A polypeptide material with third-order nonlinear optical properties and its preparation method and application

By self-assembling the polypeptide monomer in a mixture of water, acetonitrile and trifluoroacetic acid, a nanotube structure with third-order nonlinear optical properties is solved, and the problem of insufficient environmental protection and bioaffinity of existing nonlinear optical materials is solved. It realizes efficient preparation of polypeptide materials and excellent nonlinear optical properties, providing new materials for biological applications.

CN116063382BActive Publication Date: 2024-11-05SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211440900.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-17
Publication Date
2024-11-05
Estimated Expiration
2042-11-17

AI Technical Summary

Technical Problem

Existing nonlinear optical materials have shortcomings in environmental protection and bioaffinity, which limits their use in biological applications, especially in the field of third-order nonlinear optical.

Method used

By fully dispersing the polypeptide monomer in a mixture of water, acetonitrile and trifluoroacetic acid, self-assembled by hydrogen bonding and π-π stacking, a nanotube structure with third-order nonlinear optical properties was formed, and an excellent nanotube structure was prepared. Polypeptide materials with nonlinear optical properties. The method is simple to operate, low cost, suitable for mild conditions, and realizes the chemical and physical stability of the material.

Benefits of technology

The obtained polypeptide material has good chemical and physical stability, excellent third-order nonlinear optical properties, and is suitable for the preparation of nonlinear optical devices. It provides new ideas for environmentally friendly, biologically affinity photoprotection and biological applications, and is prepared. The method is green and environmentally friendly and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003948202580000021
    Figure BDA0003948202580000021
  • Figure FDA0005012989270000011
    Figure FDA0005012989270000011
  • Figure HDA0003948202590000011
    Figure HDA0003948202590000011
Patent Text Reader

Abstract

The present invention provides a polypeptide material with third-order nonlinear optical properties, and a preparation method and application thereof. The preparation method of the polypeptide material of the present invention comprises the steps of: fully dispersing polypeptide monomers in a mixed solution of water, acetonitrile and trifluoroacetic acid, incubating to obtain a polypeptide solution; then filtering and drying to obtain a polypeptide material with third-order nonlinear optical properties; the method for preparing the polypeptide material of the present invention is simple to operate and low in cost; the obtained polypeptide material has good chemical and physical stability; and also has excellent nonlinear optical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonlinear optical materials, and in particular relates to a polypeptide material with third-order nonlinear optical performance and a preparation method and application thereof. Background Art

[0002] Nonlinear optical materials refer to materials whose optical parameters such as refractive index, absorption coefficient and polarizability are obviously dependent on the intensity of the incident light. There are many types of nonlinear optical materials. According to the nonlinear effect, they can be divided into second-order nonlinear optical materials, third-order nonlinear optical materials and higher-order nonlinear optical materials. According to the physical state of the material, they can be divided into liquid nonlinear optical materials, solid nonlinear optical materials and gas nonlinear optical materials, etc. Nonlinear optical materials have important applications in many fields due to their excellent refractive index, high nonlinearity, fast response, mechanical, photochemical and chemical stability, coherent blue light and green light, such as in many applications in displays, high-resolution printing and signal processing. However, the existing nonlinear optical materials need further research in terms of environmental protection and bioaffinity, which limits the biological application of nonlinear optical materials.

[0003] As a new type of biomaterial, peptide nanomaterials have many advantages, such as bioaffinity, easy preparation, good stability, etc. However, there are few reports on the use of peptide nanomaterials in the field of third-order nonlinear optics.

[0004] Therefore, there is an urgent need to develop an environmentally friendly and biocompatible nonlinear optical material. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a polypeptide material with third-order nonlinear optical properties and a preparation method and application thereof. The method for preparing the polypeptide material of the present invention is simple to operate and low in cost; the obtained polypeptide material has good chemical and physical stability; and also has excellent nonlinear optical properties.

[0006] The technical solution of the present invention is as follows:

[0007] A polypeptide material with third-order nonlinear optical performance. The microscopic morphology of the polypeptide material is a nanotube with a tube diameter of 35-70nm and a length of 2-10μm.

[0008] The method for preparing the above-mentioned polypeptide material having third-order nonlinear optical properties comprises the steps of:

[0009] The polypeptide monomer is fully dispersed in a mixed solution of water, acetonitrile and trifluoroacetic acid, and incubated to obtain a polypeptide solution; and then filtered and dried to obtain a polypeptide material having third-order nonlinear optical properties;

[0010] The structural formula of the polypeptide monomer is as follows:

[0011]

[0012] Preferably according to the present invention, in the mixed solution of water, acetonitrile and trifluoroacetic acid, the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1-2:0.01-0.02, and the pH of the mixed solution is 1.5-2; preferably, the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125, and the pH of the mixed solution is 1.7.

[0013] Preferably according to the present invention, the mass ratio of the polypeptide monomer to the volume ratio of the mixed solution is 0.2-2 mg / mL.

[0014] Preferably, according to the present invention, the method for fully dispersing the polypeptide monomer comprises the steps of: adding a mixture of water, acetonitrile and trifluoroacetic acid to the polypeptide monomer, vortexing for 1-3 minutes at room temperature, and ultrasonicating for 10-20 minutes.

[0015] Preferably, according to the present invention, the incubation temperature is 35-40° C., and the incubation time is 20-30 h; preferably, the incubation temperature is 37° C., and the incubation time is 24 h.

[0016] According to the present invention, preferably, the dispersion and incubation are both performed in a sealed environment.

[0017] According to the present invention, the polypeptide monomer can be directly commercially available.

[0018] The above-mentioned polypeptide material with third-order nonlinear optical performance is applied as a third-order nonlinear optical material to nonlinear optical devices.

[0019] The technical features and beneficial effects of the present invention are as follows:

[0020] 1. The present invention fully disperses polypeptide monomers of specific structure in a mixed solution of water, acetonitrile and trifluoroacetic acid, and the polypeptide monomer molecules self-assemble in the solution to form a polypeptide nanotube crystal structure through hydrogen bonds and π-π stacking between aromatic groups. Among them, the mixed solution of water and acetonitrile is conducive to the dissolution of polypeptide monomer powder and the self-assembly of polypeptide monomers; trifluoroacetic acid adjusts the pH value and provides an acidic incubation environment, which is conducive to the self-assembly of polypeptide monomers; water, acetonitrile and trifluoroacetic acid in the present invention work together to achieve the self-assembly of polypeptide monomers of specific structure in the present invention. The suitable constant temperature of the present invention can increase the speed of polypeptide self-assembly. The self-assembly method of the present invention is only for polypeptide molecules of specific structure in the present invention. The preparation method of the present invention is simple, mild, low cost, and green and environmentally friendly.

[0021] 2. The self-assembly obtained by the present invention is a nanotube with a diameter of 35-70nm and a length of 2-10μm, which is macroscopically regular and orderly. The polypeptide material prepared by the present invention has good chemical and optical stability and excellent third-order nonlinear optical properties, and can be used to prepare nonlinear optical devices. The polypeptide material prepared by the present invention is expected to become an environmentally friendly, bio-affinity light-protective biomaterial, providing new ideas for the design and development of optical and semiconductor materials and biological applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a transmission electron micrograph of the polypeptide material prepared in Example 1.

[0023] Figure 2 The third-order nonlinear optical absorption diagram (left) and refraction diagram (right) of the polypeptide material prepared in Example 1 are shown.

[0024] Figure 3 This is an atomic force microscope image of the polypeptide material prepared in Comparative Example 1.

[0025] Figure 4 This is an atomic force microscope image of the polypeptide material prepared in Comparative Example 2.

[0026] Figure 5 This is an atomic force microscope image of the polypeptide material prepared in Comparative Example 3. DETAILED DESCRIPTION

[0027] The present invention is further described below with reference to specific examples, but is not limited thereto. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0028] The polypeptide monomers used in the examples are available from Hefei Guopeptide Biotechnology Co., Ltd.

[0029] Example 1

[0030] A method for preparing a polypeptide material having third-order nonlinear optical properties comprises the steps of:

[0031] (1) Add a mixture of water, acetonitrile and trifluoroacetic acid to the polypeptide monomer powder to obtain a 0.2 mg / mL polypeptide solution, and seal the mixture with a sealing film. In the mixture of water, acetonitrile and trifluoroacetic acid, the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125, and the pH of the mixture is 1.7.

[0032] (2) The polypeptide solution was vortexed for 2 minutes at room temperature, ultrasonicated for 15 minutes, and placed in a 37°C constant temperature incubator for 24 hours to obtain a polypeptide solution. The polypeptide material with third-order nonlinear optical properties was then obtained by filtration and drying.

[0033] Using a transmission electron microscope, take 10 microliters of the above polypeptide solution and drop it on the copper mesh. Wait for 2 minutes, absorb the remaining liquid, and drop 10 microliters of the newly prepared 0.15% uranyl acetate solution on the copper mesh to stain the polypeptide for transmission electron microscope testing. Wait for 2 minutes and then absorb it. The copper mesh was placed at room temperature for 12 hours before testing. Figure 1 It can be seen that the polypeptide self-assembles into an ordered nanotube structure with a diameter of about 60nm and a length of about 5 microns.

[0034] Test of third-order nonlinear optical performance: Take 30 microliters of the above peptide solution and drop it on a freshly torn mica sheet and wait for it to dry. After drying, place the mica sheet under a laser beam with a wavelength of 532nm for Z-scan test. Figure 2 As shown in (left), when the sample moves from the negative direction to the positive direction and approaches the focus, the light intensity increases, the total absorption coefficient becomes larger and larger, and the energy transmitted through the sample decreases. When the sample is at the focus, the transmitted energy reaches the minimum value, forming a valley. After the sample passes the focus, as the light intensity continues to decrease, the absorption coefficient gradually decreases, and the energy transmitted through the sample gradually increases. At a distance from the focus, linear absorption is restored, and finally it appears as a single valley anti-saturation absorption curve that is symmetrical about the focus. Figure 2 As shown in (right), the sample moves from the negative direction to the positive direction. As the sample approaches the focus, the light intensity acting on the sample increases continuously. The sample in the area of ​​the light spot will produce a lens effect, which collimates the light beam before the focus and converges the light beam after passing the focus, making the transmission first larger and then smaller, showing a negative nonlinear refraction curve with a peak first and a valley later. The above shows that the polypeptide material of the present invention has excellent third-order nonlinear optical properties.

[0035] Example 2

[0036] A method for preparing a polypeptide material having third-order nonlinear optical properties comprises the steps of:

[0037] (1) Add a mixture of water, acetonitrile and trifluoroacetic acid to the polypeptide monomer powder to obtain a 2 mg / mL polypeptide solution, and seal the mixture with a sealing film. In the mixture of water, acetonitrile and trifluoroacetic acid, the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125, and the pH of the mixture is 1.7.

[0038] (2) The polypeptide solution was vortexed for 2 minutes at room temperature, ultrasonicated for 15 minutes, and placed in a 37°C constant temperature incubator for 24 hours to obtain a polypeptide solution. The polypeptide material with third-order nonlinear optical properties was then obtained by filtration and drying.

[0039] Example 3

[0040] A method for preparing a polypeptide material having third-order nonlinear optical properties comprises the steps of:

[0041] (1) Add a mixture of water, acetonitrile and trifluoroacetic acid to the polypeptide monomer powder to obtain a 1.5 mg / mL polypeptide solution, and seal the mixture with a sealing film. In the mixture of water, acetonitrile and trifluoroacetic acid, the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125, and the pH of the mixture is 1.7.

[0042] (2) The polypeptide solution was vortexed for 2 minutes at room temperature, ultrasonicated for 15 minutes, and placed in a 37°C constant temperature incubator for 24 hours to obtain a polypeptide solution. The polypeptide material with third-order nonlinear optical properties was then obtained by filtration and drying.

[0043] Comparative Example 1

[0044] A method for preparing a polypeptide material comprises the steps of:

[0045] (1) Prepare a mixture of water, acetonitrile and trifluoroacetic acid, wherein the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125; then add a 200 mmol / L sodium hydroxide aqueous solution to adjust the pH of the mixture to 4. Add the above mixture to the polypeptide monomer powder to obtain a 0.2 mg / mL polypeptide solution, and seal with a sealing film.

[0046] (2) The polypeptide solution was vortexed for 2 minutes at room temperature, ultrasonicated for 15 minutes, and placed in a 37°C constant temperature incubator for 24 hours to obtain a polypeptide solution, which was then filtered and dried to obtain a polypeptide material.

[0047] The atomic force microscope photo of the polypeptide material prepared in this comparative example is as follows Figure 3 As shown, the microscopic morphology of the prepared polypeptide material is not as good as the polypeptide material prepared in Example 1 of the present invention.

[0048] Comparative Example 2

[0049] A method for preparing a polypeptide material comprises the steps of:

[0050] (1) Prepare a mixture of water, acetonitrile and trifluoroacetic acid, wherein the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125; then add a 200 mmol / L sodium hydroxide aqueous solution to adjust the pH of the mixture to 6. Add the above mixture to the polypeptide monomer powder to obtain a 0.2 mg / mL polypeptide solution, and seal with a sealing film.

[0051] (2) The polypeptide solution was vortexed for 2 minutes at room temperature, ultrasonicated for 15 minutes, and placed in a 37°C constant temperature incubator for 24 hours to obtain a polypeptide solution, which was then filtered and dried to obtain a polypeptide material.

[0052] The atomic force microscope photo of the polypeptide material prepared in this comparative example is as follows Figure 4As shown, the microscopic morphology of the prepared polypeptide material is not as good as the polypeptide material prepared in Example 1 of the present invention.

[0053] Comparative Example 3

[0054] A method for preparing a polypeptide material comprises the steps of:

[0055] (1) Prepare a mixture of water, acetonitrile and trifluoroacetic acid, wherein the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125; then add a 200 mmol / L sodium hydroxide aqueous solution to adjust the pH of the mixture to 13. Add the above mixture to the polypeptide monomer powder to obtain a 0.2 mg / mL polypeptide solution, and seal with a sealing film.

[0056] (2) The polypeptide solution was vortexed for 2 minutes at room temperature, ultrasonicated for 15 minutes, and placed in a 37°C constant temperature incubator for 24 hours to obtain a polypeptide solution, which was then filtered and dried to obtain a polypeptide material.

[0057] The atomic force microscope photo of the polypeptide material prepared in this comparative example is as follows Figure 5 As shown, the microscopic morphology of the prepared polypeptide material is not as good as the polypeptide material prepared in Example 1 of the present invention.

Claims

1. A polypeptide material with third-order nonlinear optical properties, characterized in that: The microscopic morphology of the polypeptide material is: nanotubes with a tube diameter of 35-70nm and a length of 2-10μm; The preparation method of the polypeptide material with third-order nonlinear optical properties comprises the steps of: fully dispersing the polypeptide monomer in a mixed solution of water, acetonitrile and trifluoroacetic acid, incubating to obtain a polypeptide solution; then filtering and drying to obtain the polypeptide material with third-order nonlinear optical properties; the structural formula of the polypeptide monomer is as follows: In the mixed solution of water, acetonitrile and trifluoroacetic acid, the volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1-2:0.01-0.02, and the pH value of the mixed solution is 1.5-2.

2. The polypeptide material having third-order nonlinear optical properties according to claim 1, characterized in that: The volume ratio of water, acetonitrile and trifluoroacetic acid is 1:1.5:0.0125, and the pH of the mixture is 1.

7.

3. The polypeptide material having third-order nonlinear optical properties according to claim 1, characterized in that: The mass ratio of the polypeptide monomer to the volume ratio of the mixed solution is 0.2-2 mg / mL.

4. The polypeptide material having third-order nonlinear optical properties according to claim 1, characterized in that: The method for fully dispersing the polypeptide monomer comprises the steps of: adding a mixed solution of water, acetonitrile and trifluoroacetic acid into the polypeptide monomer, vortexing for 1-3 minutes at room temperature, and ultrasonicating for 10-20 minutes.

5. The polypeptide material having third-order nonlinear optical properties according to claim 1, characterized in that: The incubation temperature is 35-40°C and the incubation time is 20-30h.

6. The polypeptide material having third-order nonlinear optical properties according to claim 5, characterized in that: The incubation temperature was 37°C and the incubation time was 24 h.

7. The polypeptide material having third-order nonlinear optical properties according to claim 1, characterized in that: Both dispersion and incubation are carried out in a sealed environment.

8. The use of the polypeptide material having third-order nonlinear optical properties as claimed in claim 1, characterized in that: As a third-order nonlinear optical material, it is used in nonlinear optical devices.