Environmentally friendly coal powder rapid combustion catalyst and preparation method thereof
The pulverized coal rapid combustion catalyst composed of iron salts, alkaline earth metal salts and nano-rare earth oxides solves the problems of large amounts of precious metals and corrosiveness in the existing technology, achieves efficient pulverized coal combustion and improves environmental protection, significantly improving Improve the energy efficiency and environmental protection of cement production.
Patent Information
- Application Number
- CN202211728497.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-31
AI Technical Summary
Existing pulverized coal catalysts contain large amounts of precious metals and corrosive substances, which lead to economic irrationality and environmental pollution, making it difficult to effectively improve the energy efficiency and environmental protection of cement production.
It uses an environmentally friendly pulverized coal rapid combustion catalyst composed of iron salts, alkaline earth metal salts and nano-rare earth oxides. It is activated by low-temperature ignition to increase oxygen in a high-temperature environment and promote the complete combustion of carbon particles. Combined with the treatment of tartaric acid and ethylene glycol, An economical and environmentally friendly catalyst is prepared and evenly attached in the coal mill to improve combustion efficiency.
It achieves a coal saving rate of 13-15% at low addition amounts, reduces SO2 and smoke emissions, improves the kiln environment, increases daily output by 3.6-4.2%, and avoids equipment corrosion and secondary pollution, which is environmentally friendly and economical. .
Smart Images

Figure CN116060136B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pulverized coal catalysts, and in particular to an environmentally friendly pulverized coal rapid combustion catalyst and a preparation method thereof. Background Art
[0002] In the cement production process, energy consumption accounts for 65% of the cost of cement clinker. Among them, coal consumption accounts for 50%-55% of the cost of cement clinker. There are many studies on the catalytic combustion of coal at home and abroad. Most of the catalysts developed for catalytic combustion technology are not economical because the amount of precious metals required is too large. Although a few catalytic combustion agents can reduce the amount of addition, they contain chlorides, nitrates or sodium and potassium salts, which are corrosive to equipment (including kiln linings) and cause secondary pollution. Summary of the invention
[0003] Based on the above problems, the purpose of the present invention is to provide an environmentally friendly coal powder rapid combustion catalyst and a preparation method thereof, and to develop an economical, practical and environmentally friendly coal powder rapid combustion catalyst.
[0004] The technical solution of the present invention is:
[0005] An environmentally friendly coal powder rapid combustion catalyst comprises the following raw materials: iron salt, alkaline earth metal salt, rare earth compound; the rare earth compound is nano rare earth oxide; the weight ratio of the iron salt, alkaline earth metal salt and rare earth compound is 10-12:30-50:0.1-0.2.
[0006] Furthermore, the iron salt includes polyaluminium iron silicate and polyaluminium iron phosphate.
[0007] Furthermore, the alkaline earth metal salt includes magnesium carbonate and calcium oxalate.
[0008] Furthermore, the rare earth compound includes at least two of lanthanum oxide, cerium oxide, and samarium oxide.
[0009] Preferably, it is composed of polyaluminium ferric silicate, polyaluminium ferric phosphate, magnesium carbonate, calcium oxalate, samarium oxide and lanthanum oxide.
[0010] Preferably, it is composed of polyaluminium ferric silicate, polyaluminium ferric phosphate, magnesium carbonate, calcium oxalate, cerium oxide and samarium oxide.
[0011] The preparation method of the environmentally friendly coal powder rapid combustion catalyst comprises the following steps: mixing the iron salt, rare earth compound and alkaline earth metal salt in proportion, grinding to 200 mesh, adding tartaric acid and ethylene glycol, ultrasonically shaking, stirring, and then adjusting the pH value to neutral, heating and stirring for 2-3 hours, and grinding again to 200-500 mesh after drying.
[0012] Furthermore, the amount of tartaric acid added is 1.1-2 times the total amount of iron salts, alkaline earth metal salts and rare earth compounds, and the heating temperature is not less than 150°C.
[0013] Furthermore, the method of using the environmentally friendly coal powder rapid combustion catalyst is: adding the catalyst and coal into the coal mill at the front end of the coal mill, so that the catalyst is evenly attached to the surface of the coal powder, wherein the amount of the catalyst is 0.1% to 0.2% of the amount of coal powder.
[0014] The pulverized coal rapid combustion catalyst of the present invention is ignited at low temperature, utilizes energy to activate oxygenation in a high temperature environment, catalyzes ash and accelerates the full combustion of carbon particles in a high temperature zone, thereby increasing the density and temperature of the flame, improving the thermal efficiency of the pulverized coal, eliminating the harm of unburned carbon particles to kiln production, reducing the reducing atmosphere in the kiln, the long and thick auxiliary kiln skin and system crusting, reducing the actual coal consumption and system power consumption, and realizing energy conservation, emission reduction, high quality and high yield.
[0015] Compared with the prior art, the beneficial effects of this solution are as follows:
[0016] The addition amount of the pulverized coal rapid combustion catalyst of the present invention is as low as 0.1% to 0.2%, the coal saving rate is 13-15%, and the SO2 emission concentration is reduced by 180-240 mg / m 3 , the dust emission concentration at the outlet is reduced by 450-550mg / m 3 After using this catalyst, the calcination environment in the kiln was improved, and the kiln output increased by 3.6-4.2% per day.
[0017] The coal powder rapid combustion catalyst of the present invention does not contain chloride salts, nitrates or sodium and potassium salts which are corrosive to equipment and cause secondary pollution, and has a small amount of rare earth compounds added, thereby being environmentally friendly and economical. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Add a catalyst for rapid combustion of pulverized coal into the system. DETAILED DESCRIPTION
[0019] The following will be combined with the attached embodiment of the present invention Figure 1 , the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.
[0020] Example 1
[0021] An environmentally friendly coal powder rapid combustion catalyst comprises the following raw materials:
[0022] Iron salts: polyaluminium ferric silicate, polyaluminium ferric phosphate; alkaline earth metal salts: magnesium carbonate, calcium oxalate; rare earth compounds: nano samarium oxide, nano lanthanum oxide; the weight ratio of the iron salts, alkaline earth metal salts and rare earth compounds is 10:30:0.1; the weight ratio of the polyaluminium ferric silicate and polyaluminium ferric phosphate is 2:1; the weight ratio of magnesium carbonate and calcium oxalate is 3:5; the weight ratio of nano samarium oxide and nano lanthanum oxide is 1:1.
[0023] The environmentally friendly coal powder rapid combustion catalyst is prepared by the following steps:
[0024] The iron salt, rare earth compound and alkaline earth metal salt are mixed in proportion, ground to 200 mesh, and tartaric acid and ethylene glycol are added, wherein the amount of tartaric acid added is 1.1 times the total amount of the iron salt, alkaline earth metal salt and rare earth compound, and the amount of ethylene glycol added is at least enough to immerse the solid raw materials. Ultrasonic vibration is performed for 1.2 hours, stirring is performed for 2 hours, and then the pH value is adjusted to neutral. The mixture is heated and stirred at 150° C. for 2 hours, filtered and dried, and then ground to 500 mesh again.
[0025] Usage: Place the pulverized coal rapid combustion catalyst in a storage tank, and control the amount of the pulverized coal rapid combustion catalyst added through a metering pump and a flow meter; mix the adjusted pulverized coal rapid combustion catalyst with the coal on the coal feeding belt scale and add them to the pulverizer, so that the pulverized coal rapid combustion catalyst is evenly attached to the surface of the pulverized coal, and then enter the kiln for combustion.
[0026] Example 2
[0027] An environmentally friendly coal powder rapid combustion catalyst comprises the following raw materials:
[0028] Iron salts: polyaluminium ferric silicate, polyaluminium ferric phosphate; alkaline earth metal salts: magnesium carbonate, calcium oxalate; rare earth compounds: nano samarium oxide, nano lanthanum oxide; the weight ratio of the iron salts, alkaline earth metal salts and rare earth compounds is 11:40:0.15; the weight ratio of the polyaluminium ferric silicate and polyaluminium ferric phosphate is 3:2; the weight ratio of magnesium carbonate and calcium oxalate is 1:1; the weight ratio of nano samarium oxide and nano cerium oxide is 5:1.
[0029] The environmentally friendly coal powder rapid combustion catalyst is prepared by the following steps:
[0030] The iron salt, rare earth compound and alkaline earth metal salt are mixed in proportion, ground to 200 mesh, and tartaric acid and ethylene glycol are added, wherein the amount of tartaric acid added is 1.5 times the total amount of the iron salt, alkaline earth metal salt and rare earth compound, and the amount of ethylene glycol added is at least enough to immerse the solid raw materials. Ultrasonic vibration is performed for 1.5 hours, stirring is performed for 1.5 hours, and then the pH value is adjusted to neutral. The mixture is heated and stirred at 170°C for 2.5 hours, filtered and dried, and then ground to 300 mesh again.
[0031] How to use Figure 1 : Place the pulverized coal rapid combustion catalyst in a storage tank, and control the amount of the pulverized coal rapid combustion catalyst added through a metering pump and a flow meter, mix the adjusted pulverized coal rapid combustion catalyst with the coal on the coal feeding belt scale and add them into the pulverizer, so that the pulverized coal rapid combustion catalyst is evenly attached to the surface of the pulverized coal, and then enters the kiln for combustion.
[0032] Example 3
[0033] An environmentally friendly coal powder rapid combustion catalyst comprises the following raw materials:
[0034] Iron salts: polyaluminium ferric silicate, polyaluminium ferric phosphate; alkaline earth metal salts: magnesium carbonate, calcium oxalate; rare earth compounds: nano samarium oxide, nano lanthanum oxide; the weight ratio of the iron salts, alkaline earth metal salts and rare earth compounds is 12:50:-0.2; the weight ratio of the polyaluminium ferric silicate and polyaluminium ferric phosphate is 7:3; the weight ratio of magnesium carbonate and calcium oxalate is 2:5; the weight ratio of nano lanthanum oxide and nano cerium oxide is 3:1.
[0035] The environmentally friendly coal powder rapid combustion catalyst is prepared by the following steps:
[0036] The iron salt, rare earth compound and alkaline earth metal salt are mixed in proportion, ground to 200 mesh, and tartaric acid and ethylene glycol are added, wherein the amount of tartaric acid added is twice the total amount of the iron salt, alkaline earth metal salt and rare earth compound, and the amount of ethylene glycol added is at least enough to immerse the solid raw materials. Ultrasonic vibration is performed for 1.5 hours, stirring is performed for 2 hours, and then the pH value is adjusted to neutral, heated and stirred at 180° C. for 3 hours, filtered and dried, and then ground to 200 mesh again.
[0037] Usage: Place the pulverized coal rapid combustion catalyst in a storage tank, and control the amount of the pulverized coal rapid combustion catalyst added through a metering pump and a flow meter; mix the adjusted pulverized coal rapid combustion catalyst with the coal on the coal feeding belt scale and add them to the pulverizer, so that the pulverized coal rapid combustion catalyst is evenly attached to the surface of the pulverized coal, and then enter the kiln for combustion.
[0038] Test example
[0039] Experimental comparison was carried out using coal powder rapid combustion catalyst, which was divided into three groups of experiments: Example 1, Example 2, Example 3 and a blank control group. The blank control group did not add coal powder rapid combustion catalyst, and then randomly counted the work improvement every day within 15 days, and calculated the average value. The specific results are shown in Table 1.
[0040]
[0041] The results show that compared with the case without adding pulverized coal rapid combustion catalyst, the addition of the pulverized coal rapid combustion catalyst can save coal by 13-15% and reduce the SO2 emission concentration by 180-240mg / m 3 , the dust emission concentration at the outlet was reduced by 450-550mg / m 3 After using this catalyst, the calcination environment in the kiln was improved and the daily output of the kiln increased by 3.6-4.2%.
[0042] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An environmentally friendly coal powder rapid combustion catalyst, It is characterized in that The invention is composed of iron salt, alkaline earth metal salt and rare earth compound; the rare earth compound is nano rare earth oxide; the weight ratio of the iron salt, alkaline earth metal salt and rare earth compound is 10-12:30-50:0.1-0.2; the iron salt includes polyaluminium ferric silicate and polyaluminium ferric phosphate; the alkaline earth metal salt includes magnesium carbonate and calcium oxalate; the rare earth compound includes at least two of lanthanum oxide, cerium oxide and samarium oxide; the preparation method specifically comprises the following steps: mixing the iron salt, rare earth compound and alkaline earth metal salt in proportion, grinding to 200 mesh, adding tartaric acid and ethylene glycol, ultrasonically shaking, stirring, then adjusting the pH value to neutral, heating and stirring for 2-3 hours, drying and grinding again to 200-500 mesh.
2. An environmentally friendly coal powder rapid combustion catalyst according to claim 1, It is characterized in that It is composed of polyaluminium ferric silicate, polyaluminium ferric phosphate, magnesium carbonate, calcium oxalate, samarium oxide and lanthanum oxide.
3. The environmentally friendly coal powder rapid combustion catalyst according to claim 1, It is characterized in that It is composed of polyaluminium ferric silicate, polyaluminium ferric phosphate, magnesium carbonate, calcium oxalate, cerium oxide and samarium oxide.
4. The environmentally friendly coal powder rapid combustion catalyst according to claim 1, It is characterized in that The added amount of tartaric acid is 1.1-2 times the total amount of iron salts, alkaline earth metal salts and rare earth compounds, and the heating temperature is not less than 150°C.
5. A method for using the environmentally friendly pulverized coal rapid combustion catalyst as claimed in any one of claims 1 to 4, It is characterized in that The catalyst is added into the coal mill together with coal at the front end of the coal mill so that the catalyst is evenly attached to the surface of the coal powder. The amount of the catalyst used is 0.1% to 0.2% of the amount of the coal powder.