A non-sintering dehydration carbonization method for preparing hard carbon and its application

The hard carbon material prepared by the non-sintering dehydration carbonization method solves the problem of insufficient electrochemical activity in sodium-ion batteries, achieves high specific capacity and good cycle stability, and is suitable for sodium-ion batteries and other battery types.

CN116062735BActive Publication Date: 2024-10-29PINGYU ZHONGXING ENERGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310273700.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-29
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

Existing carbon materials have insufficient electrochemical activity in sodium-ion batteries, especially the unfavorable interlayer spacing of Na+ ions embedded in graphite, which limits their application in sodium-ion batteries.

Method used

The non-sintered dehydration carbonization method is used to prepare hard carbon materials with rich defects and unique pore structure by dissolving organic matter in deionized water to form a high-concentration supersaturated solution, followed by dropping a strong oxidant and performing centrifugal cleaning and drying.

Benefits of technology

The prepared hard carbon material has excellent electrochemical properties and is suitable for sodium-ion battery negative electrodes. It shows high specific capacity and good cycle stability and is suitable for sodium-ion batteries, lithium-ion batteries and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116062735B_ABST
    Figure CN116062735B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of new energy storage materials, specifically a non-sintering dehydration carbonization method for preparing hard carbon and its application. The method comprises the steps of 1) dissolving a large amount of organic matter in a small amount of deionized water until a supersaturated solution is formed; 2) adding a strong oxidant dropwise to the product obtained in step 1) to obtain a hard carbon product; 3) washing the obtained product with deionized water by centrifugation and drying to obtain a hard carbon material. The prepared material has relatively excellent electrochemical properties, and the preparation process is simple and low-cost, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy storage materials, and specifically relates to a non-sintering dehydration carbonization method for preparing hard carbon and application thereof. Background Art

[0002] Carbon has abundant allotropes, such as diamond, graphite, amorphous carbon, carbon nanotubes, graphene, and carbonyne. Due to its excellent performance and wide application, it has always been a hot research topic. Therefore, it is very important to explore new carbon allotropes with different spatial arrangements of carbon atoms, which will bring new properties, functions, and applications. For example, graphite is the most commonly used anode material for commercial lithium-ion batteries (LIBs), but has almost no electrochemical activity for sodium-ion batteries (SIBs) because Na + Ion insertion into graphite interlayer spacing (0.335 nm) is thermodynamically unfavorable.

[0003] Hard carbon is generally considered to be non-graphitizable carbon or disordered carbon, in which randomly oriented small-sized pseudo-graphites with fingerprint layer stacking are formed by sp 3 The hybridized carbon atoms are fixed by strong cross-linking and cannot form a real graphic structure even at temperatures above 3000 ° C. It has a large interlayer spacing of more than 0.37 nm between the stacked graphene layers, which is conducive to the Na + The intercalation / deintercalation of ions and the favorable capacity displayed make it one of the most promising anode materials for SIBs. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a non-sintering dehydration carbonization method, by which a hard carbon material is obtained. In this method, the raw material cost is low, the preparation method is simple and easy, and it can provide excellent performance as an electrode material and has broad application prospects.

[0005] In order to achieve the above invention object, the specific technical solution of the present invention is:

[0006] A non-sintering dehydration carbonization method, by which a hard carbon material is prepared, comprises the following steps:

[0007] 1) Dissolve a large amount of organic matter in a small amount of deionized water until a supersaturated solution is formed;

[0008] 2) adding a strong oxidant to the product obtained in step (1) to obtain a hard carbon product;

[0009] 3) The product obtained in step (2) is centrifugally cleaned with deionized water and dried to obtain a hard carbon material.

[0010] As a preferred embodiment of the present application, the organic matter in step 1) is any one of sucrose, glucose, trehalose, ketohexose or starch.

[0011] As a preferred embodiment of the present application, the ratio of organic matter to deionized water is 0.5 g:1 mL to 4 g:1 mL.

[0012] As a better implementation in the present application, the strong oxidant in step 2) is sulfuric acid.

[0013] As a preferred embodiment of the present application, the ratio of the strong oxidant to the product obtained in step (1) is 0.1 mL: 1 g-1 mL: 1 g; more preferably 1 mL: 1 g.

[0014] As a preferred embodiment of the present application, the centrifugal speed in step 3) is 3000-12000 rpm, the time is 3-10 minutes, and the drying temperature is 60-120°C.

[0015] Another invention objective of the present application is to protect a hard carbon material obtained by adopting any one of the above technical solutions or any combination of the technical solutions.

[0016] The present invention also provides an application of the hard carbon material prepared by the above method, and the hard carbon material can be used as a negative electrode material for sodium ion batteries. For example, it is used to prepare a hard carbon negative electrode for sodium ion batteries. In the activation process of 100mA / g, the first efficiency is 75.6% and the specific capacity is 263mAh / g. At a current density of 1A / g, the specific capacity is 165mAh / g, indicating that the material has excellent electrochemical properties.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (i) In this method, a highly concentrated supersaturated solution is used, and then a strong oxidizing agent and water are used to generate high temperatures to carbonize organic matter to obtain a hard carbon material. The hard carbon material prepared by this method has abundant defects, which can enhance the electrochemical properties of the material.

[0019] (ii) The hard carbon material prepared by this method has rich closed-pore structure, more defects, good physical and chemical properties, unique pore structure and excellent conductivity, so it can be better used in lithium-ion batteries, sodium-ion batteries, lithium / sodium-sulfur batteries, lithium / sodium-selenium batteries, aqueous batteries, air batteries, sensors, environmental purification, energy, catalysis and other important fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the SEM image of hard carbon material 1# obtained in Example 1.

[0021] Figure 2 This is the TEM image of hard carbon material 1# obtained in Example 1.

[0022] Figure 3 These are the XPS graphs of hard carbon materials 1#, 2#, 3#, 4#, and 5# obtained in Examples 1, 2, 3, 4, and 5.

[0023] Figure 4 These are the XRD patterns of hard carbon materials 1#, 2#, 3#, 4#, and 5# obtained in Examples 1, 2, 3, 4, and 5.

[0024] Figure 5 This is the Raman graph of the hard carbon material 1# obtained in Example 1.

[0025] Figure 6 This is the first cycle charge and discharge curve of the hard carbon material 1# obtained in Example 1.

[0026] Figure 7 The hard carbon material 1# obtained in Example 1 is 1A g -1 Cyclic curves at current density of .

[0027] Figure 8 The charge and discharge curves of the hard carbon material 1# obtained in Example 1 at different numbers of cycles at a current density of 1 A / g.

[0028] Fig. 9 This is the CV curve of the hard carbon material 1# obtained in Example 1 at a scan rate of 0.1 mV / s. DETAILED DESCRIPTION

[0029] In order to make the content of the present invention easier to understand, the process described in the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments.

[0030] In the following examples, the inert atmosphere described is argon atmosphere. The reagents used in this application are all commercially available products.

[0031] Embodiment 1:

[0032] A non-sintering dehydration carbonization method comprises the following steps:

[0033] (1) Dissolve 20 g of sucrose in 20 mL of deionized water to form a highly concentrated supersaturated solution;

[0034] (2) adding 20 mL of sulfuric acid (12 M) dropwise to the obtained product to obtain a hard carbon product;

[0035] (3) The obtained product was centrifuged at 12000 rpm for 5 minutes with deionized water, and the process was repeated 4 times. The material was then transferred to a forced air drying oven at 70°C until dried to obtain hard carbon material 1#.

[0036] The hard carbon material was prepared by the same method and steps as in Example 1, except that the volume of sulfuric acid was replaced with 10 mL, 30 mL, 40 mL, 50 mL or 100 mL respectively. The specific performance data are shown in Table 1:

[0037] Table 1:

[0038]

[0039] The hard carbon material was prepared by the same method and steps as in Example 1, except that sulfuric acid was replaced by hydrochloric acid or nitric acid. However, no reaction occurred.

[0040] Embodiment 2:

[0041] A non-sintering dehydration carbonization method comprises the following steps:

[0042] (1) Dissolve 20 g of glucose in 20 mL of deionized water to form a highly concentrated supersaturated solution;

[0043] (2) adding 20 mL of sulfuric acid (12 M) dropwise to the obtained product to obtain a hard carbon product;

[0044] (3) The obtained product was centrifuged at 12000 rpm for 5 minutes with deionized water, and the process was repeated 4 times. The material was then transferred to a forced air drying oven at 70° C. until dried to obtain hard carbon material 2#.

[0045] The hard carbon material was prepared by the same method and steps as in Example 2, except that the volume of sulfuric acid was replaced with 10 mL, 30 mL, 40 mL, 50 mL or 100 mL. The specific performance data are shown in Table 2:

[0046] Table 2:

[0047]

[0048] The hard carbon material was prepared by the same method and steps as in Example 2, except that sulfuric acid was replaced by hydrochloric acid or nitric acid, respectively. However, no reaction occurred.

[0049] Embodiment 3:

[0050] A non-sintering dehydration carbonization method comprises the following steps:

[0051] (1) Dissolve 20 g of trehalose in 20 mL of deionized water to form a high concentration supersaturated solution;

[0052] (2) adding 20 mL of sulfuric acid (12 M) dropwise to the obtained product to obtain a hard carbon product;

[0053] (3) The obtained product was centrifuged at 12000 rpm for 5 minutes with deionized water, and the process was repeated 4 times. The material was then transferred to a forced air drying oven at 70°C until dried to obtain hard carbon material 3#.

[0054] The hard carbon material was prepared by the same method and steps as in Example 3, except that the volume of sulfuric acid was replaced with 10 mL, 30 mL, 40 mL, 50 mL or 100 mL. The specific performance data are shown in Table 3:

[0055] Table 3

[0056]

[0057] The hard carbon material was prepared by the same method and steps as in Example 3, except that sulfuric acid was replaced by hydrochloric acid or nitric acid, respectively. However, no reaction occurred.

[0058] Embodiment 4:

[0059] A non-sintering dehydration carbonization method comprises the following steps:

[0060] (1) Dissolve 20 g of ketohexose in 20 mL of deionized water to form a highly concentrated supersaturated solution;

[0061] (2) adding 20 mL of sulfuric acid (12 M) dropwise to the obtained product to obtain a hard carbon product;

[0062] (3) The obtained product was centrifuged at 12000 rpm for 5 minutes with deionized water, and the process was repeated 4 times. The material was then transferred to a forced air drying oven at 70°C until dried to obtain hard carbon material 4#.

[0063] The hard carbon material was prepared by the same method and steps as in Example 4, except that the volume of sulfuric acid was replaced with 10 mL, 30 mL, 40 mL, 50 mL or 100 mL respectively. The specific performance data are shown in Table 4:

[0064] Table 4:

[0065]

[0066] The hard carbon material was prepared by the same method and steps as in Example 4, except that sulfuric acid was replaced by hydrochloric acid or nitric acid, respectively. However, no reaction occurred.

[0067] Embodiment 5:

[0068] A non-sintering dehydration carbonization method comprises the following steps:

[0069] (1) Dispersing 20 g of starch in 20 mL of deionized water to form a highly concentrated supersaturated solution;

[0070] (2) adding 20 mL of sulfuric acid (12 M) dropwise to the obtained product to obtain a hard carbon product;

[0071] (3) The obtained product was centrifuged at 12000 rpm for 5 minutes with deionized water, and the process was repeated 4 times. The material was then transferred to a forced air drying oven at 70°C until dried to obtain hard carbon material 5#.

[0072] The hard carbon material was prepared by the same method and steps as in Example 5, except that the volume of sulfuric acid was replaced with 10 mL, 30 mL, 40 mL, 50 mL or 100 mL respectively. The specific performance data are shown in Table 5:

[0073] Table 5:

[0074]

[0075] The hard carbon material was prepared by the same method and steps as in Example 5, except that sulfuric acid was replaced by hydrochloric acid or nitric acid, respectively. However, no reaction occurred.

[0076] Comparative Example 1:

[0077] The method for preparing hard carbon materials by solid phase method is prepared according to the following steps:

[0078] Sucrose was pyrolyzed at 1300°C in an inert atmosphere for 3 hours with a heating rate of 3°C per minute to obtain a hard carbon material.

[0079] The hard carbon material was prepared by the same method and steps as in Comparative Example 1, except that the pyrolysis temperature was replaced with 900, 1100, 1500 or 1700° C. The specific performance data are shown in Table 6

[0080] Table 6:

[0081]

[0082] Comparative Example 2:

[0083] The method for preparing hard carbon materials by solid phase method is prepared according to the following steps:

[0084] Glucose was pyrolyzed at 1300°C in an inert atmosphere for 3 hours at a heating rate of 3°C per minute to obtain a hard carbon material.

[0085] The hard carbon material was prepared by the same method and steps as in Comparative Example 2, except that the pyrolysis temperature was replaced with 900, 1100, 1500 or 1700° C. The specific performance data are shown in Table 7:

[0086] Table 7:

[0087]

[0088] Comparative Example 3:

[0089] The method for preparing hard carbon materials by solid phase method is prepared according to the following steps:

[0090] Trehalose was pyrolyzed at 1300°C in an inert atmosphere for 3 hours at a heating rate of 3°C per minute to obtain a hard carbon material.

[0091] The hard carbon material was prepared by the same method and steps as in Comparative Example 3, except that the pyrolysis temperature was replaced with 900, 1100, 1500 or 1700° C. The specific performance data are shown in Table 8:

[0092] Table 8:

[0093]

[0094] Comparative Example 4:

[0095] The method for preparing hard carbon materials by solid phase method is prepared according to the following steps:

[0096] Ketohexose was pyrolyzed at 1300°C in an inert atmosphere for 3 hours with a heating rate of 3°C per minute to obtain a hard carbon material.

[0097] The hard carbon material was prepared by the same method and steps as in Comparative Example 4, except that the pyrolysis temperature was replaced with 900, 1100, 1500 or 1700° C. The specific performance data are shown in Table 9:

[0098] Table 9:

[0099]

[0100] Comparative Example 5:

[0101] The method for preparing hard carbon materials by solid phase method is prepared according to the following steps:

[0102] The starch was pyrolyzed at 1300°C in an inert atmosphere for 3 hours with a heating rate of 3°C per minute to obtain a hard carbon material.

[0103] The hard carbon material was prepared by the same method and steps as in Comparative Example 5, except that the pyrolysis temperature was replaced with 900, 1100, 1500 or 1700° C. The specific performance data are shown in Table 10:

[0104] Table 10:

[0105]

[0106] experiment:

[0107] The hard carbon materials 1#, 2#, 3#, 4#, 5# prepared in Examples 1, 2, 3, 4, 5 and the materials prepared in Comparative Examples 1, 2, 3, 4, 5 were respectively made into negative electrodes for sodium ion batteries and relevant performance tests were carried out.

[0108] Take hard carbon materials 1#, 2#, 3#, 4#, 5# and the materials obtained from comparative examples 1, 2, 3, 4, 5 respectively, mix with PVDF binder at a mass ratio of 90:10, add appropriate amount of NMP, grind into paste in an agate mortar, and apply it on the aluminum current collector. The coating mass is about 2.5 mg of electrode active material. Then the electrode is vacuum dried at 120°C for 12 hours to obtain the negative electrode of the sodium ion battery. Sodium metal is used as the positive electrode, the electrolyte is NaPF6 in EC+DMC (vol%: 1:1), and the voltage range is 0.01-3V. The charge and discharge tester is Land CT2001A. The specific results are shown in Table 11.

[0109] Table 11 Comparison of electrochemical properties of hard carbon materials 1#, 2#, 3#, 4#, 5# and materials in comparative examples 1, 2, 3, 4, 5:

[0110]

[0111] Figure 1 The SEM images of the hard carbon material 1# obtained in Example 1 at different magnifications, where a is 2000 times and b is 10000 times. From the low-magnification SEM images, it can be seen that the material is blocky and has a rough surface, accompanied by the appearance of voids, which is the result of sulfuric acid etching.

[0112] Figure 2 The TEM images of the hard carbon material 1# obtained in Example 1 at different magnifications, where the scale bar of a is 20nm and b is 1nm. It can be seen from the TEM images that there are abundant micropores and mesopores. At the same time, the disordered lattice gaps of the hard carbon can be observed.

[0113] Figure 3 The XPS graphs of hard carbon materials 1#, 2#, 3#, 4#, and 5# show that only C and O elements exist in the materials.

[0114] Figure 4 The XRD patterns of hard carbon materials 1#, 2#, 3#, 4#, and 5# are shown in Figure 1. The broad diffraction peak at about 20 degrees shows that the obtained material is a hard carbon material, and no other impurity peaks are detected.

[0115] Figure 5This is the Raman graph of the hard carbon material 1# obtained in Example 1. The D peak and G peak belonging to the carbon material are clearly seen at 1350 and 1580.

[0116] Figure 6 This is the first cycle charge-discharge curve of the hard carbon material 1# obtained in Example 1. As can be seen from the figure, at a current density of 100 mA / g, a platform begins to appear at around 0.1 V and a higher capacity is given.

[0117] Figure 7 The hard carbon material 1# obtained in Example 1 is 1A g -1 Cyclic curves at current density of . As can be seen from the figure, during the activation process of 100mA / g, the initial efficiency of the material is 75.6% and the specific capacity is 263mAh / g. At a current density of 1A / g, the capacity is 165mAh / g, indicating that the material has good electrochemical properties.

[0118] Figure 8 The charge-discharge curves of the hard carbon material 1# obtained in Example 1 at different cycle numbers at a current density of 1 A / g are shown in the figure. As can be seen from the figure, the material has good cycle stability.

[0119] Fig. 9 This is the CV curve of the hard carbon material 1# obtained in Example 1 at a scan rate of 0.1 mV / s. As can be seen from the figure, the first cycle and the second cycle are basically overlapped, which indirectly verifies that the material has excellent cycle stability.

[0120] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. Application of hard carbon materials as negative electrode materials for sodium ion batteries, It is characterized in that The preparation method of the hard carbon material is a non-sintering dehydration carbonization method, comprising the following steps: 1) Dissolving a large amount of organic matter in a small amount of deionized water until a supersaturated solution is formed; the organic matter is any one of sucrose, glucose, trehalose, ketohexose or starch; 2) adding a strong oxidant to the product obtained in step (1) to obtain a hard carbon product; the ratio of the strong oxidant to the product obtained in step (1) is 0.1 mL: 1 g to 1 mL: 1 g; the strong oxidant is sulfuric acid; 3) The product obtained in step (2) is washed by centrifugation with deionized water and dried to obtain a hard carbon material; the centrifugal speed is 3000-12000 rpm, the time is 3-10 minutes, and the drying temperature is 60-120°C.

2. Use of the hard carbon material as claimed in claim 1 as a negative electrode material for sodium ion batteries, Features: In step 1), the ratio of organic matter to deionized water is 0.5 g:1 mL to 4 g:1 mL.

3. Use of the hard carbon material as claimed in claim 1 as a negative electrode material for sodium ion batteries, Features: The organic matter in step 1) is sucrose, glucose or trehalose.

4. Use of the hard carbon material as claimed in any one of claims 1 to 3 as a negative electrode material for a sodium ion battery, Features: This hard carbon material is used to prepare the hard carbon negative electrode of sodium ion battery. The initial efficiency in the activation process of 100mA / g is 75.6%, and the specific capacity is 263mAh / g; at the current density of 1A / g, the specific capacity is 165mAh / g.

Citation Information

Patent Citations

  • Low porosity, functionalized, carbon micro-powders