability, and complex traditional process equipment, difficult operation, and high production costs.
The catalyst is prepared using 50-90 parts by weight of composite molecular sieve, 10-50 parts by weight of alumina and 0.5-8 parts by weight of modified elements. The catalyst is formed by alkali treatment, molding and multi-stage calcination to form a catalyst with rich pore structure, suitable for fixation Bed craftsmanship.
It improves the activity and stability of the catalyst, enhances the selectivity of p-cresol and m-cresol, has a long life span, and is suitable for industrial promotion.
Smart Images

Figure BDA0003329276080000121 
Figure BDA0003329276080000122 
Figure BDA0003329276080000123
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of isomerization catalysts, and in particular to an o-cresol isomerization catalyst and a preparation method thereof, and an o-cresol isomerization method. Background Art
[0002] p-Cresol and m-Cresol are important chemical raw materials. Currently, they are in short supply in China and need to be imported in large quantities to meet domestic market demand.
[0003] The traditional method for preparing o-cresol is a natural separation method, that is, distilling o-cresol from coal tar, because the by-product coal tar phenol in coal coking and city gas production contains about 30% phenol, 10%-13% o-cresol, 14%-18% m-cresol, 9%-12% p-cresol, and 13%-15% xylenol. The o-cresol can be recovered by separation. However, the raw materials of this method are non-renewable resources and cannot meet the requirements of sustainable development.
[0004] The production of m-p-cresol by isomerization of o-cresol has the advantages of high selectivity, few by-products, good atom economy, and low environmental pollution, and has great application prospects. However, the current o-cresol isomerization production process generally has the following problems: 1) the catalyst activity is low, the product selectivity is poor, and the stability needs to be improved; 2) the moving bed or fluidized bed process is mostly used, which has complex equipment, difficult operation, and high production cost.
[0005] Therefore, there is an urgent need to provide an o-cresol isomerization catalyst that can be used in a fixed bed process and has high catalyst activity, good product selectivity, and long catalyst service life. Summary of the invention
[0006] The purpose of the present invention is to solve the technical problem that the catalytic performance of an o-cresol isomerization catalyst is poor, and to provide an o-cresol isomerization catalyst and a preparation method thereof, as well as an o-cresol isomerization method.
[0007] In order to achieve the above-mentioned object, the first aspect of the present invention provides an o-cresol isomerization catalyst, which comprises 50-90 parts by weight of a composite molecular sieve, 10-50 parts by weight of alumina and 0.5-8 parts by weight of a modifying element; wherein the composite molecular sieve comprises a nano HZSM-5 molecular sieve and a nano IM-5 molecular sieve, and the modifying element is selected from one or more of F, Cl and P.
[0008] The second aspect of the present invention provides a method for preparing the o-cresol isomerization catalyst according to the first aspect of the present invention, the method comprising the following steps:
[0009] (1) mixing a mixed powder containing nano HZSM-5 molecular sieve and nano IM-5 molecular sieve with an alkali solution for alkali treatment to obtain an alkali-modified mixed powder;
[0010] (2) mixing the alkali-modified mixed powder, the alumina precursor and the optional nitric acid and then molding them to obtain molded particles, and then calcining the molded particles for the first time to obtain a calcined product;
[0011] (3) The calcined product is mixed with a solution containing a modifying element precursor and then impregnated, then dried to obtain an impregnated product, and then the impregnated product is calcined for a second time to obtain the o-cresol isomerization catalyst.
[0012] The third aspect of the present invention provides a method for isomerizing o-cresol, which comprises contacting o-cresol with the o-cresol isomerization catalyst described in the first aspect of the present invention or the o-cresol isomerization catalyst prepared by the preparation method described in the second aspect of the present invention to carry out an isomerization reaction to obtain p-cresol and m-cresol.
[0013] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:
[0014] 1) The o-cresol isomerization catalyst provided by the present invention uses nano HZSM-5 molecular sieve and nano IM-5 molecular sieve as active components, and uses a modifying element to modify the catalyst. At the same time, by performing alkali treatment and variable temperature calcination during the preparation process, an o-cresol isomerization catalyst with rich pore structure and large specific surface area can be obtained, so that the o-cresol isomerization catalyst can not only have a high o-cresol conversion rate and m-cresol yield, but also has high stability of the catalyst, can be regenerated for multiple times, and has a long catalyst life;
[0015] 2) The preparation method of the o-cresol isomerization catalyst provided in the present invention is applicable to a fixed bed, is simple to operate, and is suitable for industrial promotion. DETAILED DESCRIPTION
[0016] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0017] The first aspect of the present invention provides an o-cresol isomerization catalyst, which comprises 50-90 parts by weight of a composite molecular sieve, 10-50 parts by weight of alumina and 0.5-8 parts by weight of a modifying element; wherein the composite molecular sieve comprises a nano HZSM-5 molecular sieve and a nano IM-5 molecular sieve, and the modifying element is selected from one or more of F, Cl and P.
[0018] In a preferred embodiment, the catalyst comprises 60-80 parts by weight of a composite molecular sieve, 20-40 parts by weight of alumina and 1-6 parts by weight of a modifying element.
[0019] In the present invention, although nano HZSM-5 molecular sieve and nano IM-5 molecular sieve also contain alumina, the content of alumina defined in the present invention when describing the composition of the catalyst refers to the content of alumina outside the composite molecular sieve, and does not include the content of alumina in the nano HZSM-5 molecular sieve and nano IM-5 molecular sieve. The content of composite molecular sieve and alumina in the catalyst in the present invention is the feed amount in the preparation process. The content of the modifying element in the catalyst in the present invention is measured by element mass and can be analyzed by X-ray fluorescence spectroscopy.
[0020] In a preferred embodiment, the grain size of the nano HZSM-5 molecular sieve is 20-200 nm, preferably 30-100 nm; the molar ratio of silicon dioxide / aluminum oxide in the nano HZSM-5 molecule is 15-100:1, preferably 30-70:1.
[0021] In a preferred embodiment, the crystal size of the nano IM-5 molecular sieve is 20-200 nm, preferably 50-200 nm; the molar ratio of silicon dioxide to aluminum oxide in the nano IM-5 molecular sieve is 20-80:1, preferably 30-60:1.
[0022] In a preferred embodiment, the nano IM-5 molecular sieve is a hydrogen-type nano IM-5 molecular sieve.
[0023] In a preferred embodiment, the mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 0.1-15:1, preferably 0.5-10:1, and more preferably 1-6:1.
[0024] In a preferred embodiment, the modifying element is selected from one of F, Cl, and P, preferably P.
[0025] In a preferred embodiment, the catalyst has a pore volume of 0.24-0.4 mL / g, preferably 0.26-0.38 mL / g, and a specific surface area of 320-450 m 2 / g, preferably 350-420m 2 / g.
[0026] The second aspect of the present invention provides a method for preparing the o-cresol isomerization catalyst according to the first aspect of the present invention, the method comprising the following steps:
[0027] (1) mixing a mixed powder containing nano HZSM-5 molecular sieve and nano IM-5 molecular sieve with an alkali solution for alkali treatment to obtain an alkali-modified mixed powder;
[0028] (2) mixing the alkali-modified mixed powder, the alumina precursor and the optional nitric acid and then molding them to obtain molded particles, and then calcining the molded particles for the first time to obtain a calcined product;
[0029] (3) The calcined product is mixed with a solution containing a modifying element precursor and then impregnated, then dried to obtain an impregnated product, and then the impregnated product is calcined for a second time to obtain the o-cresol isomerization catalyst.
[0030] In step (1):
[0031] In a preferred embodiment, the grain size of the nano HZSM-5 molecular sieve is 20-200 nm, preferably 30-100 nm; the molar ratio of silicon dioxide / aluminum oxide in the nano HZSM-5 molecule is 15-100:1, preferably 30-70:1.
[0032] In a preferred embodiment, the crystal size of the nano IM-5 molecular sieve is 20-200 nm, preferably 50-200 nm; the molar ratio of silicon dioxide to aluminum oxide in the nano HZSM-5 molecule is 20-80:1, preferably 30-60:1.
[0033] In a preferred embodiment, the nano IM-5 molecular sieve is a hydrogen-type nano IM-5 molecular sieve.
[0034] In a preferred embodiment, the mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 0.1-15:1, preferably 0.5-10:1, and more preferably 1-6:1.
[0035] In a preferred embodiment, the preparation method of the mixed powder comprises mixing the nano HZSM-5 molecular sieve and the nano IM-5 molecular sieve, ball milling with ethanol as a medium for 4-6 hours, and then drying at 90-120° C. for 2-6 hours.
[0036] In a preferred embodiment, the alkali in the alkali solution is selected from NaOH, KOH, Na 2 CO 3 and K 2 CO 3 One or more of the above, preferably NaOH and / or KOH.
[0037] In a preferred embodiment, the concentration of the alkali solution is 0.01-1 mol / L, preferably 0.05-0.2 mol / L.
[0038] In a preferred embodiment, the mass ratio of the mixed powder to the alkali solution is 1:4-10, preferably 1:5-7.
[0039] In a preferred embodiment, the operating conditions of the alkali treatment include: the alkali treatment temperature is 50-90°C, preferably 60-85°C; the alkali treatment time is 0.5-5h, 1-4h.
[0040] Among them, in the present invention, the alkali treatment is carried out under stirring conditions. Through the alkali treatment, the pore structure of the catalyst can be enriched, and the conversion rate of the catalyst and the selectivity of m-p-cresol can be improved.
[0041] In a preferred embodiment, the alkali-modified mixed powder is washed until the washing liquid becomes neutral, and then dried at 60-150° C. for 1-10 h.
[0042] In step (2):
[0043] In a preferred embodiment, the alumina precursor is selected from one or more of aluminum sol, aluminum gel, and pseudo-boehmite, preferably pseudo-boehmite.
[0044] In a preferred embodiment, based on the mass of oxides in the alumina precursor, the mass ratio of the alkali-modified mixed powder to the alumina precursor is 50-90:10-50, and more preferably 60-80:20-40.
[0045] In a preferred embodiment, the concentration of the nitric acid is 3-10 wt %, preferably 5-8 wt %.
[0046] In a preferred embodiment, the mass of the nitric acid is 20-55%, preferably 30-45%, of the total mass of the alkali-modified mixed powder and the alumina precursor, wherein the mass of the alumina precursor in the total mass of the alkali-modified mixed powder and the alumina precursor is calculated based on the total mass of the alumina precursor.
[0047] In a preferred embodiment, the molding is selected from compression molding, rolling molding, spray molding, and extrusion molding, preferably extrusion molding.
[0048] The present invention does not specifically limit the operating conditions of the molding, and the molding can be performed according to conventional operations in the art. The present invention also does not specifically limit the molding shape of the molded particles, which can be clover, four-leaf clover, cylindrical, hollow, etc. The specific shape can be selected according to actual needs.
[0049] In a preferred embodiment, before the shaped particles are subjected to the first calcination, the shaped particles are first dried, for example, at 60-150° C. for 1-10 h.
[0050] In a preferred embodiment, the operating conditions of the first calcination include: first calcining at 150-250°C for 1-10h, then calcining at 300-400°C for 1-10h, and then calcining at 500-600°C for 2-14h; preferably, first calcining at 180-220°C for 2-6h, then calcining at 330-370°C for 2-6h, and then calcining at 530-570°C for 4-8h.
[0051] Among them, in the present invention, the pore structure of the catalyst can be further improved by multi-stage variable temperature calcination, thereby improving the conversion rate of the catalyst and the selectivity of m-p-cresol.
[0052] In step (3):
[0053] In a preferred embodiment, the modifying element precursor is selected from one or more of an ammonium salt or acid containing P, an ammonium salt or acid containing F, and an ammonium salt or acid containing Cl; for example, the modifying element precursor is selected from (NH 4 ) 2 HPO 4 NH 4 )H 2 PO 4 , H 3 PO 4 NH 4 F, HF, NH 4 One or more of Cl, HCl.
[0054] In a preferred embodiment, the solvent in the solution containing the modifying element precursor is water, and the concentration of the modifying element precursor is 2-20 wt %, preferably 4-15 wt %.
[0055] In a preferred embodiment, the feed amounts of the calcined product and the solution containing the modifying element precursor are such that in the prepared catalyst, the mass ratio of the composite molecular sieve to the modifying element is 50-90:0.5-8, preferably 60-80:1-6.
[0056] Among them, in the present invention, the modifying element may be lost during the preparation process. In order to obtain a catalyst with a certain modifying element content, the modifying element is preferably fed in excess. Preferably, the mass ratio of the calcined product to the solution containing the modifying element precursor is 1:2-15, preferably 1:3-10, and more preferably 1:5-7.
[0057] In a preferred embodiment, the impregnation operating conditions include: an impregnation temperature of 50-90°C, preferably 60-85°C; and an impregnation time of 2-12h, preferably 0.5-4h.
[0058] In a preferred embodiment, the impregnated product is dried before the second calcination, for example, at 60-150° C. for 1-10 h.
[0059] In a preferred embodiment, the operating conditions of the second calcination include: the second calcination temperature is 400-600° C., preferably 450-560° C.; the second calcination time is 2-10 h, preferably 3-8 h.
[0060] The third aspect of the present invention provides a method for isomerizing o-cresol, which comprises contacting o-cresol with the o-cresol isomerization catalyst described in the first aspect of the present invention or the o-cresol isomerization catalyst prepared by the preparation method described in the second aspect of the present invention to carry out an isomerization reaction to obtain p-cresol and m-cresol.
[0061] In a preferred embodiment, the operating conditions of the isomerization reaction include: a reaction temperature of 300-450°C, a reaction pressure of 0.1-2.5 MPa, a mass space velocity of o-cresol of 1-5 h -1 , the volume ratio of hydrogen to o-cresol is 200-600:1.
[0062] In a preferred embodiment, the reaction is carried out in a fixed bed reactor.
[0063] The present invention will be described in detail below through examples. The content of the modifying element in the catalyst is analyzed by X-ray fluorescence spectroscopy, and the pore volume and specific surface area are measured by BET method. The IM-5 molecular sieve in the examples and comparative examples is a hydrogen-type IM-5 molecular sieve, namely, HIM-5 molecular sieve.
[0064] Example 1
[0065] (1) HZSM-5 molecular sieve (grain size of 50 nm, silica / alumina molar ratio of 50:1) and HIM-5 molecular sieve (grain size of 50 nm, silica / alumina molar ratio of 50:1) were mixed in a mass ratio of 2:1, put into a ball mill, ball milled for 6 h with ethanol as a medium, and then dried at 110° C. for 4 h to obtain a mixed powder containing nano-HZSM-5 molecular sieve and nano-HIM-5 molecular sieve;
[0066] The mixed powder was mixed with 0.1 mol / L NaOH solution at a mass ratio of 1:6, and alkali-treated at 80°C for 2 hours under stirring, and then filtered, washed with deionized water until the washing liquid was neutral, and dried at 110°C for 4 hours to obtain an alkali-modified mixed powder;
[0067] (2) The alkali-modified mixed powder is mixed with pseudo-boehmite and 5 wt% of dilute nitric acid, and the mixed mixture is extruded to obtain molded particles, and the molded particles are dried at 110° C. for 4 hours and then calcined for the first time, first at 200° C. for 2 hours, then at 350° C. for 2 hours, and then at 560° C. for 4 hours to obtain a calcined product; wherein the mass ratio of the alkali-modified mixed powder to the pseudo-boehmite is 6:4 based on the mass of aluminum oxide in the pseudo-boehmite, and the amount of dilute nitric acid added is 30% of the total mass of the alkali-modified mixed powder and the pseudo-boehmite;
[0068] (3) The above calcined product was mixed with 10 wt% (NH 4 ) 2 HPO 4 The solutions were mixed in a mass ratio of 1:5, impregnated at 80°C for 2 hours while stirring, and then dried to obtain an impregnated product; the impregnated product was dried at 110°C for 4 hours, then calcined for a second time, and calcined at 500°C for 6 hours to obtain o-cresol isomerization catalyst A-1.
[0069] Among them, in the obtained o-cresol isomerization catalyst A-1, the mass ratio of composite molecular sieve: alumina: modifying element P is 60:40:4.33; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.29 mL / g, and the specific surface area is 383 m 2 / g.
[0070] Example 2
[0071] The same as Example 1, except that: in step (3), the above-mentioned calcined product is mixed with 4wt% NH 4 The Cl solution was mixed in a mass ratio of 1:6, impregnated at 85°C for 0.5h while stirring, and then dried to obtain an impregnated product; the obtained impregnated product was dried at 110°C for 4h and then calcined for a second time, and calcined at 500°C for 6h to obtain o-cresol isomerization catalyst A-2.
[0072] Among them, in the obtained o-cresol isomerization catalyst A-2, the mass ratio of composite molecular sieve: alumina: modified element Cl is 60:40:3.77; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.31 mL / g, and the specific surface area is 376 m 2 / g.
[0073] Example 3
[0074] Same as Example 1, except that:
[0075] In step (2), the mass ratio of the alkali-modified mixed powder to the pseudo-boehmite is 7:3 based on the mass of aluminum oxide in the pseudo-boehmite;
[0076] In step (3), the above-mentioned calcined product is mixed with 15wt% NH 4 The F solutions were mixed in a mass ratio of 1:7, immersed for 1 hour at 90°C while stirring, and then dried to obtain an impregnated product; the obtained impregnated product was dried at 110°C for 4 hours and then calcined for a second time at 500°C for 6 hours.
[0077] Among them, in the obtained o-cresol isomerization catalyst A-3, the mass ratio of composite molecular sieve: alumina: modifying element F is 70:30:4.05; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.32 mL / g, and the specific surface area is 387 m 2 / g.
[0078] Example 4
[0079] The same as Example 1, except that: in step (1), the HZSM-5 molecular sieve in Example 1 is replaced by an HZSM-5 molecular sieve with a grain size of 50 nm and a silica / alumina molar ratio of 70, and the HZSM-5 molecular sieve and the HIM-5 molecular sieve are mixed in a mass ratio of 2.5:1.
[0080] Among them, in the obtained o-cresol isomerization catalyst A-4, the mass ratio of composite molecular sieve: alumina: modified element P is 60:40:3.89; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2.5:1; the pore volume is 0.32mL / g, and the specific surface area is 382m 2 / g.
[0081] Example 5
[0082] The same as Example 1, except that: in step (1), the HZSM-5 molecular sieve and the HIM-5 molecular sieve are mixed in a mass ratio of 1:1.
[0083] Among them, in the obtained o-cresol isomerization catalyst A-5, the mass ratio of composite molecular sieve: alumina: modified element P is 60:40:4.12; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 1:1; the pore volume is 0.35 mL / g, and the specific surface area is 407 m 2 / g.
[0084] Example 6
[0085] The same as Example 1, except that the alkali solution in step (1) is 0.15 mol / L KOH.
[0086] Among them, in the obtained o-cresol isomerization catalyst A-6, the mass ratio of composite molecular sieve: alumina: modified element P is 60:40:3.76; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.3mL / g, and the specific surface area is 379m 2 / g.
[0087] Comparative Example 1
[0088] The same as Example 1, except that the alkali treatment in step (1) is omitted, step (3) is omitted, and the mono-burned product in step (2) is used as o-cresol isomerization catalyst D-1.
[0089] Among them, in the o-cresol isomerization catalyst D-1, the mass ratio of composite molecular sieve: alumina is 60:40; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.2mL / g, and the specific surface area is 339m 2 / g.
[0090] Comparative Example 2
[0091] The same as Example 1, except that the alkali treatment in step (1) is omitted to obtain o-cresol isomerization catalyst D-2.
[0092] Among them, in the o-cresol isomerization catalyst D-2, the mass ratio of composite molecular sieve: alumina: modified element Cl is 60:40:4.71; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.22mL / g, and the specific surface area is 350m 2 / g.
[0093] Comparative Example 3
[0094] The same as Example 1, except that step (3) is omitted and the mono-burned product in step (2) is used as o-cresol isomerization catalyst D-3.
[0095] Among them, in the o-cresol isomerization catalyst D-3, the mass ratio of composite molecular sieve:alumina is 60:40; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.23mL / g, and the specific surface area is 335m 2 / g.
[0096] Comparative Example 4
[0097] The same as Example 1, except that the HZSM-5 molecular sieve in Example 1 is replaced by an HZSM-5 molecular sieve with a grain size of 2 μm and a silica / alumina molar ratio of 50:1, to obtain o-cresol isomerization catalyst D-4.
[0098] Among them, in the o-cresol isomerization catalyst D-4, the mass ratio of composite molecular sieve: alumina: modified element P is 60:40:3.67; the mass ratio of HZSM-5 molecular sieve to HIM-5 molecular sieve is 2:1; the pore volume is 0.19 mL / g, and the specific surface area is 327 m 2 / g.
[0099] Test Example 1
[0100] The o-cresol isomerization catalysts prepared in Examples 1-6 and Comparative Examples 1-4 were respectively loaded into a fixed bed microreactor with H 2 As carrier gas, the reaction temperature is 400℃, the reaction pressure is 0.1MPa, and the mass space velocity of o-cresol is 1h -1 , the isomerization reaction of o-cresol was carried out under the condition that the volume ratio of hydrogen to o-cresol was 400. The test results are shown in Table 1.
[0101] The reaction was stopped when the instantaneous conversion rate of o-cresol in the reaction dropped to 10% during the reaction. The o-cresol conversion rate, the m-cresol yield, the p-cresol yield and the phenol yield were calculated based on the o-cresol feed amount and the product generation amount during the whole reaction process.
[0102]
[0103]
[0104]
[0105]
[0106] Table 1
[0107]
[0108] As shown in Table 1, the ortho-cresol isomerization catalyst provided in the present invention has an ortho-cresol conversion rate of more than 52%, a meta-cresol yield of more than 37%, a p-cresol yield of more than 14%, and a catalyst single-pass life of more than 180 hours. The catalyst has not only good activity and high selectivity, but also good stability and long service life.
[0109] Test Example 2
[0110] The deactivated catalysts obtained after the reaction in Examples 1-6 and Comparative Examples 1-4 were regenerated by burning carbon with air containing 5% oxygen by volume, and then the test in Test Example 1 was repeated under the same conditions. When the regeneration test was performed, if the initial o-cresol conversion rate of the regenerated catalyst was measured to be lower than 30%, the regeneration test was stopped. The regeneration times and the experimental results of the o-cresol conversion rate, m-cresol yield, p-cresol yield and phenol yield in the last regeneration are shown in Table 2.
[0111] Table 2
[0112]
[0113] It can be seen from Table 1 that the o-cresol isomerization catalyst provided in the present invention has good regeneration performance and long service life, and is suitable for industrial promotion.
[0114] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. An o-cresol isomerization catalyst, It is characterized in that The catalyst comprises 50-90 parts by weight of a composite molecular sieve, 10-50 parts by weight of alumina and 0.5-8 parts by weight of a modifying element; wherein the composite molecular sieve comprises a nano HZSM-5 molecular sieve and a nano IM-5 molecular sieve, and the modifying element is selected from one or more of F, Cl and P; Wherein, the grain size of the nano HZSM-5 molecular sieve is 20-200 nm, and the molar ratio of silicon dioxide to aluminum oxide of the nano HZSM-5 molecular sieve is 15-100:1; The crystal size of the nano IM-5 molecular sieve is 20-200 nm, and the molar ratio of silicon dioxide to aluminum oxide of the nano IM-5 molecular sieve is 20-80:1; The mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 0.1-15:1; The catalyst has a pore volume of 0.24-0.4 mL / g and a specific surface area of 320-450 m 2 / g.
2. The catalyst according to claim 1, in, The crystal size of the nano HZSM-5 molecular sieve is 30-100 nm, and the molar ratio of silicon dioxide to aluminum oxide of the nano HZSM-5 molecular sieve is 30-70:1; And / or, the crystal size of the nano IM-5 molecular sieve is 50-200 nm, and the molar ratio of silicon dioxide to aluminum oxide of the nano IM-5 molecular sieve is 30-60:1; And / or, the nano IM-5 molecular sieve is a hydrogen nano IM-5 molecular sieve; And / or, the mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 0.5-10:
1.
3. The catalyst according to claim 2, in, The mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 1-6:
1.
4. The catalyst according to claim 1 or 2, in, The modifying element is selected from one of F, Cl and P.
5. The catalyst according to claim 4, in, The modifying element is P.
6. The catalyst according to claim 1, in, The pore volume of the catalyst is 0.26-0.38 mL / g and the specific surface area is 350-420 m 2 / g.
7. A method for preparing the o-cresol isomerization catalyst according to any one of claims 1 to 6, It is characterized in that The method comprises the following steps: (1) mixing a mixed powder containing nano-HZSM-5 molecular sieve and nano-IM-5 molecular sieve with an alkali solution for alkali treatment to obtain an alkali-modified mixed powder; (2) mixing the alkali-modified mixed powder, the alumina precursor and the optional nitric acid, and then forming the mixture to obtain formed particles, and then calcining the formed particles for the first time to obtain a calcined product; (3) The calcined product is mixed with a solution containing a modifying element precursor and then impregnated, then dried to obtain an impregnated product, and then the impregnated product is calcined for a second time to obtain the o-cresol isomerization catalyst.
8. The preparation method according to claim 7, in, In step (1), the mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 0.1-15:1; And / or, the alkali in the alkali solution is selected from NaOH, KOH, Na 2 CO 3 and K 2 CO 3 One or more of the following; And / or, the concentration of the alkali solution is 0.01-1 mol / L; And / or, the mass ratio of the mixed powder to the alkali solution is 1:2-10; And / or, the operating conditions of the alkali treatment include: the alkali treatment temperature is 50-90° C., and the alkali treatment time is 0.5-5 h.
9. The preparation method according to claim 8, in, In step (1), the mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 0.5-10:1; And / or, the alkali in the alkali solution is NaOH and / or KOH; And / or, the concentration of the alkali solution is 0.05-0.2 mol / L; And / or, the mass ratio of the mixed powder to the alkali solution is 1:5-7; And / or, the operating conditions of the alkali treatment include: the alkali treatment temperature is 60-85° C., and the alkali treatment time is 1-4 h.
10. The preparation method according to claim 9, in, In step (1), the mass ratio of the nano HZSM-5 molecular sieve to the nano IM-5 molecular sieve is 1-6:
1.
11. The preparation method according to claim 7, in, In step (2), the alumina precursor is selected from one or more of aluminum sol, aluminum gel, and pseudo-boehmite; and / or, based on the mass of the oxide in the alumina precursor, the mass ratio of the alkali-modified mixed powder to the alumina precursor is 50-90:10-50; and / or, the concentration of the nitric acid is 3-10wt%; And / or, the mass of the nitric acid is 20-55% of the total mass of the alkali-modified mixed powder and the alumina precursor; And / or, the operating conditions of the first calcination include: first calcining at 150-250°C for 1-10h, then calcining at 300-400°C for 1-10h, and then calcining at 500-600°C for 2-14h.
12. The preparation method according to claim 11, in, In step (2), the alumina precursor is pseudo-boehmite; and / or, based on the mass of the oxide in the alumina precursor, the mass ratio of the alkali-modified mixed powder to the alumina precursor is 60-80:20-40; and / or, the concentration of the nitric acid is 5-8wt%; And / or, the mass of the nitric acid is 30-45% of the total mass of the alkali-modified mixed powder and the alumina precursor.
13. The preparation method according to claim 7, in, In step (3), the modifying element precursor is selected from one or more of an ammonium salt or acid containing P, an ammonium salt or acid containing F, and an ammonium salt or acid containing Cl; and / or, the solvent in the solution containing the modified element precursor is water, and the concentration of the modified element precursor is 2-20wt%; And / or, the feeding amounts of the calcined product and the solution containing the modifying element precursor are such that in the prepared catalyst, the mass ratio of the composite molecular sieve to the modifying element is 50-90:0.5-8.
14. The preparation method according to claim 13, in, The solvent in the solution containing the modified element precursor is water, and the concentration of the modified element precursor is 4-10wt%; And / or, the feeding amounts of the calcined product and the solution containing the modifying element precursor are such that the mass ratio of the composite molecular sieve to the modifying element in the prepared catalyst is 60-80:1-6.
15. The preparation method according to claim 7, in, In step (3), the operating conditions of the impregnation include: an impregnation temperature of 50-90° C. and an impregnation time of 2-12 h; And / or, the operating conditions of the second calcination include: the second calcination temperature is 400-600° C., and the second calcination time is 2-10 hours.
16. The preparation method according to claim 15, in, In step (3), the operating conditions of the impregnation include: an impregnation temperature of 60-85°C and an impregnation time of 0.5-4h; And / or, the operating conditions of the second calcination include: the second calcination temperature is 450-560° C., and the second calcination time is 3-8 hours.
17. A method for isomerizing o-cresol, It is characterized in that The method comprises contacting o-cresol with the o-cresol isomerization catalyst described in any one of claims 1 to 6 or the o-cresol isomerization catalyst prepared by the preparation method described in any one of claims 7 to 16 to carry out an isomerization reaction to obtain p-cresol and m-cresol.
18. The method according to claim 17, in, The operating conditions of the isomerization reaction include: reaction temperature of 300-450°C; reaction pressure of 0.1-2.5MPa; mass space velocity of o-cresol of 1-5h -1 ; The volume ratio of hydrogen to o-cresol is 200-600:1.