A method for recycling waste hydrogenation catalyst
Through low-temperature roasting and acid solution treatment, combined with organic amines to adjust the pH value, the problems of cumbersome steps and difficult impurity removal in the recycling process of used hydrogenation catalysts are solved, and efficient metal recovery and new catalyst activity improvement are achieved, which is suitable for large batches of catalysts. of reuse.
Patent Information
- Application Number
- CN202111272120.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The existing technology has complicated steps, high costs, and low recovery rates in the recycling process of used hydrogenation catalysts. It is especially unsuitable when processing large quantities of catalysts, and it is difficult to effectively remove impurities such as iron and calcium, which affects the metal recovery efficiency.
Low-temperature roasting is used to convert the metals in the spent hydrogenation catalyst into the oxidized state. An acid solution is added to remove calcium and adjust the pH value. It is combined with organic amines to remove iron impurities to form a highly active metal impregnating solution, which can be directly used to prepare new hydrogenation catalysts.
The metal recovery steps are simplified, the recovery efficiency is improved, and waste generation is reduced. The new catalyst obtained has high activity and is suitable for the reuse of Ni(Co)-Mo series catalysts.
Smart Images

Figure BDA0003329168470000101 
Figure BDA0003329168470000111 
Figure BDA0003329168470000121
Abstract
Description
Technical Field
[0001] The invention belongs to the field of waste catalyst recycling, and specifically relates to a method for recycling waste hydrogenation catalysts. Background Art
[0002] Hydrogenation catalysts are scrapped after several cycles of use. The usual method is to extract the active metals in the spent catalysts in steps and convert them into metal salts or oxides to achieve metal recycling. However, impurities such as iron and calcium in spent hydrogenation catalysts will affect the performance of hydrogenation catalysts. In the process of metal recycling, it usually takes a relatively high cost to remove them.
[0003] CN109837393A discloses a method for selectively recovering valuable metals in waste hydrogenation catalysts. The method first calcines the waste hydrogenation catalyst at high temperature and then crushes it, and then treats it with solutions three times. Molybdenum, nickel, vanadium and aluminum can be selectively recovered in sequence, and the recovery rate is high. This method recovers the metals in the catalyst separately, and the process is cumbersome. If the hydrogenation catalyst is prepared again, the metal needs to be dissolved again, which consumes a lot of energy.
[0004] CN112439462A discloses a method for recycling and reusing waste hydrogenation catalysts, which comprises: heat treating and grinding the waste hydrogenation catalysts to obtain waste catalyst powders, separating the waste catalyst powders, and using the low-density waste catalyst powders for slurry bed catalytic hydrogenation reactions. This method cannot completely recycle the metals in the catalyst, and the activity of the low-density powders is much different from that of fresh catalysts.
[0005] CN112547080A discloses a method for recycling and reusing a supported hydrogenation catalyst. The method is to crush the screened waste catalyst to less than 50 microns, then add it to the kneading process of carrier preparation in a certain proportion, and then extrusion molding, drying, and roasting in an inert gas atmosphere to obtain a mixed carrier. The carbon on the waste catalyst weakens the interaction between the metal and the carrier, and the active component impregnation liquid is supplemented for loading. The prepared catalyst has a high hydrodesulfurization activity. This method can only process a small amount of waste catalysts, and is not suitable for the treatment of a large number of waste catalysts in industrial production processes.
[0006] CN112619658A discloses a method for recycling waste hydrogenation catalysts. The method comprises extracting and removing oil from the waste hydrogenation catalyst, roasting and removing carbon, crushing, screening, and then mixing with alkali, roasting, impregnating the roasted waste catalyst powder with hot water, filtering, obtaining filtrate and residue, and then adding polymer monomer I to the filtrate to obtain solution I; mixing the residue with acid for reaction, filtering, adding polymer monomer II to the filtrate to obtain solution II; performing parallel gelation reaction with solution I and solution II, aging, adding initiator to the aged suspension, performing polymerization reaction, separating the material from solid and liquid, extruding into strips, and then drying and roasting to obtain a hydrogenation catalyst. This treatment method has complicated steps, generates a large amount of waste, and has high environmental costs. Summary of the invention
[0007] In order to simplify the steps of recovering active metals in spent hydrogenation catalysts, improve metal recovery efficiency, and reduce waste generated during the metal recovery process, the present invention provides a method for recovering and reusing spent hydrogenation catalysts. The method has the characteristics of simple metal recovery steps, less residual impurities, and high activity of the obtained new hydrogenation catalyst, and is particularly suitable for metal recovery and reuse of Ni(Co)-Mo series catalysts.
[0008] The present invention provides a method for recycling and reusing a waste hydrogenation catalyst, the method comprising the following steps:
[0009] (1) calcining the waste hydrogenation catalyst in an oxygen atmosphere; mixing the calcined product with an acid solution and heating to reflux;
[0010] (2) adjusting the pH value of the reflux product obtained in step (1) to 3.5-4.5 using an organic amine, and performing solid-liquid separation; the boiling point of the organic amine at normal pressure is greater than or equal to 100° C.;
[0011] (3) Using the liquid product filtered out in step (2) as an impregnation liquid to impregnate a carrier, and subjecting the carrier to heat treatment to obtain a regenerated hydrogenation catalyst.
[0012] According to the present invention, in step (1), the waste hydrogenation catalyst, based on the mass of the waste hydrogenation catalyst and measured by mass fraction, comprises:
[0013] 5% to 40% molybdenum, calculated as molybdenum trioxide;
[0014] 2% to 10% of at least one selected from nickel and cobalt, calculated as oxide;
[0015] Calculated as calcium oxide, 0.01% to 1.0% calcium;
[0016] 0.01% to 3.0% iron calculated as ferric oxide;
[0017] The content of S element is 3% to 15%;
[0018] 40% to 80% carrier.
[0019] According to the present invention, further, in step (1), the waste hydrogenation catalyst may contain 2.1% to 12.0% of carbon deposits.
[0020] According to the present invention, the carrier in step (1) is a conventional carrier; the carrier includes one or more of aluminum oxide, silicon oxide, amorphous silicon aluminum, and titanium-containing aluminum oxide.
[0021] According to the present invention, the calcination temperature in step (1) is 280-600° C., preferably 320-550° C., and the calcination time is 2-20 hours, preferably 2-12 hours.
[0022] According to the present invention, in the calcined product of step (1), the carbon deposit content is less than 2.0 wt %, preferably less than 0.6 wt %, by mass fraction.
[0023] According to the present invention, the acid solution in step (1) is a mixed acid solution of phosphoric acid and sulfuric acid. Further, in the mixed acid solution, the molar concentration of phosphoric acid is 0.1 to 3.0 mol / L, preferably 0.3 to 2.0 mol / L, and the molar concentration of sulfuric acid is 0.05 to 1.0 mol / L, preferably 0.1 to 0.6 mol / L.
[0024] According to the present invention, the volume ratio of the acid solution in step (1) to the mass ratio of the calcined product obtained in step (1) is 1:1 to 4:1 ml / g, preferably 1.5:1 to 3.0:1 ml / g.
[0025] According to the present invention, the temperature of the heating reflux in step (1) is 80 to 105° C., preferably 95 to 100° C.; the heating time is 2.0 to 12.0 hours, preferably 4.0 to 8.0 hours.
[0026] According to the present invention, in step (2), the pH value is adjusted after the reflux product is cooled to 30-50°C. The boiling point of the organic amine at normal pressure is greater than or equal to 100°C, preferably 100-300°C. Further, the organic amine includes at least one of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, dipropylamine, dibutylamine, pentamethylenediamine, and 1,2,3-propylenetriamine. Preferably, the organic amine in step (2) is added in the form of an organic amine solution, wherein the mass concentration of the organic amine solution is 2% to 20%, preferably 5% to 15%.
[0027] According to the present invention, the solid-liquid separation method in step (2) is suction filtration. Preferably, the mixture after adjusting the pH value is heated before suction filtration. The heating temperature is 50 to 100°C, preferably 60 to 70°C. The heating time is 0.5 to 4 hours, preferably 1 to 2 hours. During suction filtration, the temperature of the filtrate is controlled to 40 to 70°C, preferably 50 to 60°C. Preferably, water can be added for dilution during suction filtration. The amount of water used is 20% to 200% of the mass of the roasting product obtained in step (1), preferably 30% to 120%.
[0028] According to the present invention, preferably, in order to meet the requirements of the impregnation amount of hydrogenation catalysts for different reactions, the impregnation liquid in step (3) can be used as a mother liquid, and the mother liquid is adjusted so that the active metal content in the adjusted mother liquid is suitable for the hydrogenation catalytic reaction. The method for adjusting the mother liquid can be a well-known method such as adding an active metal source or adding water for dilution. The active metal source is at least one of a soluble salt of an active metal and a metal oxide. The active metal source includes a molybdenum source and at least one selected from a nickel source and a cobalt source. Conventional additives used in hydrogenation catalyst impregnation liquids can also be added to the impregnation liquid.
[0029] According to the present invention, preferably, in the impregnation solution obtained after adjusting the mother liquor in step (3), the content of metallic molybdenum element, calculated on an atom basis, is 0.5 to 5.0 mol / L, preferably 0.8 to 4.0 mol / L.
[0030] According to the present invention, preferably, in the impregnation solution obtained after adjusting the mother liquor in step (3), the content of metallic nickel and / or cobalt element is 0.2 to 2.0 mol / L, preferably 0.3 to 1.5 mol / L, in terms of atoms.
[0031] According to the present invention, the carrier in step (3) can be selected conventionally, preferably including one or more of aluminum oxide, silicon oxide, amorphous silicon aluminum, and titanium-containing aluminum oxide; in the titanium-containing aluminum oxide, the titanium-aluminum molar ratio is 0.1 to 0.4, calculated on an atomic basis.
[0032] According to the present invention, preferably, the specific surface area of the carrier is 150 to 500 m 2 / g, preferably 200-400m 2 / g, and the pore volume of the carrier is 0.2 to 1.2 cm 3 / g, 0.3~1.0cm 3 / g. The carrier may be doped with one or more of the modifying elements such as phosphorus, silicon, boron, fluorine, magnesium, sodium, zinc, etc. The amount of the modifying element added is a conventional amount, preferably accounting for 0.5% to 6.0% of the carrier mass.
[0033] According to the present invention, the method of impregnating the carrier in step (3) is one of the well-known unsaturated impregnation, equal volume impregnation, and supersaturated impregnation. The heat treatment method is at least one of drying and roasting; the atmosphere of the heat treatment can be an oxygen-containing or oxygen-free atmosphere. The conditions of the heat treatment are: the heat treatment temperature is 80 to 800°C, preferably 100 to 550°C, and the heat treatment time is 2 to 20 hours, preferably 4 to 15 hours.
[0034] Compared with the prior art, the present invention has the following advantages:
[0035] 1. In the present invention, the method for recycling and reusing the waste hydrogenation catalyst comprises the following steps: firstly, the industrial waste catalyst is calcined at low temperature, mainly to convert the sulfided metal into an oxidized state, and further, the carbon deposits covering the surface of the catalyst can be removed; then, an acid solution (preferably phosphoric acid or sulfuric acid) is added to the catalyst to remove Ca and destroy a part of the pores of the carrier to expose the metal more fully; high-temperature heating is performed, and a high-boiling-point organic amine is used to adjust the pH value of the solution to 3.5-4.5, and while ensuring the removal of the iron element, the phosphomolybdenum heteropolyacid is not hydrolyzed, so as to obtain a Ni(Co)-Mo impregnation solution substantially free of Ca and Fe ions, and further, by adding appropriate metals and additives, the solution can be used as an impregnation solution.
[0036] 2. The method of the present invention can directly convert the molybdenum and nickel (cobalt) metals on the waste catalyst into an impregnation solution that can be used to prepare a new hydrogenation catalyst, eliminating the cumbersome process of separating molybdenum and nickel (cobalt) into their respective oxides (or metal salts) and then dissolving them in the prior art, greatly improving the efficiency, with less residual impurities, and is particularly suitable for metal recovery and reuse of Ni (Co) -Mo series catalysts. On the other hand, the combination of the steps of precipitating metal ions with an acid solution and adjusting the pH value with a specific organic amine in the method of the present invention can efficiently remove iron and calcium impurities on the waste catalyst from the impregnation solution without affecting the content of the molybdenum metal element. The regenerated catalyst prepared from the recovered active metal-containing impregnation solution is suitable for hydrogenation catalyst reactions and has high activity. DETAILED DESCRIPTION
[0037] The method of the present invention is described in detail below by way of examples.
[0038] In the present invention, the alumina carrier A used in the following examples is prepared as follows: 3000g of aluminum hydroxide dry rubber powder, 30.0g of sesbania powder, 30.0g of cellulose, and 20.0g of citric acid are uniformly mixed, and then mixed with 2800g of 2% nitric acid solution by mass, and the mixture is kneaded for 20 minutes using a kneading machine, and extruded using an extruder, the extrusion pressure is 30.0MPa, and the orifice plate is a 1.6mm clover. The extruded carrier is dried at 120°C for 4.0 hours, calcined at 600°C for 4.0 hours, and shaped to a length of 3 to 8mm. The obtained alumina carrier is recorded as carrier A. The specific surface area of carrier A is 320m 2 / g, pore volume is 0.92cm 3 / g.
[0039] In the present invention, the analysis method of metal elements in the catalyst and the solution is: GB / T 38904-2020.
[0040] In the present invention, the analysis method for the carbon deposit content in the catalyst is: GB / T 14265-2017.
[0041] In the present invention, the calculation method of the utilization rate S (wt%) of a certain metal in the waste catalyst is:
[0042] S=(a×m1-b) / (c×m2)×100%
[0043] Wherein a is the mass of the newly prepared catalyst, m1 is the mass fraction of the metal in the new catalyst, b is the mass of the metal added in step (3), c is the mass of the spent catalyst, and m2 is the mass fraction of the metal in the spent catalyst.
[0044] Embodiment 1:
[0045] (1) 200.0 g of Mo-Ni hydrogenation catalyst, which was used in industry, was calcined in a muffle furnace at 450° C. for 4 hours. The calcined product was recorded as ZC-1.
[0046] The composition of the waste hydrogenation catalyst Mo-Ni hydrogenation treatment catalyst is: 20.71% of molybdenum calculated as molybdenum trioxide; 4.07% of nickel calculated as nickel oxide; 0.44% of calcium calculated as calcium oxide; 1.24% of iron calculated as ferric oxide; 8.22% of carbon deposits, 10.35% of sulfur, and the balance is carrier aluminum oxide.
[0047] In the calcined product, the carbon deposit content is 0.52 wt % by mass.
[0048] Deionized water, phosphoric acid and sulfuric acid were used to prepare a 200 ml solution. The obtained mixed acid solution was recorded as AQ-1, wherein the molar concentration of phosphoric acid was 0.4 mol / L, and the molar concentration of sulfuric acid was 0.2 mol / L.
[0049] Take 100.0g ZC-1, add 200ml mixed acid solution AQ-1, heat to reflux, control the heating temperature to 100℃, and the time is 6.0 hours.
[0050] (2) After stopping heating, cool to 40°C, slowly add 10% by mass ethylenediamine solution to the reflux product, measure the pH value of the solution during this period, and stop dropping when the pH value of the solution is 4.0. At this time, the mass of the added solution is 24.6g. Continue to heat the solution to 65°C for 1.0 hour. Filter the solution at a temperature between 50 and 60°C. During the filtration process, the amount of water added is 80.0g. The filtrate obtained is recorded as FQ-1.
[0051] (3) 4.5 g of molybdenum trioxide and 3.5 g of nickel nitrate hexahydrate were added to FQ-1 in step (2), and the mixture was heated and concentrated to 70.0 ml. The obtained impregnation solution was recorded as JQ-1. The content of the metal molybdenum element in the impregnation solution was 2.23 mol / L and the content of the metal nickel element was 0.86 mol / L in terms of atoms.
[0052] Take 70g of alumina carrier A, impregnate the above JQ-1 onto carrier A, dry at 120°C for 5 hours, and then calcine at 420°C for 4 hours. The obtained catalyst is recorded as CT-1.
[0053] Embodiment 2:
[0054] (1) Take 200.0 g of Mo-Ni hydrogenation catalyst, which is a waste hydrogenation catalyst used in industry, and calcine it in a muffle furnace at 450° C. for 4 hours. The calcined product is recorded as ZC-2.
[0055] The composition of the waste hydrogenation catalyst Mo-Ni hydrogenation treatment catalyst is: 34.98% of molybdenum calculated as molybdenum trioxide; 7.85% of nickel calculated as nickel oxide; 0.23% of calcium calculated as calcium oxide; 0.63% of iron calculated as ferric oxide; 7.54% of carbon deposits, 16.29% of sulfur, and the rest is carrier aluminum oxide.
[0056] In the calcined product of step (1), the carbon deposit content is 0.86wt% by mass.
[0057] Deionized water, phosphoric acid and sulfuric acid were used to prepare a 200 ml solution. The obtained mixed acid solution was recorded as AQ-2, wherein the molar concentration of phosphoric acid was 0.6 mol / L, and the molar concentration of sulfuric acid was 0.05 mol / L.
[0058] Take 100.0g ZC-2, add 200ml mixed acid solution AQ-2, heat to reflux, control the heating temperature to 100℃, and the time is 6.0 hours.
[0059] (2) After stopping heating, cool to 50°C, slowly add 10% by mass of 1,2,3-propanetriamine to the solution, measure the pH value of the solution during this period, and stop dropping when the pH value of the solution is 4.0. At this time, the mass of the added solution is 33.7g. Continue to heat the solution to 65°C for 1.0 hour. Filter the solution at a temperature between 50 and 60°C. During the filtration process, the amount of water added is 80.0g. The filtrate obtained is recorded as FQ-2.
[0060] (3) 4.5 g of molybdenum trioxide and 3.5 g of nickel nitrate hexahydrate were added to the above FQ-2, and the mixture was heated and concentrated to 70.0 ml. The obtained impregnation solution was recorded as JQ-2. That is, in the impregnation solution, the content of the metal molybdenum element was 3.25 mol / L and the content of the metal nickel element was 1.03 mol / L in terms of atoms.
[0061] Take 70.0 g of alumina carrier A, impregnate the above JQ-2 onto carrier A, dry at 120° C. for 5 hours, and then calcine at 420° C. for 4 hours. The obtained catalyst is recorded as CT-2.
[0062] Embodiment 3:
[0063] (1) 200.0 g of Mo-Ni hydrogenation catalyst, which was used in industry, was calcined in a muffle furnace at 450° C. for 4 hours. The calcined product was recorded as ZC-3.
[0064] The composition of the waste hydrogenation catalyst Mo-Ni hydrogenation treatment catalyst is: 14.56% of molybdenum calculated as molybdenum trioxide; 3.12% of nickel calculated as nickel oxide; 0.72% of calcium calculated as calcium oxide; 2.61% of iron calculated as ferric oxide; 9.58% of carbon deposits, 7.27% of sulfur, and the rest is carrier aluminum oxide.
[0065] In the calcined product of step (1), the carbon deposit content is 0.44 wt % by mass.
[0066] Deionized water, phosphoric acid and sulfuric acid were used to prepare a 200 ml solution. The obtained mixed acid solution was recorded as AQ-3, wherein the molar concentration of phosphoric acid was 0.30 mol / L, and the molar concentration of sulfuric acid was 0.40 mol / L.
[0067] Take 100.0g ZC-3, add 200ml mixed acid solution AQ-3, heat to reflux, control the heating temperature to 100℃, and the time is 6.0 hours.
[0068] (2) After stopping heating, cool to 50°C, slowly add 10% by mass of 1,2,3-propanetriamine to the solution, measure the pH value of the solution during this period, and stop dropping when the pH value of the solution is 4.0. At this time, the mass of the added solution is 28.8g. Continue to heat the solution to 65°C for 1.0 hour. Filter the solution at a temperature between 50 and 60°C. During the filtration process, the amount of water added is 80.0g. The filtrate obtained is recorded as FQ-3.
[0069] (3) 4.5 g of molybdenum trioxide and 3.5 g of nickel nitrate hexahydrate were added to the above FQ-3, and the mixture was heated and concentrated to 70.0 ml. The obtained impregnation solution was recorded as JQ-3. That is, in the impregnation solution, the content of the metal molybdenum element was 1.69 mol / L and the content of the metal nickel element was 0.71 mol / L in terms of atoms.
[0070] Take 70.0 g of alumina carrier A, impregnate the above JQ-3 onto carrier A, dry at 120° C. for 5 hours, and then calcine at 420° C. for 4 hours. The obtained catalyst is recorded as CT-3.
[0071] Embodiment 4:
[0072] (1) Take 200.0 g of industrial waste hydrogenation catalyst Mo-Co hydrogenation treatment catalyst and calcine it in a muffle furnace at 450° C. for 4 hours. The calcined product is recorded as ZC-4.
[0073] The composition of the waste hydrogenation catalyst Mo-Co hydrogenation treatment catalyst is: 21.08% of molybdenum calculated as molybdenum trioxide; 4.23% of cobalt calculated as cobalt oxide; 0.50% of calcium calculated as calcium oxide; 1.46% of iron calculated as ferric oxide; 6.84% of carbon deposits, 11.22% of sulfur, and the balance is carrier aluminum oxide.
[0074] In the calcined product of step (1), the carbon deposit content is 0.59wt% by mass.
[0075] Deionized water, phosphoric acid and sulfuric acid were used to prepare a 200 ml solution. The obtained mixed acid solution was recorded as AQ-4, wherein the molar concentration of phosphoric acid was 0.40 mol / L, and the molar concentration of sulfuric acid was 0.20 mol / L.
[0076] Take 100.0g ZC-4, add 200ml AQ-3, heat to reflux, control the heating temperature to 100℃, and the time is 6.0 hours. After stopping heating, cool to 50℃, slowly add 10% by mass dibutylamine to the solution, measure the pH value of the solution during the process, and stop dropping when the pH value of the solution is 3.5. The mass of the solution added is 40.1g. Continue to heat the solution to 65℃ for 1.0 hour. Filter the solution at a temperature between 50 and 60℃. During the filtration process, add 80.0g of water, and the filtrate obtained is recorded as FQ-4.
[0077] (3) 4.5 g of molybdenum trioxide and 3.5 g of cobalt nitrate hexahydrate were added to FQ-4, and the mixture was heated and concentrated to 70.0 ml. The obtained impregnation solution was recorded as JQ-4. That is, in the impregnation solution, the content of the metal molybdenum element was 2.25 mol / L, and the content of the metal cobalt element was 0.86 mol / L in terms of atoms.
[0078] Take 70.0 g of alumina carrier A, impregnate JQ-4 onto carrier A, dry at 120° C. for 5 hours, and then calcine at 420° C. for 4 hours. The resulting catalyst is recorded as CT-4.
[0079] Embodiment 5:
[0080] (1) 200.0 g of Mo-Co hydrogenation catalyst, a waste hydrogenation catalyst used in industry, was calcined in a muffle furnace at 450° C. for 4 hours. The calcined product was recorded as ZC-5.
[0081] The composition of the waste hydrogenation catalyst Mo-Co hydrogenation treatment catalyst is: 21.08% of molybdenum calculated as molybdenum trioxide; 4.23% of cobalt calculated as cobalt oxide; 0.50% of calcium calculated as calcium oxide; 1.46% of iron calculated as ferric oxide; 6.84% of carbon deposits, 11.22% of sulfur, and the balance is carrier aluminum oxide.
[0082] In the calcined product of step (1), the carbon deposit content is 0.5 wt % by mass.
[0083] Deionized water, phosphoric acid and sulfuric acid were used to prepare a 200 ml solution. The obtained mixed acid solution was recorded as AQ-5, wherein the molar concentration of phosphoric acid was 0.45 mol / L, and the molar concentration of sulfuric acid was 0.25 mol / L.
[0084] Take 100.0g ZC-5, add 200ml AQ-5, heat to reflux, control the heating temperature to 100℃, and the time is 6.0 hours. After stopping heating, cool to 50℃, slowly add 10% pentamethylenediamine by mass to the solution, measure the pH value of the solution during the process, and stop dropping when the pH value of the solution is 4.5. The mass of the solution added is 48.2g. Continue to heat the solution to 65℃ for 1.0 hour. Filter the solution at a temperature between 50 and 60℃. During the filtration process, add 80.0g of water, and the filtrate obtained is recorded as FQ-5.
[0085] 4.5 g of molybdenum trioxide and 3.5 g of cobalt nitrate hexahydrate were added to FQ-5, and the mixture was heated and concentrated to 70.0 ml. The obtained impregnation solution was recorded as JQ-5. That is, in the impregnation solution, the content of the metal molybdenum element was 2.30 mol / L and the content of the metal cobalt element was 0.87 mol / L in terms of atoms.
[0086] Take 70.0 ml of alumina carrier A, impregnate JQ-5 onto carrier A, dry at 120°C for 5 hours, and then calcine at 420°C for 4 hours. The obtained catalyst is recorded as CT-5.
[0087] Comparative Example 1:
[0088] (1) 200.0 g of industrially used Mo-Ni hydrogenation catalyst was calcined in a muffle furnace at 450° C. for 4 hours. The calcined product was recorded as DZC-1.
[0089] The composition of the waste hydrogenation catalyst Mo-Ni hydrogenation treatment catalyst is: 20.71% of molybdenum calculated as molybdenum trioxide; 4.07% of nickel calculated as nickel oxide; 0.44% of calcium calculated as calcium oxide; 1.24% of iron calculated as ferric oxide; 8.22% of carbon deposits, 10.35% of sulfur, and the balance is carrier aluminum oxide.
[0090] In the calcined product of step (1), the carbon deposit content is 0.52 wt % by mass.
[0091] Take 100.0g DZC-1, add 200ml deionized water, heat to reflux, control the heating temperature to 100℃, and the time is 6.0 hours.
[0092] (2) After stopping heating, the solution was filtered at a temperature between 50 and 60°C. During the filtration process, 80.0 g of water was added. The filtrate obtained was recorded as DFQ-1.
[0093] (3) Add nickel and molybdenum elements to DFQ-1 in step (2) in the same amount as that in step (3) of Example 1, heat and concentrate to 70.0 ml. The resulting impregnation solution is recorded as DJQ-1.
[0094] Take 70.0 ml of alumina carrier A, impregnate DJQ-1 onto carrier A, dry at 120°C for 5 hours, and then calcine at 420°C for 4 hours. The obtained catalyst is recorded as DCT-1.
[0095] Comparative Example 2:
[0096] (1) Take 200.0 g of industrial waste Mo-Ni hydroprocessing catalyst and calcine it in a muffle furnace at 450° C. for 4 hours. The calcined product is recorded as DZC-2.
[0097] The composition of the waste hydrogenation catalyst Mo-Ni hydrogenation treatment catalyst is: 20.71% of molybdenum calculated as molybdenum trioxide; 4.07% of nickel calculated as nickel oxide; 0.44% of calcium calculated as calcium oxide; 1.24% of iron calculated as ferric oxide; 8.22% of carbon deposits, 10.35% of sulfur, and the balance is carrier aluminum oxide.
[0098] In the calcined product of step (1), the carbon deposit content is 0.52 wt % by mass.
[0099] Deionized water and phosphoric acid were used to prepare a 200 ml solution, and the obtained mixed acid solution was recorded as DAQ-2, wherein the molar concentration of phosphoric acid was 0.4 mol / L.
[0100] Take 100.0g DZC-2, add 200ml DAQ-2, heat to reflux, control the heating temperature to 100℃, and keep the heating time for 6.0 hours.
[0101] (2) After stopping heating, the solution was cooled and filtered at a temperature between 50 and 60°C. During the filtration process, 80.0 g of water was added. The filtrate obtained was recorded as DFQ-2.
[0102] (3) Add nickel and molybdenum elements to DFQ-2 in the same amount as that in step (3) of Example 1, heat and concentrate to 70.0 ml. The resulting impregnation solution is recorded as DJQ-2.
[0103] Take 70.0 g of alumina carrier A, impregnate DJQ-2 onto carrier A, dry at 120° C. for 5 hours, and then calcine at 420° C. for 4 hours. The resulting catalyst is recorded as DCT-2.
[0104] Comparative Example 3:
[0105] (1) 200.0 g of Mo-Ni hydrogenation catalyst, which was used in industry, was calcined in a muffle furnace at 450° C. for 10 hours. The calcined product was recorded as DZC-3.
[0106] The composition of the waste hydrogenation catalyst Mo-Ni hydrogenation treatment catalyst is: 20.71% of molybdenum calculated as molybdenum trioxide; 4.07% of nickel calculated as nickel oxide; 0.44% of calcium calculated as calcium oxide; 1.24% of iron calculated as ferric oxide; 8.22% of carbon deposits, 10.35% of sulfur, and the balance is carrier aluminum oxide.
[0107] In the calcined product of step (1), the carbon deposit content is 0.52 wt % by mass.
[0108] Deionized water, phosphoric acid and sulfuric acid were used to prepare a 200 ml solution, and the obtained mixed acid solution was recorded as DAQ-3, wherein the molar concentration of phosphoric acid was 0.4 mol / L, and the molar concentration of sulfuric acid was 0.2 mol / L.
[0109] Take 100.0g DZC-3, add 200ml DAQ-3, heat to reflux, control the heating temperature to 100℃, and keep the heating time for 6.0 hours.
[0110] (2) After stopping heating, the pH of the mixed solution was tested to be 1.0. The solution was filtered at a temperature between 50 and 60°C. During the filtration process, 80.0 g of water was added. The filtrate obtained was recorded as DFQ-3.
[0111] Nickel and molybdenum elements were added to DFQ-3 in the same amount as that in step (3) of Example 1, and heated to concentrate to 70.0 ml. The obtained impregnation solution was recorded as DJQ-3.
[0112] Take 70.0g of alumina carrier A, impregnate DJQ-3 on carrier A, dry at 120℃ for 5 hours, and then calcine at 420℃ for 4 hours. The obtained catalyst is recorded as DCT-3. The weight of DCT-3 is 98.9g
[0113] Comparative Example 4:
[0114] Take 23.0g of molybdenum trioxide, 17.0g of nickel nitrate hexahydrate, 5.0g of 85% phosphoric acid, and 100ml of deionized water, heat at 100°C for 6 hours, evaporate and concentrate to 70.0ml, and the prepared solution is recorded as DJQ-4. That is, in the impregnation solution, the content of metal molybdenum element is 2.28mol / L, and the content of metal nickel element is 0.84mol / L in terms of atoms.
[0115] Take 70.0 g of alumina carrier A, impregnate DJQ-4 onto carrier A, dry at 120° C. for 5 hours, and then calcine at 420° C. for 4 hours. The resulting catalyst is recorded as DCT-4.
[0116] Comparative Example 5:
[0117] Take 23.0g of molybdenum trioxide, 17.0g of cobalt nitrate hexahydrate, 5.0g of 85% phosphoric acid, and 100ml of deionized water, heat at 100°C for 6 hours, evaporate and concentrate to 70.0ml, and the prepared solution is recorded as DJQ-5. That is, in the impregnation solution, the content of metal molybdenum element is 2.28mol / L, and the content of metal cobalt element is 0.83mol / L in terms of atoms.
[0118] Take 70.0 g of alumina carrier A, impregnate DJQ-5 onto carrier A, dry at 120° C. for 5 hours, and then calcine at 420° C. for 4 hours. The obtained catalyst is recorded as DCT-5.
[0119] Comparative Example 6:
[0120] (1) Take 200.0 g of Mo-Ni hydrogenation catalyst, which is a waste hydrogenation catalyst used in industry, and calcine it in a muffle furnace at 450° C. for 4 hours. The calcined product is recorded as DZC-6.
[0121] The composition of the waste hydrogenation catalyst Mo-Ni hydrogenation treatment catalyst is: 20.71% of molybdenum calculated as molybdenum trioxide; 4.07% of nickel calculated as nickel oxide; 0.44% of calcium calculated as calcium oxide; 1.24% of iron calculated as ferric oxide; 8.22% of carbon deposits, 10.35% of sulfur, and the balance is carrier aluminum oxide.
[0122] In the calcined product, the carbon deposit content is 0.52 wt % by mass.
[0123] Deionized water, phosphoric acid and sulfuric acid were used to prepare a 200 ml solution. The obtained mixed acid solution was recorded as DAQ-6, wherein the molar concentration of phosphoric acid was 0.4 mol / L, and the molar concentration of sulfuric acid was 0.2 mol / L.
[0124] Take 100.0g DZC-6, add 200ml mixed acid solution DAQ-6, heat to reflux, control the heating temperature to 100℃, and the time is 6.0 hours.
[0125] (2) After stopping heating, cool to 40°C, slowly add 10% by mass diethylamine solution to the reflux product, measure the pH value of the solution during this period, and stop adding when the pH value of the solution is 4.0. Continue to heat the solution to 65°C for 1.0 hour. Filter the solution at a temperature between 50 and 60°C. During the filtration process, add 80.0 g of water. The filtrate obtained is recorded as DFQ-6.
[0126] (3) Add nickel and molybdenum elements to the DFQ-6 in step (2) in the same amount as that in step (3) of Example 1, heat and concentrate to 70.0 ml. The resulting impregnation solution is recorded as DJQ-6.
[0127] Take 70g of alumina carrier A, impregnate the above DJQ-6 onto carrier A, dry at 120°C for 5 hours, and then calcine at 420°C for 4 hours. The obtained catalyst is recorded as DCT-6.
[0128] Table 1 shows the metal content in the catalyst finally obtained in each of the above examples. Table 2 shows the metal recovery rate of each corresponding example.
[0129] Table 1 Metal content in the final catalyst obtained in each example
[0130]
[0131]
[0132] Table 2 Utilization rate of active metals in waste catalysts in various cases
[0133] Mo, wt% Ni, wt% Co, wt% Example 1 84.18 90.79 - Example 2 80.85 86.57 Example 3 86.14 91.39 Example 4 80.96 - 84.59 Example 5 82.89 - 87.53 Comparative Example 1 20.08 19.22 - Comparative Example 2 86.59 93.07 - Comparative Example 3 84.62 90.9 - Comparative Example 6 82.06 91.11 -
[0134] The catalysts prepared in the examples and comparative examples were experimentally evaluated. The evaluation method was as follows: the catalyst was sieved, 20 ml of 20-30 mesh particles were taken, mixed with 20 ml of quartz sand of the same mesh size in a 1:1 ratio, and then loaded into a reaction tube. The reaction raw material was VGO, and the properties were shown in Table 2.
[0135] Before evaluation, the catalyst was subjected to in-situ sulfurization under the following conditions: 5% DMDS cyclohexane solution, 6.0 MPa liquid pressure, 1.5 h liquid hourly space velocity -1 , hydrogen-oil volume ratio 500:1, first stage of vulcanization, temperature 230℃, duration 5.0h, second stage of vulcanization, temperature 340℃, duration 3.0h. After the vulcanization, the temperature of the reaction tube was lowered to room temperature, and then the raw materials were switched to conduct reaction evaluation.
[0136] The reaction evaluation conditions were 370°C, reaction pressure 15.0 MPa, liquid hourly space velocity 1.0 h -1 , hydrogen-to-oil volume ratio 1000:1, after 300h of reaction, the samples were sampled and analyzed. The properties of the samples after hydrogenation reaction are shown in Table 3.
[0137] Table 3 VGO raw material properties
[0138]
[0139] Table 4 Properties of products after hydrogenation reaction
[0140]
[0141] From the analysis and evaluation results of the metal content of the catalyst, it can be seen that the method of the embodiment of the present invention can effectively utilize more than 80% of valuable metals such as Mo, Ni, Co, etc. in the waste catalyst, and can effectively prevent Ca and Fe impurities from entering the solution. The catalytic activity of the hydrogenation catalyst prepared from the impregnation solution is comparable to that of the catalyst prepared from fresh raw materials under the same metal loading. Compared with the comparative example, the method of the embodiment of the present invention has a significant advantage in the utilization rate of metals in the waste catalyst.
Claims
1. A method for recycling and reusing a waste hydrogenation catalyst, the method comprising the following steps: (1) calcining the spent hydrogenation catalyst in an oxygen atmosphere; mixing the calcined product with an acid solution and heating to reflux; (2) adjusting the pH value of the reflux product obtained in step (1) to 3.5-4.5 using an organic amine, and performing solid-liquid separation; (3) using the liquid product filtered out in step (2) as an impregnation liquid to impregnate the carrier, and subjecting the impregnation liquid to heat treatment to obtain a regenerated hydrogenation catalyst; The acid solution in step (1) is a mixed acid solution of phosphoric acid and sulfuric acid, wherein: The molar concentration of phosphoric acid is 0.1~3.0 mol / L, and the molar concentration of sulfuric acid is 0.05~1.0 mol / L; The boiling point of the organic amine in step (2) at normal pressure is 100-300°C; In step (1), the waste hydrogenation catalyst, based on the mass of the catalyst, comprises: 5% to 40% molybdenum calculated as molybdenum trioxide; 2% to 10% of at least one selected from nickel and cobalt, calculated as oxide; Calcium, 0.01% to 1.0% as calcium oxide; 0.01% to 3.0% iron as ferric oxide; The sulfur content is 3%~15%; 50%~80% carrier.
2. The method according to claim 1, characterized in that: The organic amine in step (2) includes at least one of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, dipropylamine, dibutylamine and pentamethylenediamine.
3. The method according to claim 2, characterized in that: The organic amine is added in the form of an organic amine solution, wherein the mass concentration of the organic amine solution is 2% to 20%.
4. The method according to claim 3, characterized in that: The mass concentration of the organic amine solution is 5%~15%.
5. The method according to claim 1, characterized in that: In step (2), the mixture is heated before solid-liquid separation; the heating temperature is 50-100° C.; and the heating time is 0.5-4 hours.
6. The method according to claim 5, characterized in that: In step (2), the mixture is heated before solid-liquid separation; the heating temperature is 60-70° C.; and the heating time is 1-2 hours.
7. The method according to claim 1, characterized in that: The solid-liquid separation method in step (2) is suction filtration; during suction filtration, the temperature of the filtrate is controlled to be 40-70°C.
8. The method according to claim 7, characterized in that: The solid-liquid separation method in step (2) is suction filtration; during suction filtration, the temperature of the filtrate is controlled to be 50-60°C.
9. The method according to claim 1, characterized in that: In step (1), the waste hydrogenation catalyst also contains 2.1% to 12.0% of carbon deposits.
10. The method according to claim 1, characterized in that: In the calcined product of step (1), the carbon deposit content is less than 2.0 wt % by mass.
11. The method according to claim 10, characterized in that: In the calcined product of step (1), the carbon deposit content is less than 0.6 wt % by mass.
12. The method according to claim 1, characterized in that: The molar concentration of phosphoric acid in step (1) is 0.3-2.0 mol / L, and the molar concentration of sulfuric acid is 0.1-0.6 mol / L; and / or the mass ratio of the volume of the acid solution in step (1) to the calcined product is 1:1-4:1 ml / g.
13. The method according to claim 1 or 12, characterized in that: The heating reflux temperature in step (1) is 80-105° C. and the heating time is 2.0-12.0 hours.
14. The method according to claim 1 or 12, characterized in that: The heating reflux temperature in step (1) is 95-100° C. and the heating time is 4.0-8.0 hours.
15. The method according to claim 1, characterized in that: The impregnation liquid in step (3) is used as a mother liquid, and the mother liquid is adjusted so that the active metal content in the adjusted mother liquid is suitable for hydrogenation catalytic reaction, wherein the adjustment method is to add an active metal source or to dilute it with water.
16. The method according to claim 15, characterized in that: In the impregnation solution obtained after adjusting the mother liquor in step (3), the content of the metal molybdenum element is 0.5-5.0 mol / L in terms of atoms; the content of the metal nickel and / or cobalt element is 0.2-2.0 mol / L.
17. The method according to claim 16, characterized in that: In the impregnation solution obtained after adjusting the mother liquor in step (3), the content of the metal molybdenum element is 0.8-4.0 mol / L in terms of atoms; and the content of the metal nickel and / or cobalt element is 0.3-1.5 mol / L.
18. The method according to claim 1, characterized in that: The carrier in step (3) includes one or more of aluminum oxide, silicon oxide, amorphous silicon aluminum, and titanium-containing aluminum oxide.
19. The method according to claim 1 or 18, characterized in that: The specific surface area of the carrier in step (3) is 150-500 m 2 / g, and the pore volume of the carrier is 0.2-1.2 cm 3 / g.
20. The method according to claim 1, characterized in that: The specific surface area of the carrier in step (3) is 200-400 m 2 / g, and the pore volume of the carrier is 0.3-1.0 cm 3 / g.
21. The method according to claim 1, characterized in that: The heat treatment conditions in step (3) are as follows: the heat treatment temperature is 80-800° C. and the heat treatment time is 2-20 hours.
22. The method according to claim 21, characterized in that: The heat treatment conditions in step (3) are: the heat treatment temperature is 100-550° C., and the heat treatment time is 4-15 hours.