Passivation additive and preparation method thereof, solar cell and preparation method thereof
By using passivation additives with a neothiophen structure in perovskite solar cells, the problem of insufficient passivation ability in the prior art is solved, and the crystal quality of the perovskite layer and the stability of the solar cell are improved.
Patent Information
- Application Number
- CN202310102858.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-01-31
AI Technical Summary
The existing passivation additives have poor passivation ability of the perovskite solar cell layer, resulting in a decrease in energy conversion efficiency and stability.
Using a passivation additive with a thiophene structure, a polyheterocyclic skeleton is formed by introducing 3,3'-dimethoxy-2,2'-bisthiophene and N-bromosuccinimide into the perovskite layer. Enhance self-aggregation and conductivity, use the coordination effect of amino and methoxy to passivate defects, and improve passivation effect.
The crystal quality and water stability of the perovskite layer are significantly improved, and the stability of the open circuit voltage and energy conversion efficiency of the solar cell is enhanced.
Smart Images

Figure CN116063279B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of photovoltaic technology, and in particular to a passivation additive and a preparation method thereof, a solar cell and a preparation method thereof. Background Art
[0002] Perovskite solar cells have the advantages of high energy conversion efficiency and can be prepared using low-temperature processes. They can be connected in series with currently mature crystalline silicon solar cells to prepare stacked solar cells, helping crystalline silicon solar cells to achieve higher energy conversion efficiency. Therefore, they have broad prospects for commercial applications.
[0003] The perovskite layer of the perovskite solar cell is a light-absorbing thin film layer composed of organic-inorganic halides with a perovskite structure. Its component formula is ABX3, where the A position is generally an organic cation, such as MA + or FA + , B position is generally Pb 2+ , X is generally a halogen ion, such as Cl - Br - or I - . In the perovskite layer, the B-site cations and the X-site anions form an octahedral structure, and the A-site cations are located in the gaps between the octahedra. The quality of the perovskite layer has a significant impact on the performance of perovskite solar cells. The perovskite layers prepared by the solution method commonly used in the industry are all polycrystalline films, which inevitably contain many defects. The defects mainly include uncoordinated ions and dangling bonds on grain boundaries and crystal surfaces. These defects will increase the non-radiative recombination of perovskite solar cells, thereby reducing the open circuit voltage of perovskite solar cells. At the same time, the presence of these defects will also increase the channels for water and oxygen to corrode the perovskite layer, which is not conducive to the higher stability of perovskite solar cells.
[0004] Therefore, in order to improve the energy conversion efficiency and stability of perovskite cells, it is necessary to passivate the defects in the perovskite layer. The current method is mainly to add passivation additives to the perovskite layer. However, the existing passivation additives are mainly alkyl or benzene ring skeletons, and their molecular conductivity and self-aggregation are not strong, resulting in poor passivation ability of the existing passivation additives for the defects of the perovskite layer. Summary of the invention
[0005] The embodiments of the present application provide a passivation additive and a preparation method thereof, a solar cell and a preparation method thereof, which are intended to improve the technical problem that the existing passivation additives have poor passivation ability for defects in the perovskite layer.
[0006] In a first aspect, an embodiment of the present application provides a method for preparing a passivation additive, comprising:
[0007] 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide in a molar ratio of 1:(1-3) are dissolved in tetrahydrofuran, reacted at 15-25° C. for at least 3 hours, and subjected to a first purification to obtain an intermediate.
[0008] Under an ammonia atmosphere, the intermediate and potassium carbonate in a molar ratio of 1:(3-5) are dissolved in a mixture of methanol and N-methylpyrrolidone, and reacted at 85-95°C for at least 36 hours; after cooling to 15-25°C, reacted at -78--75°C for at least 12 hours for a second purification.
[0009] In the above technical scheme, the molecular skeleton of the prepared passivation additive has two interconnected thiophene units (i.e., a thiophene structure) to form a polyheterocyclic skeleton; the sulfur atoms in the thiophene structure can enhance the interaction between molecules. Compared with the passivation additives with alkyl or benzene ring skeletons, the passivation additives of the present application have a stronger self-aggregation effect, which can reduce the residue of the passivation additive inside the perovskite layer grains, improve the crystallization quality of the perovskite layer, and increase the concentration of the passivation additive at the grain boundaries and surface of the perovskite layer, thereby improving the passivation effect on the perovskite layer; the thiophene structure also has a higher electron cloud density and a stronger intramolecular push-pull electron effect. Compared with the passivation additives with alkyl or benzene ring skeletons, the passivation additives of the present application have a stronger conductivity, which can reduce the influence of the enrichment of the passivation additive at the grain boundaries and surface of the perovskite layer on the charge conduction between the perovskite layer grains.
[0010] In addition, the α-positions of both ends of the thiophene structure of the passivation additive prepared in the present application are connected to amino groups, and the N atom of -NH2 is connected to the Pb 2+ The coordination effect between them can passivate defects, and -NH2 can occupy the vacancies of organic cations at the grain boundaries and surfaces of the perovskite layer. While passivating the defects, it also allows the passivation additive molecules to be arranged at the grain boundaries and surfaces of the perovskite layer, playing a hydrophobic role and improving the water stability of the perovskite layer. -NH2 can also form hydrogen bonds with the halogen ions of the perovskite layer to connect the grains of the perovskite layer, further achieving passivation of defects.
[0011] The two β positions of the thiophene structure are connected to methoxy groups. The non-covalent bond interaction between the oxygen atom in the methoxy group and the sulfur atom in the adjacent thiophene unit can limit the molecular conformational torsion of the thiophene, improve the planarity of the thiophene, and enhance the conjugation between the two thiophene units, so as to further improve the conductivity and self-aggregation ability of the passivation additive, which is conducive to further enhancing the passivation effect. The sulfur atom in the thiophene structure and the oxygen atom in the methoxy group have lone pairs of electrons, which can also bind to the Pb 2+ Coordination bonds are formed between them, thereby improving the passivation effect of the passivation additive on the defects of the perovskite layer.
[0012] In combination with the first aspect, in an optional embodiment of the present application, the first purification is column chromatography purification, and the eluent for the first purification is petroleum ether and dichloromethane in a volume ratio of (2.5 to 3.5):1; and / or, the second purification is column chromatography purification, and the eluent for the second purification is n-hexane and ethyl acetate in a volume ratio of (4.5 to 5.5):1.
[0013] In the above technical scheme, the first purification is column chromatography purification, and the eluent of the first purification is petroleum ether and dichloromethane in a volume ratio of (2.5-3.5):1, which can be quickly eluted to obtain the purified intermediate. The second purification is column chromatography purification, and the eluent of the second purification is n-hexane and ethyl acetate in a volume ratio of (4.5-5.5):1, which can be quickly eluted to obtain the purified passivation additive.
[0014] In combination with the first aspect, in an optional embodiment of the present application, the molar concentrations of 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide in tetrahydrofuran are 0.1-0.2M and 0.25-0.35M, respectively; and / or, the molar concentrations of the intermediate and potassium carbonate in the mixed solution are 0.1-0.15M and 0.45-0.55M, respectively.
[0015] In the above technical scheme, the molar concentrations of 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide in tetrahydrofuran are 0.1-0.2M and 0.25-0.35M, respectively, which is beneficial to increase the reaction rate of forming intermediates; the molar concentrations of the intermediates and potassium carbonate in the mixed solution are 0.1-0.15M and 0.45-0.55M, respectively, which is beneficial to the reaction rate of the intermediate conversion to form a passivating additive.
[0016] Optionally, in the mixed solution, the volume ratio of methanol to N-methylpyrrolidone is 1:(0.8-1.2).
[0017] In a second aspect, the present application provides a passivation additive, which is prepared by the preparation method of the passivation additive provided in the first aspect.
[0018] In the above technical scheme, the passivation additive provided by the present application has a thiophene structure skeleton, and the α positions at both ends of the thiophene structure are connected to amino groups, and the two β positions of the thiophene structure are connected to methoxy groups, which can not only improve the self-aggregation effect of the passivation additive, but also improve the conductivity of the passivation additive, which is beneficial to improve the passivation effect of the passivation additive on the defects of the perovskite layer, and further help to improve the stability of the open circuit voltage and energy conversion efficiency of the solar cell.
[0019] In a third aspect, the present application provides a passivation additive, the structural formula of the passivation additive is as follows:
[0020]
[0021] In the above technical scheme, the passivation additive provided by the present application has a thiophene structure skeleton, and the α positions at both ends of the thiophene structure are connected to amino groups, and the two β positions of the thiophene structure are connected to methoxy groups, which can not only improve the self-aggregation effect of the passivation additive, but also improve the conductivity of the passivation additive, which is beneficial to improve the passivation effect of the passivation additive on the defects of the perovskite layer, and further help to improve the stability of the open circuit voltage and energy conversion efficiency of the solar cell.
[0022] In a fourth aspect, the present application provides a solar cell, wherein the perovskite layer of the solar cell comprises: a perovskite active material and the passivation additive provided in the second aspect or the third aspect.
[0023] In the above technical solution, the perovskite layer of the solar cell contains perovskite active materials and the passivation additive provided in the second aspect or the third aspect of the present application. The presence of the passivation additive can effectively passivate the defects of the perovskite layer, thereby facilitating improving the conductivity, open circuit voltage and energy conversion efficiency stability of the solar cell.
[0024] In combination with the fourth aspect, in an optional embodiment of the present application, the mass of the passivation additive is 0.05 to 0.2% of the mass of the perovskite active material.
[0025] In the above technical solution, the mass of the passivation additive is 0.05-0.2% of the mass of the perovskite active material, which is not only conducive to ensuring the passivation effect of the passivation additive on the defects of the perovskite layer, but also conducive to avoiding the situation where too much passivation additive causes a certain degree of damage to the crystallization of the perovskite layer.
[0026] In a fifth aspect, the present application provides a method for preparing the solar cell provided in the fourth aspect, comprising: coating a solution containing a perovskite active material and a passivation additive onto the surface of a hole transport layer, and then performing an annealing treatment.
[0027] In the above technical scheme, the perovskite layer of the formed solar cell can contain perovskite active materials and the passivation additives provided in the second aspect or the third aspect of the present application, which can effectively passivate the defects of the perovskite layer, thereby facilitating improving the conductivity, open circuit voltage and energy conversion efficiency stability of the solar cell.
[0028] In combination with the fifth aspect, in an optional implementation manner of the present application, the temperature of the annealing treatment is 90 to 110° C., and the time of the annealing treatment is 5 to 30 minutes.
[0029] In the above technical solution, the above annealing conditions are conducive to accelerating the crystallization of the perovskite layer and improving the crystallization quality of the perovskite layer.
[0030] In combination with the fifth aspect, in an optional implementation manner of the present application, the coating is performed by spin coating, the spin coating rotation speed is 3000-4000 rpm, and the spin coating time is 20-50 s.
[0031] In the above technical solution, the above spin coating conditions are conducive to improving the flatness and thickness uniformity of the formed perovskite layer.
[0032] Optionally, the molar concentration of the perovskite active material in the solution is 1-2M.
[0033] Optionally, the perovskite active material is CH3NH3PbI3.
[0034] Optionally, the solvent of the solution is a mixture of N,N-dimethylformamide and dimethyl sulfoxide, and the volume ratio of N,N-dimethylformamide to dimethyl sulfoxide is (2-5):1. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 This is a flow chart of the preparation process of the passivation additive provided in this application.
[0037] Figure 2 This is a schematic diagram of the structure of the solar cell provided in this application.
[0038] Figure 3 This is the optimal conformation diagram of the passivation additive provided in Example 1 of the present application.
[0039] Figure 4 This is the optimal conformation diagram of the passivation additive provided in Comparative Example 1 of the present application.
[0040] Figure 5 This is the HOMO electron cloud distribution diagram of the passivation additive provided in Example 1 of the present application.
[0041] Figure 6 This is the LUMO electron cloud distribution diagram of the passivation additive provided in Example 1 of the present application.
[0042] Figure 7 This is the HOMO electron cloud distribution diagram of the passivation additive provided in Comparative Example 1 of the present application.
[0043] Figure 8This is the LUMO electron cloud distribution diagram of the passivation additive provided in Comparative Example 1 of the present application.
[0044] Fig. 9 A comparison chart of the open circuit voltage stability of the solar cells provided in Example 2 of the present application and Comparative Example 2.
[0045] Fig.10 A comparison chart of the energy conversion efficiency stability of the solar cells provided in Example 2 of the present application and Comparative Example 2.
[0046] Fig.11 This is a graph of electron mobility of the space charge limited current test of the passivation additives provided in Example 1 and Comparative Example 1 of the present application.
[0047] Icon: 10 - solar cell; 110 - transparent conductive layer; 120 - hole transport layer; 130 - perovskite layer; 140 - electron transport layer; 150 - buffer layer; 160 - metal electrode. DETAILED DESCRIPTION
[0048] The quality of the perovskite layer has a significant impact on the performance of perovskite solar cells. The perovskite layers prepared by the solution method commonly used in the industry are all polycrystalline thin films, which inevitably contain many defects. The defects mainly include uncoordinated ions and dangling bonds at grain boundaries and crystal surfaces. These defects will increase the non-radiative recombination of perovskite solar cells, thereby reducing the open circuit voltage of perovskite solar cells. At the same time, the presence of these defects will also increase the channels for water and oxygen to erode the perovskite layer, which is not conducive to the higher stability of perovskite solar cells. Therefore, it is necessary to add a passivation additive with a passivation effect to the perovskite layer.
[0049] The passivation additive molecules need to have a strong self-aggregation effect at the grain boundaries and surfaces of the perovskite layer. The self-aggregation effect can not only reduce the residue of the passivation additive inside the grains of the perovskite layer and improve the crystallization quality of the perovskite layer, but also increase the concentration of the passivation additive at the grain boundaries and surfaces of the perovskite layer, thereby improving the passivation effect on the perovskite layer. At the same time, the passivation additive also needs to have a strong electrical conductivity, which can minimize the impact of the enrichment of the passivation additive at the grain boundaries and surfaces of the perovskite layer on the charge conduction between the grains of the perovskite layer.
[0050] However, the inventors have found that the existing passivation additives are mainly alkyl or benzene ring skeletons, which have weak self-aggregation and conductivity, resulting in poor passivation ability of the existing passivation additives for defects in the perovskite layer.
[0051] Therefore, the present application provides a passivation additive and a preparation method thereof, which can improve the self-aggregation effect and conductivity of the passivation additive, so as to improve the passivation ability of the passivation additive on the defects of the perovskite layer.
[0052] The preparation method of the passivation additive provided in the present application comprises: dissolving 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide in tetrahydrofuran at a molar ratio of 1:(1-3), reacting at 15-25°C for at least 3 hours, and performing a first purification to obtain an intermediate. Under an ammonia atmosphere, dissolving the intermediate and potassium carbonate at a molar ratio of 1:(3-5) in a mixed solution of methanol and N-methylpyrrolidone, reacting at 85-95°C for at least 36 hours; after cooling to 15-25°C, reacting at -78--75°C for at least 12 hours, and performing a second purification.
[0053] The molecular skeleton of the passivation additive prepared by the above method has two interconnected thiophene units (i.e., thiophene structures) to form a polyheterocyclic skeleton; and the α positions at both ends of the thiophene structures of the passivation additive are connected to amino groups, and the two β positions of the thiophene structures are connected to methoxy groups.
[0054] The sulfur atoms in the thiophene structure of the passivation additive prepared in the present application can enhance the interaction between molecules. Compared with the passivation additives with alkyl or benzene ring skeletons, the passivation additives with thiophene structure in the present application have stronger self-aggregation, which can reduce the residue of the passivation additive inside the perovskite layer grains, improve the crystallization quality of the perovskite layer, and increase the concentration of the passivation additive at the grain boundaries and surfaces of the perovskite layer, thereby improving the passivation effect on the perovskite layer; the thiophene structure also has a higher electron cloud density and a stronger intramolecular push-pull electron effect. Compared with the passivation additives with alkyl or benzene ring skeletons, the passivation additives with thiophene structure in the present application have stronger conductivity, which can reduce the influence of the enrichment of the passivation additive at the grain boundaries and surfaces of the perovskite layer on the charge conduction between the perovskite layer grains. In addition, compared with the single thiophene unit structure, the π bond conjugation between the two thiophene rings in the thiophene structure of the present application can increase the delocalization area of the electrons, thereby improving the conductivity of the passivation additive.
[0055] The α positions of both ends of the thiophene structure of the passivation additive prepared in this application are connected to amino groups, and the N atom of -NH2 is connected to the Pb 2+ The coordination effect between them can passivate defects, and -NH2 can occupy the vacancies of organic cations at the grain boundaries and surfaces of the perovskite layer. While passivating the defects, it also allows the passivation additive molecules to be arranged at the grain boundaries and surfaces of the perovskite layer, playing a hydrophobic role and improving the water stability of the perovskite layer. -NH2 can also form hydrogen bonds with the halogen ions of the perovskite layer to connect the grains of the perovskite layer, further achieving passivation of defects.
[0056] The two β positions of the thiophene structure of the passivation additive prepared in the present application are connected to methoxy groups. The non-covalent bond interaction between the oxygen atom in the methoxy group and the sulfur atom in the adjacent thiophene unit can limit the molecular conformational distortion of the thiophene, improve the planarity of the thiophene, and enhance the conjugation between the two thiophene units, so as to further improve the conductivity and self-aggregation ability of the passivation additive, which is conducive to further enhancing the passivation effect. The sulfur atom in the thiophene structure and the oxygen atom in the methoxy group have lone pairs of electrons, which can also interact with the Pb 2+ Coordination bonds are formed between them, thereby improving the passivation effect of the passivation additive on the defects of the perovskite layer.
[0057] Figure 1 For the preparation process flow chart of the passivation additive provided in the embodiment of the present application, please refer to Figure 1 , the preparation method comprises the following steps:
[0058] S110, dissolving 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide in tetrahydrofuran at a molar ratio of 1:(1-3), reacting at 15-25° C. for at least 3 hours, and performing a first purification to obtain an intermediate.
[0059] The synthetic route of the intermediate formed from 3,3'-dimethoxy-2,2'-bithiophene is as follows:
[0060]
[0061] As an example, the molar ratio of 3,3'-dimethoxy-2,2'-bithiophene (CAS No. 118583-86-1) to N-bromosuccinimide (NBS) can be 1:1, 1:1.5, 1:1.8, 1:2.0, 1:2.2, 1:2.5 or 1:3, etc.
[0062] Furthermore, the molar ratio of 3,3'-dimethoxy-2,2'-bithiophene (CAS No. 118583-86-1) to N-bromosuccinimide (NBS) is 1:(2-2.5), which can allow 3,3'-dimethoxy-2,2'-bithiophene to react fully, so that bromine groups are connected to the α positions of both ends of the thiophene structure.
[0063] As an example, the reaction temperature for forming the intermediate can be 15°C, 18°C, 20°C, 22°C or 25°C, etc., and the reaction time for forming the intermediate can be 3h, 4h, 5h, 6h, 8h or various long times, etc.
[0064] In the present application, the reaction time for forming the intermediate is at least 6 h, which is conducive to the sufficient reaction of 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide.
[0065] In the present application, the molar concentrations of 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide in tetrahydrofuran (THF) are 0.1-0.2 M and 0.25-0.35 M, respectively, which is beneficial to increase the reaction rate of forming intermediates.
[0066] As an example, the molar concentration of 3,3'-dimethoxy-2,2'-bithiophene in tetrahydrofuran can be 0.1M, 0.12M, 0.15M, 0.18M or 0.2M, etc., and the molar concentration of N-bromosuccinimide in tetrahydrofuran can be 0.25M, 0.27M, 0.3M, 0.32M or 0.35M, etc.
[0067] In the present application, the first purification adopts column chromatography purification method, and the eluent of the first purification is petroleum ether and dichloromethane in a volume ratio of (2.5-3.5):1, which can quickly elute to obtain the purified intermediate.
[0068] As an example, in the eluent of the first purification, the volume ratio of petroleum ether to dichloromethane can be 2.5:1, 2.7:1, 3.0:1, 3.2:1 or 3.5:1, etc.
[0069] Furthermore, the eluent for the first purification is petroleum ether and dichloromethane in a volume ratio of (2.8-3.2):1, which is conducive to further rapid elution to obtain the purified intermediate.
[0070] It should be noted that in the present application, 3,3'-dimethoxy-2,2'-bithiophene can be purchased or synthesized by itself. For example, the synthesis route of 3,3'-dimethoxy-2,2'-bithiophene can be as follows:
[0071]
[0072] As an example, in the above-mentioned synthesis route, the synthesis steps of compound 2 are as follows: 3-methoxythiophene (i.e., compound 1) is dissolved in THF, stirred at a low temperature of -78°C for 10 minutes, then a n-hexane solution containing n-BuLi (n-butyl lithium) is added dropwise and stirring is continued for 1 hour, a n-hexane solution of trimethyltin chloride is added, and the mixture is moved to room temperature and stirred for 12 hours. After the reaction is completed, the reaction solution is poured into water to quench the reaction, extracted with dichloromethane, the organic phase is spun to remove the solvent, and the crude product is purified by silica gel column chromatography (the eluent is petroleum ether) to obtain a colorless oily liquid compound 2.
[0073] The synthesis steps of compound 3 are as follows: N-bromosuccinimide (NBS) is added to a THF solution of 3-methoxythiophene (i.e., compound 1). The mixture is stirred at room temperature for 6 hours to obtain a light yellow solution. After the reaction is completed, the solvent is removed by rotary evaporation, and the crude product is purified by silica gel column chromatography (eluent: petroleum ether / dichloromethane = 4 / 1) to obtain a colorless oily liquid compound 3.
[0074] The synthesis steps of 3,3'-dimethoxy-2,2'-bithiophene are as follows: in a round-bottom flask, compound 2 and compound 3 are dissolved in degassed toluene. Under argon protection, tetrakistriphenylphosphine palladium (i.e., Pd(PPh3)4) is added, and the reaction is moved to a 100°C oil bath and stirred for 24 hours. After the reaction is completed, the reaction solution is poured into water to quench the reaction, extracted with dichloromethane, the organic phase is dried with anhydrous magnesium sulfate, and the magnesium sulfate is removed by vacuum filtration. The filtrate is spun to remove the solvent, and the crude product is purified by silica gel column chromatography (eluent: petroleum ether / dichloromethane = 4 / 1) to obtain 3,3'-dimethoxy-2,2'-bithiophene as a white solid.
[0075] S120, under an ammonia atmosphere, dissolving the intermediate and potassium carbonate in a molar ratio of 1:(3-5) in a mixed solution of methanol and N-methylpyrrolidone, and reacting at 85-95° C. for at least 36 hours; after cooling to 15-25° C., reacting at -78--75° C. for at least 12 hours, and performing a second purification to obtain a passivation additive.
[0076] Among them, the synthetic route of forming the passivation additive from the intermediate is as follows:
[0077]
[0078] As an example, the molar ratio of the intermediate to potassium carbonate can be 1:3, 1:3.2, 1:3.5, 1:4.0, 1:4.5, 1:4.8 or 1:5.0, etc.
[0079] Furthermore, the molar ratio of the intermediate to potassium carbonate is 1:(3.8-4.2), which allows the intermediate to react fully, so that the α positions of both ends of the thiophene structure are connected to amino groups.
[0080] In the present application, the intermediate reacts with potassium carbonate at 85-95° C. for at least 36 h (i.e., the first reaction). As an example, the temperature of the first reaction can be 85° C., 87° C., 90° C., 92° C., or 95° C., etc., and the time of the first reaction can be 36 h, 40 h, 48 h, 50 h, or various long times, etc.
[0081] In the present application, the time of the first reaction is at least 48 hours, which is conducive to the sufficient reaction of the intermediate with potassium carbonate.
[0082] In the present application, after the first reaction, the reaction is carried out at -78 to -75°C for at least 12 hours (i.e., the second reaction) after cooling to 15 to 25°C (e.g., room temperature). As an example, the temperature of the second reaction can be -78°C, -77°C, -76°C, or -75°C, etc., and the time of the second reaction can be 12 hours, 15 hours, 17 hours, 20 hours, or various long times, etc.
[0083] As an example, the second reaction can be carried out in a dry ice acetone bath, the temperature of which is approximately -78°C.
[0084] In the present application, the molar concentrations of the intermediate and potassium carbonate in the mixed solution are 0.1-0.15 M and 0.45-0.55 M, respectively, which is beneficial to the reaction rate of the intermediate conversion to form the passivation additive.
[0085] As an example, the molar concentration of the intermediate in the mixed solution can be 0.1M, 0.12M, 0.14M or 0.15M, etc. The molar concentration of potassium carbonate in the mixed solution can be 0.45M, 0.47M, 0.5M, 0.52M or 0.55M, etc.
[0086] In the present application, the second purification is column chromatography purification, and the eluent of the second purification is n-hexane and ethyl acetate in a volume ratio of (4.5-5.5):1, which can quickly elute to obtain the purified passivation additive.
[0087] As an example, in the second purification eluent, the volume ratio of n-hexane to ethyl acetate can be 4.5:1, 4.7:1, 5.0:1, 5.2:1 or 5.5:1, etc.
[0088] Furthermore, the eluent for the second purification is n-hexane and ethyl acetate in a volume ratio of (4.8-5.2):1, which is conducive to further rapid elution to obtain the purified passivation additive.
[0089] Furthermore, the second purified eluent also contains triethylamine, and the volume fraction of triethylamine in the entire second purified eluent is 0.45-0.55%, which is conducive to further rapid elution to obtain the purified passivation additive.
[0090] In the present application, in the mixed solution, the volume ratio of methanol (MeOH) to N-methylpyrrolidone (NMP) is 1:(0.8-1.2).
[0091] The present application provides a passivation additive, and the passivation additive is prepared by the preparation method of the passivation additive provided above.
[0092] The passivation additive provided in the present application has a thiophene structure skeleton, and the α positions at both ends of the thiophene structure are connected to amino groups, and the two β positions of the thiophene structure are connected to methoxy groups, which can not only improve the self-aggregation effect of the passivation additive, but also improve the conductivity of the passivation additive, which is beneficial to improving the passivation effect of the passivation additive on the defects of the perovskite layer, and further helps to improve the stability of the open circuit voltage and energy conversion efficiency of the solar cell.
[0093] The present application also provides a passivation additive, the structural formula of the passivation additive is as follows:
[0094]
[0095] The passivation additive provided in the present application has a thiophene structure skeleton, and the α positions at both ends of the thiophene structure are connected to amino groups, and the two β positions of the thiophene structure are connected to methoxy groups, which can not only improve the self-aggregation effect of the passivation additive, but also improve the conductivity of the passivation additive, which is beneficial to improving the passivation effect of the passivation additive on the defects of the perovskite layer, and further helps to improve the stability of the open circuit voltage and energy conversion efficiency of the solar cell.
[0096] The present application also provides a solar cell 10, Figure 2 For a schematic diagram of the structure of the solar cell 10 provided in the embodiment of the present application, please refer to Figure 2 The solar cell 10 includes a transparent conductive layer 110, a hole transport layer 120, a perovskite layer 130, an electron transport layer 140, a buffer layer 150 and a metal electrode 160 stacked in sequence. The perovskite layer 130 contains a perovskite active material and the passivation additive provided above.
[0097] Since the passivation additive provided in the present application can effectively passivate the defects of the perovskite layer 130 , the conductivity, open circuit voltage and stability of energy conversion efficiency of the solar cell 10 can be improved.
[0098] In the present application, the mass of the passivation additive is 0.05-0.2% of the mass of the perovskite active material, which is not only conducive to ensuring the passivation effect of the passivation additive on the defects of the perovskite layer 130, but also conducive to avoiding the situation where too much passivation additive causes a certain degree of damage to the crystallization of the perovskite layer 130. If the amount of the passivation additive added is small, it may lead to poor passivation effect of the passivation additive on the defects of the perovskite layer 130; if the amount of the passivation additive added is large, it may destroy the crystallization of the perovskite layer 130, which is not conducive to ensuring the efficiency of the solar cell 10.
[0099] The present application also provides a method for preparing the solar cell 10 provided above, comprising: coating a solution containing a perovskite active material and a passivation additive onto the surface of the hole transport layer 120 , and then performing an annealing treatment to form a perovskite layer 130 .
[0100] The preparation method of the solar cell 10 provided in the present application can ensure that the perovskite layer 130 of the formed solar cell 10 contains perovskite active materials and the passivation additive provided in the present application, which can effectively passivate the defects of the perovskite layer 130, thereby facilitating improving the conductivity, open circuit voltage and energy conversion efficiency stability of the solar cell 10.
[0101] It should be noted that the present application does not limit the preparation process of the transparent conductive layer 110 , the hole transport layer 120 , the electron transport layer 140 , the buffer layer 150 and the metal electrode 160 , and conventional processes in the current industry may be used.
[0102] In the present application, the annealing temperature for forming the perovskite layer 130 is 90-110° C., and the annealing time is 5-30 minutes. The above annealing conditions are conducive to accelerating the crystallization of the perovskite layer 130 and improving the crystal quality of the perovskite layer 130 .
[0103] As an example, the temperature of the annealing treatment for forming the perovskite layer 130 can be 90°C, 95°C, 100°C, 102°C, 105°C or 110°C, etc., and the time of the annealing treatment for forming the perovskite layer 130 can be 5min, 10min, 15min, 20min, 25min or 30min, etc.
[0104] In the present application, a solution containing a perovskite active material and a passivation additive is applied to the surface of the hole transport layer 120 by spin coating, wherein the spin coating speed is 3000-4000 rpm and the spin coating time is 20-50 s. The above spin coating conditions are conducive to improving the flatness and thickness uniformity of the formed perovskite layer 130.
[0105] As an example, the spin coating rotation speed can be 3000 rpm, 3100 rpm, 3300 rpm, 3500 rpm, 3700 rpm or 4000 rpm, etc., and the spin coating time is 20s, 25s, 30s, 40s or 50s, etc.
[0106] In the present application, the solvent in the solution containing the perovskite active material and the passivation additive is a mixture of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), and the volume ratio of N,N-dimethylformamide to dimethyl sulfoxide is (2-5):1.
[0107] Furthermore, the perovskite active material is CH3NH3PbI3, and the molar concentration of the perovskite active material in the solution is 1 to 2M.
[0108] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0109] Example 1
[0110] This embodiment provides a passivation additive, which is prepared by the following steps:
[0111] (1) N-bromosuccinimide (0.53 g, 3.00 mmol) and 3,3'-dimethoxy-2,2'-bithiophene (0.34 g, 1.50 mmol) were dissolved in 10 mL of THF. The mixture was stirred at room temperature for 6 h to obtain a yellow solution. After the reaction was completed, the solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography (eluent: petroleum ether / dichloromethane = 3 / 1) to obtain an intermediate (white solid).
[0112] (2) Add the intermediate (0.38 g, 1.00 mmol), a mixture of MeOH and NMP (8 mL) with a volume ratio of 1:1, and potassium carbonate (0.052 g, 4 mmol) to a 25 mL two-necked flask, connect the flask to an ammonia bottle and purge it with ammonia, and heat it to 90°C for 48 h. Then cool the reaction flask to room temperature and immerse it in a dry ice acetone bath. Disconnect the ammonia bottle from the reaction flask, and carefully discharge the excess ammonia into the fume hood while warming the reaction flask to room temperature. Transfer the reaction solution to a round-bottom flask, remove the volatile solvent by rotary evaporation, and purify the crude product by silica gel column chromatography (eluent: n-hexane / ethyl acetate = 5 / 1, and add 0.5% triethylamine by volume to the eluent) to obtain a passivation additive (white solid, denoted as DADT-O).
[0113] Example 2
[0114] This embodiment provides a method for preparing a solar cell, which is prepared by the following steps:
[0115] (1) A 1 mg / mL 2PACz (CAS No. 20999-38-6) ethanol solution was spin-coated on a UV-ozone treated conductive glass layer (i.e., an ITO glass substrate) as a hole transport layer at a spin coating speed of 5000 rpm for 30 s. After the spin coating, the substrate was annealed at 100°C for 10 min.
[0116] (2) A 1.5 mol / L CH3NH3PbI3 solution (wherein the solvent is a mixture of DMF and DMSO in a volume ratio of 4 / 1) was spin-coated on the hole transport layer as a perovskite layer. The spin-coating speed was 3500 rpm and the spin-coating time was 35 s. At the 12th second before the spin-coating, 200 μL of chlorobenzene was added as an anti-solvent. After the spin-coating, the layer was annealed at 100°C for 15 min.
[0117] The CH3NH3PbI3 solution is added with DADT-O prepared in Example 1, and the added amount of DADT-O is 0.1 wt% of the mass of CH3NH3PbI3.
[0118] (3) Add 20 mg / mL PC 61 The chlorobenzene solution of BM was spin-coated on the perovskite layer as an electron transport layer. The spin-coating speed was 3000 rpm and the spin-coating time was 30 s. After the spin-coating, the layer was annealed at 100 °C for 10 min.
[0119] (4) A 0.5 mg / mL BCP (copper bath spirit) ethanol solution was spin-coated on the electron transport layer as a buffer layer. The spin coating speed was 4000 rpm and the spin coating time was 30 s. After the spin coating, the film was annealed at 100 °C for 1 min.
[0120] (5) A 100 nm thick layer of elemental silver is deposited on the buffer layer by thermal evaporation to serve as the metal electrode of the perovskite solar cell.
[0121] Comparative Example 1
[0122] This comparative example provides a passivation additive, which is prepared by the following steps:
[0123]
[0124] 5,5'-dibromo-2,2'-bithiophene (CAS: 4805-22-5) (0.32 g, 1.00 mmol), a mixture of MeOH and NMP (8 mL) with a volume ratio of 1:1, and potassium carbonate (0.052 g, 4 mmol) were added to a 25 mL two-necked flask. The flask was connected to an ammonia bottle and purged with ammonia, and heated to 90 ° C for 48 h. The reaction flask was then cooled to room temperature and immersed in a dry ice acetone bath. The ammonia bottle was disconnected from the reaction flask, and the excess ammonia was carefully discharged into the fume hood, while the reaction flask was heated to room temperature. The reaction solution was transferred to a round-bottomed flask, and the volatile solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography (eluent: n-hexane / ethyl acetate = 7 / 1, and triethylamine with a volume fraction of 0.5% was added to the eluent) to obtain a passivation additive (white solid, denoted as DADT).
[0125] Comparative Example 2
[0126] This comparative example provides a method for preparing a solar cell. The difference between this comparative example and Example 2 is that the DADT prepared in Comparative Example 1 is replaced by the DADT-O used in Example 2.
[0127] Experimental Example 1
[0128] Density functional theory (DFT) calculations were performed on the passivation additives prepared in Example 1 and Comparative Example 1, and the optimal conformation diagrams of the passivation additives prepared in Example 1 and Comparative Example 1 were respectively as follows: Figure 3 and Figure 4 As shown, the electron cloud distribution diagrams of the passivation additives prepared in Example 1 and Comparative Example 1 are respectively as shown in Figure 5-6 and Figure 7-8 shown.
[0129] in, Figure 3 Part A in the middle is the front view of the optimal conformation of DADT-O. Figure 3 Part B in the middle is a top view of the optimal conformation of DADT-O; Figure 4 Part A in the middle is the front view of the optimal conformation of DADT. Figure 4 Part B in the middle is a top view of the optimal conformation of DADT; Figure 5 The middle one is the HOMO electron cloud distribution diagram of DADT-O. Figure 6 is the LUMO electron cloud distribution diagram of DADT-O, Figure 7 is the HOMO electron cloud distribution diagram of DADT, Figure 8 This is the LUMO electron cloud distribution diagram of DADT.
[0130] from Figure 3 and Figure 4 It can be seen from the comparison that the two thiophenes in the DADT-O molecule prepared in Example 1 have better coplanarity, which is more conducive to charge transfer and molecular self-aggregation.
[0131] from Figures 5 to 8 It can be seen that the DADT-O prepared in Example 1 has higher HOMO and LUMO energy levels and is more suitable for charge transport.
[0132] Experimental Example 2
[0133] The stability of the open circuit voltage (Voc) of the solar cells prepared in Example 2 and Comparative Example 2 was tested to test the change in the open circuit voltage of the solar cells during 380 hours in a nitrogen atmosphere. The test results are as follows: Fig. 9 shown.
[0134] from Fig. 9It can be seen that the solar cell prepared in Example 2 exhibits excellent open circuit voltage stability, and its open circuit voltage has no obvious attenuation during being placed in a nitrogen atmosphere for 380 hours; and the open circuit voltage stability of the solar cell prepared in Comparative Example 2 is higher, indicating that the passivation additive DADT-O prepared in Example 1 of the present application can effectively passivate the defects of the perovskite layer in the prepared solar cell compared with the passivation additive DADT prepared in Comparative Example 1, thereby improving the stability of the open circuit voltage of the prepared solar cell.
[0135] Experimental Example 3
[0136] The stability of the energy conversion efficiency (PCE) of the solar cells prepared in Example 2 and Comparative Example 2 was tested to test the change in energy conversion efficiency of the solar cells during 380 hours in a nitrogen atmosphere. The test results are as follows: Fig.10 shown.
[0137] from Fig.10 It can be seen that the solar cell prepared in Example 2 exhibits excellent energy conversion efficiency stability, and the attenuation of its energy conversion efficiency during 380 hours in a nitrogen atmosphere is less than 2%; and the energy conversion efficiency stability is higher than that of the solar cell prepared in Comparative Example 2, indicating that the passivation additive DADT-O prepared in Example 1 of the present application can effectively passivate the defects of the perovskite layer in the prepared solar cell compared with the passivation additive DADT prepared in Comparative Example 1, thereby improving the stability of the energy conversion efficiency of the prepared solar cell.
[0138] Experimental Example 4
[0139] The electron mobility of the passivation additives prepared in Example 1 and Comparative Example 1 was tested, and the test results are as follows: Fig.11 shown.
[0140] from Fig.11 It can be seen that the electron mobility of the DADT-O molecule prepared in Example 1 is 8.87×10 -4 cm 2 V -1 s -1 , has good conductivity and will not hinder the transmission of electrons between the grains of the perovskite layer.
[0141] In summary, the passivation additive provided in the present application has a thiophene structure skeleton, and the α positions at both ends of the thiophene structure are connected to amino groups, and the two β positions of the thiophene structure are connected to methoxy groups, which can not only improve the self-aggregation effect of the passivation additive, but also improve the conductivity of the passivation additive, which is beneficial to improving the passivation effect of the passivation additive on the defects of the perovskite layer, and further helps to improve the stability of the open circuit voltage and energy conversion efficiency of the solar cell.
[0142] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
Claims
1. A method for preparing a passivation additive, characterized in that: include: Dissolve 3,3'-dimethoxy-2,2'-bithiophene and N-bromosuccinimide in tetrahydrofuran at a molar ratio of 1:(1-3), react at 15-25°C for at least 3h, and perform a first purification to obtain an intermediate; Under an ammonia atmosphere, dissolving the intermediate and potassium carbonate in a molar ratio of 1:(3-5) in a mixed solution of methanol and N-methylpyrrolidone, reacting at 85-95°C for at least 36 hours; after cooling to 15-25°C, reacting at -78--75°C for at least 12 hours, and performing a second purification; The structural formula of the passivation additive is as follows: ; The structural formula of the intermediate is as follows: 。 2. The preparation method according to claim 1, characterized in that: The first purification is column chromatography purification, and the eluent of the first purification is petroleum ether and dichloromethane in a volume ratio of (2.5-3.5):1; And / or, the second purification is column chromatography purification, and the eluent of the second purification is n-hexane and ethyl acetate in a volume ratio of (4.5~5.5):
1.
3. The preparation method according to claim 1 or 2, characterized in that: The molar concentrations of the 3,3'-dimethoxy-2,2'-bithiophene and the N-bromosuccinimide in the tetrahydrofuran are 0.1-0.2M and 0.25-0.35M, respectively; And / or, the molar concentrations of the intermediate and the potassium carbonate in the mixed solution are 0.1-0.15 M and 0.45-0.55 M, respectively.
4. The preparation method according to claim 3, characterized in that: In the mixed liquid, the volume ratio of the methanol to the N-methylpyrrolidone is 1:(0.8~1.2).
5. A passivation additive, characterized in that: The structural formula of the passivation additive is as follows: 。 6. A solar cell, characterized in that: The perovskite layer of the solar cell comprises: a perovskite active material and the passivation additive according to claim 5; The mass of the passivation additive is 0.05-0.2% of the mass of the perovskite active material.
7. A method for preparing a solar cell according to claim 6, characterized in that: include: After coating the solution containing the perovskite active material and the passivation additive onto the surface of the hole transport layer, an annealing treatment is performed.
8. The method for preparing a solar cell according to claim 7, characterized in that: The temperature of the annealing treatment is 90-110° C., and the time of the annealing treatment is 5-30 minutes.
9. The method for preparing a solar cell according to claim 7, characterized in that: The coating is carried out by spin coating, the rotation speed of the spin coating is 3000-4000 rpm, and the time of the spin coating is 20-50 s.
10. The method for preparing a solar cell according to claim 9, characterized in that: The molar concentration of the perovskite active material in the solution is 1-2M.
11. The method for preparing a solar cell according to claim 9, characterized in that: The perovskite active material is CH3NH3PbI3.
12. The method for preparing a solar cell according to claim 9, characterized in that: The solvent of the solution is a mixture of N,N-dimethylformamide and dimethyl sulfoxide, and the volume ratio of the N,N-dimethylformamide to the dimethyl sulfoxide is (2-5):1.