Aluminum hydroxide core-shell structure flame retardant and preparation method thereof

By coating aluminum diethylphosphinate and melamine cyanuric acid on the surface of aluminum hydroxide, forming a core-shell structure flame retardant of aluminum hydroxide, the problems of low flame retardant efficiency and degradation of material mechanical properties are solved, and the problem of low flame retardant efficiency of aluminum hydroxide and reduced mechanical properties of materials is achieved. Efficient flame retardant performance improvement and mechanical performance improvement, suitable for flame retardant and processing of composite materials.

CN118895017APending Publication Date: 2024-11-05BEIJING INST OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410879986.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Aluminum hydroxide has low flame retardant efficiency and large amount of addition, which affects the material's processability and mechanical properties. It is difficult to maintain the material's processability and mechanical properties while improving the flame retardant properties.

Method used

By coating aluminum diethylphosphinate and melamine cyanuric acid layer by layer on the surface of aluminum hydroxide, using aqueous solution reaction and supramolecular self-assembly reaction, a flame retardant of aluminum hydroxide core-shell structure is formed to form an aluminum phosphate-reinforced carbon layer to form an aluminum phosphate reinforced carbon layer and inert gases, improve flame retardant properties, and enhance polymer interaction through hydrogen bonds to improve mechanical properties.

Benefits of technology

The flame retardant performance of the material is significantly improved, the amount of flame retardant added is reduced, and the effect of reaching the V-0 level of UL-94 vertical combustion test at a lower addition is achieved, while improving the processability and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895017A_ABST
    Figure CN118895017A_ABST
Patent Text Reader

Abstract

The invention relates to an aluminum hydroxide core-shell structure flame retardant and a preparation method thereof, and belongs to the technical field of flame retardance. According to the invention, through a simple aqueous solution reaction, the surface of aluminum hydroxide is coated with aluminum diethylphosphinate (ADP) and melamine cyanuric acid (MCA) layer by layer. In the combustion process, aluminum hydroxide and aluminum diethylphosphinate generate an aluminum phosphate reinforced carbon layer, melamine cyanuric acid is decomposed, absorbs heat and generates inert gas to inhibit gas-phase combustion, so that the polymer plays a role in gas phase and condensation during combustion, and the flame retardant property of the material is greatly improved. Meanwhile, the melamine cyanuric acid on the outermost layer is rich in a large amount of amino groups, and hydroxyl groups can form hydrogen bonds with the polymer, so that the interaction between the melamine cyanuric acid and the polymer is enhanced, and the mechanical property of the composite material is improved. The preparation method of the flame retardant is simple and efficient, and the preparation process is green and environment-friendly. The preparation of the aluminum hydroxide core-shell structure flame retardant is not reported in literatures until now.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum hydroxide core-shell structure flame retardant and a preparation method thereof, belonging to the technical field of flame retardancy. Background Art

[0002] Polymer materials have the advantages of light weight, good processability and low price, and are widely used in social life and industrial production. However, polymer materials are composed of elements such as C, H, and O, which are extremely easy to burn and cause fires, and have a high fire hazard. In order to ensure the orderly progress of social production and the safety of the lives of the majority of residents, polymers must be flame-retardant to reduce the fire hazard of the materials. Aluminum hydroxide (ATH) is non-toxic, harmless and inexpensive. It can not only improve the flame retardant properties of materials but also act as a filler. It is the most widely used flame retardant in polymers. However, aluminum hydroxide has low flame retardant efficiency. In order to achieve the flame retardant level required by the polymer, the amount added to the polymer must be more than 60%. This seriously damages the mechanical properties of the material, causing the material to be too brittle and difficult to process, making the polymer material unable to even meet basic usage requirements.

[0003] In order to reduce the damage of aluminum hydroxide to the mechanical properties of the material, aluminum hydroxide is generally surface treated to improve the compatibility between aluminum hydroxide and the polymer. The methods for modifying particles mainly include microencapsulation, inorganic particle coating and coupling agent surface modification. Microcapsule coating usually requires a large amount of organic reagents, the preparation method is complicated, and the waste liquid is difficult to handle; inorganic particle coating can only enhance the interaction between the flame retardant and the polymer through the interlocking effect between the surface particles and the polymer, the compatibility is not improved, and the improvement of mechanical properties is limited; and the modification of the coupling agent on the particle surface is usually limited to the thickness of the monolayer, the modification effect is single, and it can only significantly improve the mechanical properties, but not the flame retardant properties. In order to improve the flame retardancy of the material while improving the mechanical properties, reduce the amount of flame retardant added, improve the processing performance, and prepare a composite material with excellent comprehensive performance, the present invention designs a hydroxide core-shell structure flame retardant. Compared with existing technologies, the preparation method is simple and the whole process is green and pollution-free. While improving the mechanical properties, it also significantly improves the flame retardant properties of the material. Compared with previous modification methods, it can achieve the UL-94 vertical burning test V-0 level with less addition. Summary of the invention

[0004] The purpose of the present invention is to solve the problems of low flame retardant efficiency of aluminum hydroxide, large addition amount, affecting material processability, and reducing the mechanical properties of polymer composite materials, and to provide an aluminum hydroxide core-shell structure flame retardant and a preparation method thereof. The method coats aluminum diethylphosphinate (ADP) and melamine cyanuric acid (MCA) layer by layer on the surface of aluminum hydroxide through a simple aqueous solution reaction. During the combustion process, aluminum hydroxide and aluminum diethylphosphinate generate aluminum phosphate reinforced carbon layers, and melamine cyanuric acid decomposes to absorb heat and produce inert gas to inhibit gas phase combustion, so that the polymer can be burned in the gas phase and condensed phase at the same time, greatly improving the flame retardant properties of the material. At the same time, the outermost melamine cyanuric acid is rich in a large number of amino groups and hydroxyls that can form hydrogen bonds with polymers, enhance the interaction with the polymer, and improve the mechanical properties of the composite material. The flame retardant preparation method is simple and efficient, and the preparation process is green and environmentally friendly. So far, there is still no literature report on the preparation of aluminum hydroxide core-shell structure flame retardants.

[0005] The purpose of the present invention is achieved through the following technical solutions.

[0006] An aluminum hydroxide core-shell structure flame retardant is prepared by coating aluminum diethylphosphinate and melamine cyanuric acid on the surface of aluminum hydroxide through simple aqueous solution ion reaction and supramolecular self-assembly reaction; the mass of aluminum diethylphosphinate is 10%-30% of the total mass, and the mass of MCA is 3%-15% of the total mass. The total mass is the sum of the masses of aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid.

[0007] The preparation of the aluminum hydroxide core-shell structure flame retardant of the present invention comprises the following steps:

[0008] (1) Dispersing aluminum hydroxide in deionized water, heating, and stirring for 10 minutes;

[0009] (2) adding a certain amount of sodium diethyl hypophosphite aqueous solution to (1), mixing evenly, adding aluminum salt solution, and heating to react;

[0010] (3) Add cyanuric acid to (2), heat and stir for 30 minutes; then add melamine and heat to react;

[0011] (4) The material after the reaction in (3) is filtered, washed with deionized water for 2 to 3 times, and dried to obtain an aluminum hydroxide core-shell structure flame retardant.

[0012] Preferably, the reaction temperature of steps (2) and (3) is between 70 and 90° C., and the reaction time is between 1 and 3 hours.

[0013] Preferably, in step (2), the molar ratio of diethylphosphite to aluminum ion is 3.5:1 to 2.5:1; and the aluminum salt includes aluminum sulfate, aluminum chloride and aluminum nitrate.

[0014] Preferably, in step (3), the molar ratio of melamine to cyanuric acid is 1.5:1 to 1:1.5;

[0015] Beneficial Effects

[0016] 1. The aluminum hydroxide core-shell structure flame retardant of the present invention uses water as the reaction solvent system, utilizes simple ion precipitation reaction and supramolecular self-assembly reaction, and can be prepared by reacting at 80° C. for 4 to 5 hours. The preparation process involves mild reaction conditions, is green and environmentally friendly, and has high preparation efficiency.

[0017] 2. The aluminum hydroxide core-shell structure flame retardant prepared by the present invention realizes the integration of the flame retardant through the fine design of the structure, so that aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid are distributed closer and more evenly in space. During the combustion of the polymer, aluminum hydroxide and aluminum diethylphosphinate can generate aluminum phosphate reinforced carbon layer faster and more efficiently, and melamine cyanuric acid decomposes to absorb heat and produce inert gas, which enhances the gas phase flame retardant effect, so that the core-shell structure flame retardant has both gas phase and condensed phase flame retardant effects, greatly improving the flame retardant properties of the material. The improvement of flame retardant properties reduces the amount of flame retardant added and improves the processability of the material.

[0018] 3. When the aluminum hydroxide core-shell structure flame retardant prepared by the present invention is applied to a polymer, the outermost layer of melamine cyanuric acid contains rich amino and hydroxyl groups, which can form intermolecular interactions such as hydrogen bonds with a variety of polymers, improve compatibility, make it more evenly dispersed in the polymer, and at the same time form stronger interfacial interactions, thereby improving the mechanical properties of the polymer composite. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0020] Figure 1 is the XRD spectrum of ATH@ADP@MCA;

[0021] Figure 2 This is the infrared spectrum curve of ATH@ADP@MCA core-shell structure flame retardant; DETAILED DESCRIPTION

[0022] The present invention is further described below in conjunction with the accompanying drawings and embodiments, which do not limit the protection scope of the present invention.

[0023] Comparative Example 1

[0024] Ethylene vinyl acetate copolymer (EVA) was melt blended in an internal mixer at 140°C for 15 minutes. The sample was rolled out using a double-roll open mixer at 110°C, and then hot-pressed at 170°C and 10 MPa using a flat vulcanizer to prepare an EVA sample.

[0025] Comparative Example 2

[0026] 55% aluminum hydroxide and 45% ethylene vinyl acetate copolymer were melt blended in an internal mixer at 140°C for 15 minutes. The sample was rolled out using a double-roll open mill at 110°C, and then hot-pressed at 170°C and 10MPa using a flat vulcanizer to prepare an EVA composite material.

[0027] Comparative Example 3

[0028] A physical mixed powder of aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid is prepared by grinding and mixing aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid. 50g of aluminum hydroxide, 8g of aluminum diethylphosphinate and 2g of melamine cyanuric acid are dried in an oven, ground and mixed evenly in a mortar, and then sieved to obtain a physical mixed powder of aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid, wherein the mass ratio of aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid is 50:8:2.

[0029] 55% of physically mixed powder and 45% of ethylene vinyl acetate copolymer were melt blended in an internal mixer at 140°C for 15 minutes. The sample was rolled out using a double-roll open mill at 110°C, and then hot-pressed at 170°C and 10MPa using a flat vulcanizer to prepare an EVA composite material.

[0030] Comparative Example 4

[0031] Dissolve 50g of aluminum hydroxide in 300mL of deionized water, transfer to a three-necked flask and stir evenly; transfer 11.08g of diethyl sodium hypophosphite and stir for 20min, dissolve 8.54g of aluminum sulfate 18hydrate in 100mL of deionized water, add dropwise to the three-necked flask and react at 90°C for 2h; finally, cool the product to room temperature, filter, wash three times with deionized water, filter, dry in an oven at 80°C to remove water, and obtain an aluminum hydroxide core-shell structure flame retardant, in which the mass ratio of aluminum hydroxide to diethyl aluminum phosphite is 50:10.

[0032] The prepared aluminum hydroxide core-shell structure flame retardant was added to an internal mixer at a ratio of 55% and ethylene vinyl acetate copolymer, and melt-blended at 140°C for 15 minutes in the internal mixer. The sample was sheeted using a double-roll open mill at 110°C; then, it was hot-pressed at 170°C and 10MPa using a flat vulcanizer to prepare an EVA composite material.

[0033] Example 1

[0034] 50g of aluminum hydroxide was dissolved in 300mL of deionized water, transferred into a three-necked flask and stirred evenly; 8.86g of diethyl sodium hypophosphite was transferred in and stirred for 20min, 6.83g of aluminum sulfate 18hydrate was dissolved in 100mL of deionized water, and added dropwise to the three-necked flask to react at 90°C for 2h; then 1g of cyanuric acid and melamine were dissolved in 100ml of deionized water respectively; the cyanuric acid solution was added into the three-necked flask and stirred for 30min, and then the melamine solution was added into the three-necked flask to continue reacting at 90°C for 3h; finally, the product was cooled to room temperature, filtered, washed with deionized water three times, filtered, dried in an oven at 80°C to remove water, and an aluminum hydroxide core-shell structure flame retardant was obtained, wherein the mass ratio of aluminum hydroxide, diethyl aluminum phosphinate and melamine cyanuric acid was 50:8:2.

[0035] like Figure 1 As shown in Figure 2, diffraction peaks of aluminum diethylphosphinate and melamine cyanuric acid were observed in ATH@ADP@MCA powder, proving the presence of aluminum diethylphosphinate and melamine cyanuric acid. Figure 2 In the experiment, the infrared absorption peaks of methylethyl and amino groups appeared in ATH@ADP@MCA, which also proved the existence of aluminum diethylphosphinate and melamine cyanuric acid, and proved the successful synthesis of hydroxide core-shell structure flame retardant.

[0036] The prepared aluminum hydroxide core-shell structure flame retardant was added to an internal mixer at a ratio of 55% and ethylene vinyl acetate copolymer, and melt-blended at 140°C for 15 minutes in the internal mixer. The sample was sheeted using a double-roll open mill at 110°C; then, it was hot-pressed at 170°C and 10MPa using a flat vulcanizer to prepare an EVA composite material.

[0037] Example 2

[0038] 50g of aluminum hydroxide was dissolved in 300mL of deionized water, transferred into a three-necked flask and stirred evenly; 6.65g of diethyl sodium hypophosphite was transferred in and stirred for 20min, 5.12g of aluminum sulfate 18hydrate was dissolved in 100mL of deionized water, and added dropwise to the three-necked flask to react at 90°C for 2h; then 2g of cyanuric acid and melamine were dissolved in 100ml of deionized water respectively; the cyanuric acid solution was added into the three-necked flask and stirred for 30min, and then the melamine solution was added into the three-necked flask to continue reacting at 90°C for 3h; finally, the product was cooled to room temperature, filtered, washed with deionized water three times, filtered, dried in an oven at 80°C to remove water, and an aluminum hydroxide core-shell structure flame retardant was obtained, wherein the mass ratio of aluminum hydroxide, diethyl aluminum phosphinate and melamine cyanuric acid was 50:6:4.

[0039] The prepared aluminum hydroxide core-shell structure flame retardant was added to an internal mixer at a ratio of 55% and ethylene vinyl acetate copolymer, and melt-blended at 140°C for 15 minutes in the internal mixer. The sample was sheeted using a double-roll open mill at 110°C; then, it was hot-pressed at 170°C and 10MPa using a flat vulcanizer to prepare an EVA composite material.

[0040] Example 3

[0041] 45g of aluminum hydroxide was dissolved in 300mL of deionized water, transferred into a three-necked flask and stirred evenly; 14.40g of diethyl sodium hypophosphite was transferred in and stirred for 20min, 11.10g of aluminum sulfate 18hydrate was dissolved in 100mL of deionized water, and added dropwise to the three-necked flask to react at 90°C for 2h; then 1g of cyanuric acid and melamine were dissolved in 100ml of deionized water respectively; the cyanuric acid solution was added into the three-necked flask and stirred for 30min, and then the melamine solution was added into the three-necked flask to continue reacting at 90°C for 3h; finally, the product was cooled to room temperature, filtered, washed with deionized water three times, filtered, dried in an oven at 80°C to remove water, and an aluminum hydroxide core-shell structure flame retardant was obtained, wherein the mass ratio of aluminum hydroxide, diethyl aluminum phosphinate and melamine cyanuric acid was 45:13:2.

[0042] The prepared aluminum hydroxide core-shell structure flame retardant was added to an internal mixer at a ratio of 55% and ethylene vinyl acetate copolymer, and melt-blended at 140°C for 15 minutes in the internal mixer. The sample was sheeted using a double-roll open mill at 110°C; then, it was hot-pressed at 170°C and 10MPa using a flat vulcanizer to prepare an EVA composite material.

[0043] Example 4

[0044] 45g of aluminum hydroxide was dissolved in 300mL of deionized water, transferred into a three-necked flask and stirred evenly; 12.19g of sodium diethylphosphite was transferred in and stirred for 20min, 9.39g of aluminum sulfate 18hydrate was dissolved in 100mL of deionized water, and added dropwise to the three-necked flask to react at 90°C for 2h; then 2g of cyanuric acid and melamine were dissolved in 100ml of deionized water respectively; the cyanuric acid solution was added into the three-necked flask and stirred for 30min, and then the melamine solution was added into the three-necked flask to continue reacting at 90°C for 3h; finally, the product was cooled to room temperature, filtered, washed with deionized water three times, filtered, dried in an oven at 80°C to remove water, and an aluminum hydroxide core-shell structure flame retardant was obtained, wherein the mass ratio of aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid was 45:11:4.

[0045] The prepared aluminum hydroxide core-shell structure flame retardant was added to an internal mixer at a ratio of 55% and ethylene vinyl acetate copolymer, and melt-blended at 140°C for 15 minutes in the internal mixer. The sample was sheeted using a double-roll open mill at 110°C; then, it was hot-pressed at 170°C and 10MPa using a flat vulcanizer to prepare an EVA composite material.

[0046] The prepared EVA composite material was subjected to oxygen index, vertical combustion test, cone calorimeter combustion test and tensile test. The specific results are shown in Table 1:

[0047] Table 1 Oxygen index, vertical combustion, cone calorimeter and tensile test data of EVA and EVA composites

[0048]

[0049] As can be seen from Table 1, pure EVA has excellent mechanical properties, but it is extremely flammable; when a large amount of ATH is directly added, the flame retardant properties are improved to a certain extent, but the mechanical properties are greatly reduced. When ATH, ADP and MCA are directly physically mixed and added to EVA, the flame retardant properties are improved to a certain extent, but the mechanical properties are further reduced. This is due to the agglomeration of particles of different flame retardants; and the comparison of Comparative Example 4 and Example 1 shows that the reduction in mechanical properties is mainly caused by poor compatibility of ADP and agglomeration of particles; when we add aluminum hydroxide core-shell structure flame retardant to EVA, the flame retardant properties are further improved, the vertical burning grade reaches V-0, the oxygen index is higher than 34, the heat release is lower than the direct physical mixing sample, and the elongation at break can be maintained at more than 130%. It shows that the aluminum hydroxide core-shell structure flame retardant of the present invention can significantly improve the flame retardant properties of the material without reducing the mechanical properties of the material, and has good application value.

[0050] The above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An aluminum hydroxide core-shell structure flame retardant, characterized in that: Aluminum diethylphosphinate and melamine cyanuric acid are coated on the surface of aluminum hydroxide through simple aqueous solution ion reaction and supramolecular self-assembly reaction; the mass of aluminum diethylphosphinate is 10% to 30% of the total mass, and the mass of MCA is 3% to 15% of the total mass; the total mass is the sum of the masses of aluminum hydroxide, aluminum diethylphosphinate and melamine cyanuric acid.

2. The method for preparing the aluminum hydroxide core-shell structure flame retardant as claimed in claim 1, characterized in that: The steps include: (1) dispersing aluminum hydroxide in deionized water, heating, and stirring uniformly; (2) adding an aqueous solution of sodium diethyl hypophosphite to step (1), mixing well, then adding an aluminum salt solution, and heating to react; (3) adding cyanuric acid to step (2), heating and stirring; then adding melamine, heating and reacting to obtain a material; (4) The material obtained in step (3) is filtered, washed with deionized water for multiple times, and dried to obtain an aluminum hydroxide core-shell structure flame retardant.

3. The method according to claim 2, characterized in that: The reaction temperature of steps (2) and (3) is between 70 and 90° C., and the reaction time is between 1 and 3 hours.

4. The method according to claim 2, characterized in that: In step (2), the molar ratio of diethylphosphite to aluminum ion is 3.5:1 to 2.5:1; and the aluminum salt includes aluminum sulfate, aluminum chloride and aluminum nitrate.

5. The method according to claim 2, characterized in that: In step (3), the molar ratio of melamine to cyanuric acid is 1.5:1 to 1:1.5.

Citation Information

Cited By

  • Melamine phosphite / aluminum phosphite with core-shell structure and preparation method thereof

    CN119371722A

  • Preparation method and application of magnesium-aluminum double-metal hydroxide coated aluminum diethylphosphinate composite halogen-free flame retardant with core-shell structure

    CN120623228A