Highly active composite aluminum powder capable of catalyzing ammonium perchlorate and preparation method thereof
By introducing fluorine-containing polymers and copper oxide on the aluminum powder, the oxide layer is weakened and uniform dispersion is achieved. High-active composite aluminum powder is prepared by electrostatic spraying method, which solves the problems of insufficient activity of aluminum powder and low catalytic efficiency of copper oxide, which is significantly Improves the combustion performance and reactivity of propellants.
Patent Information
- Application Number
- CN202111269664.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Among the existing aluminum/ammonium perchlorate propellants, aluminum powder is insufficient in activity, and the research on copper oxide catalyzed ammonium perchlorate is mainly focused on morphological control and uniform mixing, and there is a lack of effective means to improve activity.
By introducing fluorine-containing polymers such as polyvinylidene fluoride or 26-type fluoro-rubber, the surface oxide layer of the aluminum powder is weakened, the high-active aluminum core is exposed, and copper oxide is added evenly, and high-active composite aluminum powder is prepared by electrostatic spraying method to achieve The uniform dispersion of copper oxide and the catalytic decomposition of ammonium perchlorate.
It significantly improves the reactivity of aluminum powder, catalyzes the decomposition performance of ammonium perchlorate, reduces the initial reaction temperature of the propellant, and improves the particle morphology, and is suitable for high-temperature environments.
Smart Images

Figure CN116063135B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of propellants and relates to a high-activity composite aluminum powder capable of catalyzing ammonium perchlorate and a preparation method thereof. Background Art
[0002] As a highly active metal, aluminum powder has a wide range of applications in the field of energetic materials. For the aluminum / ammonium perchlorate system, when it is used as the main component of the propellant, the activity of aluminum powder has a great influence on the combustion performance of the propellant. At present, the main method to increase the activity of aluminum powder is coating. The mechanism of increasing activity varies with different coating materials. The main coating material is fluorine-containing polymer. Although there are many studies on aluminum / fluorine-containing polymers, the mechanism of increasing their activity is still at a relatively preliminary level, that is, fluorine is more oxidizing than oxygen, and can react with the alumina shell of the aluminum ball and remove the alumina shell. However, there has been no further research on the relationship between the decomposition starting temperature of the fluorine-containing polymer and the increase in the activity of aluminum powder.
[0003] As a commonly used fluorine-containing polymer, polyvinylidene fluoride has the characteristics of strongest toughness, low friction coefficient, strong corrosion resistance, aging resistance, weather resistance, and good radiation resistance. Type 26 fluororubber (VITON) is a copolymer of vinylidene fluoride and hexafluoropropylene. Its high temperature resistance is the same as that of silicone rubber. It is the best elastomer at present. It has high chemical stability, excellent vacuum performance, and excellent physical and mechanical properties. It has been applied to cutting-edge technologies such as modern aviation, missiles, rockets, space navigation, ships, atomic energy, and industrial fields such as automobiles, shipbuilding, chemicals, petroleum, telecommunications, instruments, and machinery.
[0004] As an oxidant, ammonium perchlorate is often used in various types of propellants. Its combustion performance is mainly related to its thermal decomposition. Studies have shown that transition metal oxides can catalyze the thermal decomposition of ammonium perchlorate, among which copper oxide has the most obvious catalytic effect on ammonium perchlorate. However, the main research direction of the existing copper oxide catalysis of ammonium perchlorate is how to control the morphology of nano copper oxide and how to mix it evenly with ammonium perchlorate ([1] C. Yang, J. Wang, F. Xiao, X. Su, Microwave hydrothermal disassembly for evolution from CuO dendrites to nanosheets and their applications in catalysis and photo-catalysis, Powder Technology 264 (2014) 36-42. [2] J. Yin, Z. Sheng, W. Zhang, Y. Zhang, H. Zhong, R. Li, Z. Jiang, X. Wang, Synthesis and catalytic properties of novel peanut shaped CuO hollow architectures, Materials Letters 131 (2014) 317-320. [3] L. Chen, L. Li, G. Li, Synthesis of CuO nanorods and their catalytic activity in the thermal decomposition of ammonium perchlorate, Journal of Alloys and Compounds 464(2008)532-536.). Summary of the invention
[0005] The purpose of the present invention is to provide a high-activity composite aluminum powder that can catalyze ammonium perchlorate and a preparation method thereof. The present invention introduces a fluorine-containing polymer to weaken the oxide layer on the surface of the insensitive aluminum powder, exposing the aluminum core, thereby improving the reaction activity of the aluminum, and at the same time, a small amount of copper oxide is added evenly, so that when the high-activity composite aluminum powder is mixed with ammonium perchlorate, the copper oxide can be evenly dispersed in the ammonium perchlorate.
[0006] The technical solution for achieving the purpose of the present invention is as follows:
[0007] The preparation method of high-activity composite aluminum powder capable of catalyzing ammonium perchlorate comprises the following steps:
[0008] Step 1, dissolving a fluorine-containing polymer in an organic solvent, dispersing it ultrasonically after it is fully dissolved, adding aluminum powder, stirring it evenly, dispersing it ultrasonically, adding copper oxide, stirring it sufficiently, dispersing it ultrasonically, stirring it, and preparing an electrostatic spray precursor solution, wherein the fluorine-containing polymer is polyvinylidene fluoride or 26-type fluororubber;
[0009] Step 2, using an electrostatic spray method to collect active aluminum powder on the negative electrode plate and age it to obtain a high-activity composite aluminum powder.
[0010] Preferably, in step 1, the concentration of the fluorine-containing polymer in the electrostatic spray precursor solution is 0.9-1.1 mg / mL.
[0011] Preferably, in step 1, the organic solvent is N,N-dimethylformamide or acetone.
[0012] Preferably, in step 1, the concentration of aluminum powder is 47-48 mg / mL.
[0013] Preferably, in step 1, the concentration of copper oxide is 2-3 mg / mL.
[0014] Preferably, in step 1, the mass ratio of aluminum powder, copper oxide and fluorine-containing polymer is 95:5:20.
[0015] Preferably, in step 1, the ultrasonic dispersion time is 8 to 12 minutes.
[0016] Preferably, in step 1, the final stirring time is 10 to 14 hours.
[0017] Preferably, in step 2, the parameters of the electrostatic spray are: the diameter of the nozzle is 0.4 to 1 mm, the distance from the nozzle to the negative plate is 5 to 10 cm, and the voltage is 24 to 28 kV.
[0018] Preferably, in step 2, the aging temperature is 68-72° C., and the aging time is 2 hours.
[0019] Compared with the prior art, the present invention has the following beneficial results:
[0020] The present invention utilizes the extremely high electronegativity of the fluorine element in the fluorine-containing polymer to react with the oxide layer on the outer layer of the aluminum powder, thereby weakening its passivation effect on the aluminum powder and exposing the highly active aluminum powder core to increase its reactivity. Secondly, the addition of copper oxide further enhances the activity of the aluminum powder in the propellant system, catalyzes the decomposition of ammonium perchlorate, and further activates the reaction between the active aluminum powder and ammonium perchlorate. In addition, the ultrasonic dispersion method can fully bring the fluorine-containing polymer, copper oxide, and aluminum powder into closer contact. The electrostatic spray method can change the particle morphology obtained by volatilizing the solvent in the conventional method, making it easier to apply in the field of propellants. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a diagram of the thermal decomposition process of type 26 fluororubber and polyvinylidene fluoride in an argon environment.
[0022] Figure 2 This is a diagram of the thermal decomposition process of aluminum / copper oxide, aluminum / copper oxide / polyvinylidene fluoride, and aluminum / copper oxide / 26 type fluororubber.
[0023] Figure 3 This is a thermal decomposition process diagram of aluminum / 26 type fluororubber, aluminum oxide / 26 type fluororubber, copper oxide / 26 type fluororubber, aluminum / polyvinylidene fluoride, aluminum oxide / vinylidene fluoride, and copper oxide / vinylidene fluoride.
[0024] Figure 4 X-ray diffraction analysis results of the calcined residues of aluminum / copper oxide / 26 type fluororubber at 400℃, 450℃ and 500℃ (b) and copper oxide / 26 type fluororubber at 500℃ (c).
[0025] Figure 5 X-ray diffraction analysis results of the residues calcined at 400 (a) and 500 °C (b) for aluminum / copper oxide / polyvinylidene fluoride, aluminum / polyvinylidene fluoride, and copper oxide / polyvinylidene fluoride.
[0026] Figure 6 This is the reaction mechanism diagram of aluminum / copper oxide / polyvinylidene fluoride.
[0027] Figure 7 This is the reaction mechanism diagram of aluminum / copper oxide / 26 type fluororubber.
[0028] Figure 8 This is a diagram of the thermal decomposition process of aluminum / copper oxide / polytetrafluoroethylene. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0030] In the following examples and comparative examples, the reaction activity of each sample was analyzed by thermal analysis. The specific method was as follows: 1 mg of the sample was placed in an 80 mL perforated alumina crucible with a lid, and the temperature was raised from 30°C to 1200°C at a heating rate of 15 K / min in an argon environment of 20 mL / min.
[0031] Example 1
[0032] (1) Preparation of aluminum / copper oxide / polyvinylidene fluoride precursor solution: 10 mg of polyvinylidene fluoride was dissolved in 10 mL of N,N-dimethylformamide solution, magnetically stirred for 0.5 hour, and then ultrasonicated for 10 minutes. After adding 47.5 mg of aluminum powder, magnetically stirred for 0.5 hour, ultrasonicated for 10 minutes, 2.5 mg of copper oxide was added, magnetically stirred for 0.5 hour, ultrasonicated for 10 minutes, and finally stirred for 12 hours to prepare a precursor solution.
[0033] (2) Preparation of high-activity composite aluminum powder by electrostatic spraying: The precursor solution was sucked up by a syringe and placed on a syringe pump, and the propulsion speed was adjusted to 1 mL / min. The negative electrode was clamped on an aluminum foil, and the positive electrode was clamped on a needle with an inner diameter of 0.51 mm. The high-voltage power supply was turned on and the power supply voltage was adjusted to 26 kV. The inter-electrode distance was adjusted to 5 cm, and electrostatic spraying was started. After the spraying was completed, the high-activity composite aluminum powder on the aluminum foil was collected and placed in a 70°C oven for aging for 2 hours to obtain a high-activity composite aluminum powder that can catalyze ammonium perchlorate.
[0034] Figure 1 (a) is the thermal decomposition process of type 26 fluororubber, which has a one-step weight loss and ends at 700°C. According to its DSC curve, the peak temperature of the first endothermic peak (a) of type 26 fluororubber is 455°C, which corresponds to the starting temperature of its weight loss. This result shows that it absorbs heat (0.46 J / g) when it starts to lose weight. The peak temperature of the endothermic peak (b) following peak (a) is 465°C, and its peak area is 10.77 J / g. The peak temperature of peak (c) corresponds to the peak temperature of the DTG curve. This shows that due to the existence of an exothermic reaction, the DSC curve is offset and peak (c) is observed.
[0035] As a blank sample, the thermal decomposition process of aluminum / copper oxide was as follows Figure 2 As shown. Since the reaction between aluminum and copper oxide is a solid-solid phase reaction, no significant weight loss is observed on the thermogravimetric curve. From its DSC curve, it can be seen that the reaction range of the thermite reaction between aluminum and copper oxide is 500-600℃, and the peak area of the main exothermic peak is 101J / g. The endothermic peaks at 660℃ and 1100℃ are caused by the melting of aluminum and copper. After the addition of polyvinylidene fluoride, the initial reaction temperature of the main exothermic peak was reduced by 120℃ respectively. In the main exothermic reaction range, the corresponding weight loss of the sample is 20%. At the same time, the intensity of the endothermic peak of the sample at 660℃ is significantly weakened, indicating that the remaining aluminum content is reduced after the main reaction is completed. It should be noted that at 880℃, a weight loss of 6% was observed on the thermogravimetric curve of aluminum / copper oxide / polyvinylidene fluoride, and an endothermic peak was observed on the corresponding DSC curve. This is due to the presence of aluminum fluoride. In summary, the addition of polyvinylidene fluoride will greatly advance the initial reaction temperature of the thermite system and greatly increase the heat release.
[0036] Example 2
[0037] (1) Preparation of aluminum / copper oxide / 26-type fluororubber precursor solution: 10 mg of 26-type fluororubber was dissolved in 10 mL of acetone solution, magnetically stirred for 0.5 hour, and then ultrasonicated for 10 minutes. After adding 47.5 mg of aluminum powder, magnetically stirred for 0.5 hour, ultrasonicated for 10 minutes, 2.5 mg of copper oxide was added, magnetically stirred for 0.5 hour, ultrasonicated for 10 minutes, and finally stirred for 12 hours to obtain a precursor solution.
[0038] (2) Preparation of high-activity composite aluminum powder by electrostatic spraying: The precursor solution was sucked up by a syringe and placed on a syringe pump, and the propulsion speed was adjusted to 1 mL / min. The negative electrode was clamped on an aluminum foil, and the positive electrode was clamped on a needle with an inner diameter of 0.51 mm. The high-voltage power supply was turned on and the power supply voltage was adjusted to 26 kV. The inter-electrode distance was adjusted to 5 cm, and electrostatic spraying was started. After the spraying was completed, the high-activity composite aluminum powder on the aluminum foil was collected and placed in a 70°C oven for aging for 2 hours to obtain a high-activity composite aluminum powder that can catalyze ammonium perchlorate.
[0039] The thermal decomposition process of polyvinylidene fluoride is significantly different from that of 26-type fluororubber. Figure 1 As shown in (b), the weight loss process of polyvinylidene fluoride starts from 400°C and ends at 530°C, with a total weight loss of 62%, which is 38% less than fluororubber. Polyvinylidene fluoride reaches the fastest decomposition rate at 469°C, and there is no endothermic peak corresponding to it at this time. Two endothermic peaks (d&e) were observed at the beginning of its thermal decomposition. At the end of peak d, the corresponding weight loss curve has only a small amount of weight loss. According to the literature [W Ma, X Wang, J Zhang (2011) Journal of Thermal Analysis and Calorimetry 103: 319. Doi: 10.1007 / s10973-010-0961], it can be seen that there is a crystal transformation of PVDF at this time. At the end of the weight loss, a small exothermic peak (f) was observed on the DSC curve of polyvinylidene fluoride, which indicates that PVDF may release a certain amount of heat during thermal decomposition.
[0040] As a blank sample, the thermal decomposition process of aluminum / copper oxide was as follows Figure 2As shown. Since the reaction between aluminum and copper oxide is a solid-solid phase reaction, no significant weight loss is observed on the thermogravimetric curve. From its DSC curve, it can be seen that the reaction range of the aluminothermic reaction between aluminum and copper oxide is 500-600°C, and the peak area of the main exothermic peak is 101J / g. The endothermic peaks at 660°C and 1100°C are caused by the melting of aluminum and copper. After adding 26-type fluororubber, the starting reaction temperature of the main exothermic peak was reduced by 70°C respectively. In the main exothermic reaction range, the corresponding weight loss of the sample is 9.34%. At the same time, the intensity of the endothermic peak of the sample at 660°C is significantly weakened, indicating that the remaining aluminum content is reduced after the main reaction is completed. It should be noted that at 880°C, the corresponding weight loss on the thermogravimetric curve of aluminum / copper oxide / 26-type fluororubber is 3%, and an endothermic peak is observed on the corresponding DSC curve. This is due to the presence of aluminum fluoride. In summary, the addition of type 26 fluororubber will greatly advance the initial reaction temperature of the thermite system and significantly increase the heat release.
[0041] Example 3
[0042] In order to study the reasons why 26-type fluororubber and polyvinylidene fluoride improve the activity of aluminum powder, a series of test samples were prepared according to the method of Example 1. The composition and mass fraction of each sample are shown in Table 1.
[0043] Table 1 Sample types and composition of each sample
[0044]
[0045] Thermal decomposition process of aluminum / 26 type fluororubber, aluminum oxide / 26 type fluororubber, copper oxide / 26 type fluororubber, aluminum / polyvinylidene fluoride, aluminum oxide / vinylidene fluoride, copper oxide / vinylidene fluoride Figure 3 As shown. The initial reaction temperature of alumina / 26 type fluororubber is 365°C, while the initial reaction temperature of alumina / vinylidene fluoride is 306°C, both of which are lower than the initial decomposition temperature of the fluorine-containing polymer itself. This shows that alumina can react with the fluorine-containing polymer before it decomposes. The small peak at 500°C for alumina / vinylidene fluoride indicates that there is a crystal transformation process from β-AlF3 to α-AlF3 at this time. However, in alumina / 26 type fluororubber, no obvious crystal transformation process can be observed. An 18% weight loss was observed on the thermogravimetric curves of alumina / vinylidene fluoride and alumina / 26 type fluororubber at 1100°C, which may be due to the sublimation of aluminum fluoride.
[0046] For the thermal decomposition of aluminum / polyvinylidene fluoride, a weak exothermic peak was observed at 350°C; and on the DSC curve of aluminum / 26 type fluororubber, a weak exothermic peak was also observed at 365°C. These two exothermic peaks are caused by the reaction of aluminum oxide and fluorine-containing polymers. After that, the main exothermic peak of aluminum / polyvinylidene fluoride is between 430 and 500°C, which is the fluorination reaction of aluminum. For aluminum / 26 type fluororubber, the main exothermic range is consistent with that of aluminum / polyvinylidene fluoride. It is worth noting that the reaction between aluminum and fluorine-containing polymers all starts before the thermal decomposition of fluorine-containing polymers, indicating that the decomposition of fluorine-containing polymers has a significant effect on the fluorination of aluminum.
[0047] For the reaction of copper oxide / 26 type fluororubber, the main exothermic range is between 410 and 500 °C, indicating that copper oxide can react with 26 type fluororubber. Similarly, for copper oxide / polyvinylidene fluoride, copper oxide can also react with polyvinylidene fluoride. However, thermal decomposition of 26 type fluororubber also exists in this reaction range, indicating that copper oxide may also react with the cracking products of 26 type fluororubber. The endothermic peak at 1070 °C indicates the presence of elemental copper in the reaction product; at the same time, no melting peak of copper fluoride was observed at 950 °C; this shows that copper oxide will only be reduced to copper element by fluorine, and cannot be further oxidized to copper fluoride.
[0048] XRD analysis of the phases of aluminum / copper oxide / 26 type fluororubber at different temperatures ( Figure 4 ) After fluorination, it can be seen that the products of aluminum, copper oxide, aluminum / copper oxide and 26-type fluororubber are aluminum fluoride, cupric fluoride, cuprous fluoride, and copper. This shows that aluminum is fluorinated into aluminum fluoride by 26-type fluororubber, and copper oxide is first replaced by cupric fluoride and then gradually reduced to form cuprous fluoride and copper.
[0049] XRD analysis of the phases of aluminum / copper oxide / polyvinylidene fluoride at different temperatures was performed ( Figure 5 ) It can be seen that the fluorination of aluminum is the same as before. The difference from aluminum / copper oxide / 26 type fluororubber is that the reduction process of copper oxide is first reduced to cuprous oxide and then to copper. It should be pointed out that no copper fluoride was found in the physical phase, which indirectly proves that the weight loss at 900℃ is the sublimation of aluminum fluoride.
[0050] From the above analysis, it can be seen that the reaction mechanism of aluminum / copper oxide / polyvinylidene fluoride is as follows Figure 6 As shown. First, due to the presence of hydroxyl groups on the surface of alumina, polyvinylidene fluoride decomposes in advance and generates free HF. HF first reacts with alumina at this time, weakening the inhibition of the alumina layer on the activity of the internal aluminum core. Subsequently, the alumina shell detaches from the aluminum core and exposes the internal highly active aluminum core. At this time, polyvinylidene fluoride further decomposes to generate more free HF, and the free HF reacts with the highly active aluminum core to generate aluminum fluoride. Reaction mechanism of aluminum / copper oxide / 26 type fluororubber ( Figure 7 ) is similar to aluminum / copper oxide / polyvinylidene fluoride, and the hydroxyl groups on the surface of aluminum oxide cause the 26 type fluororubber to decompose prematurely.
[0051] Comparative Example 1
[0052] (1) Preparation of aluminum / copper oxide / polytetrafluoroethylene precursor solution: 10 mg of polytetrafluoroethylene was dissolved in 10 mL of n-hexane, magnetically stirred for 0.5 hour, and then ultrasonicated for 10 minutes. After adding 47.5 mg of aluminum powder, magnetically stirred for 0.5 hour, ultrasonicated for 10 minutes, 2.5 mg of copper oxide was added, magnetically stirred for 0.5 hour, ultrasonicated for 10 minutes, and finally stirred for 12 hours to prepare a precursor solution.
[0053] (2) Preparation of highly active composite aluminum powder by electrostatic spraying: The precursor solution was drawn up by a syringe and placed on a syringe pump, and the propulsion speed was adjusted to 1 mL / min. The negative electrode was clamped on an aluminum foil, and the positive electrode was clamped on a needle with an inner diameter of 0.51 mm. The high-voltage power supply was turned on and the power supply voltage was adjusted to 26 kV. The inter-electrode distance was adjusted to 5 cm, and electrostatic spraying was started. After the spraying was completed, the composite aluminum powder on the aluminum foil was collected and placed in a 70°C oven for aging for 2 hours to obtain a composite aluminum powder that can catalyze ammonium perchlorate.
[0054] Depend on Figure 8 It can be seen that the main reaction range of the thermal decomposition process of polytetrafluoroethylene is 500-620°C, and its weight loss is 100%. While losing weight, the thermal decomposition reaction absorbs heat. Compared with the aluminothermic reaction between aluminum and copper oxide, it can be seen that the exothermic range of the aluminothermic reaction is 500-600°C, and the peak area of the main exothermic peak is 101J / g. From the thermal decomposition process of aluminum / copper oxide / polytetrafluoroethylene, it can be seen that its main exothermic range is between 500 and 620°C, and its area is 702.6J / g. At the same time, no obvious weight loss was observed in the main exothermic range, that is, the starting temperature of the aluminothermic reaction could not be observed to be advanced, and no reaction between polytetrafluoroethylene and aluminum was observed, indicating that the improvement of the activity of aluminum powder by polytetrafluoroethylene is very limited.
Claims
1. A method for preparing a highly active composite aluminum powder capable of catalyzing ammonium perchlorate, characterized in that: The following steps are involved: Step 1, dissolving a fluorine-containing polymer in an organic solvent, dispersing it ultrasonically after it is fully dissolved, adding aluminum powder, stirring it evenly, dispersing it ultrasonically, adding copper oxide, stirring it sufficiently, dispersing it ultrasonically, stirring it, and preparing an electrostatic spray precursor solution, wherein the concentration of aluminum powder is 47-48 mg / mL, the concentration of copper oxide is 2-3 mg / mL, the fluorine-containing polymer is 26 type fluororubber, and the mass ratio of aluminum powder, copper oxide and fluorine-containing polymer is 95:5:20; Step 2, using an electrostatic spray method to collect active aluminum powder on the negative electrode plate and age it to obtain a high-activity composite aluminum powder.
2. The preparation method according to claim 1, characterized in that In step 1, the concentration of the fluorinated polymer in the electrostatic spray precursor solution is 0.9-1.1 mg / mL.
3. The preparation method according to claim 1, characterized in that: In step 1, the organic solvent is N,N-dimethylformamide or acetone.
4. The preparation method according to claim 1, characterized in that: In step 1, the ultrasonic dispersion time is 8 to 12 minutes.
5. The preparation method according to claim 1, characterized in that: In step 1, the final stirring time is 10 to 14 hours.
6. The preparation method according to claim 1, characterized in that In step 2, the parameters of the electrostatic spray are: the diameter of the nozzle is 0.4-1 mm, the distance from the nozzle to the negative plate is 5-10 cm, and the voltage is 24-28 kV.
7. The preparation method according to claim 1, characterized in that: In step 2, the aging temperature is 68-72° C., and the aging time is 2 hours.
8. High-activity composite aluminum powder obtained according to the preparation method described in any one of claims 1 to 7.
Citation Information
Patent Citations
Double oxide composite type super thermite and preparation method thereof
CN102500383A
Preparation method for nanometer thermite film
CN108179456A