Thermoplastic composite material with low volatile organic compound content and preparation method and application thereof

Through multi-component material system design and vacuum technology, the volatile organic compound content of long fiber-reinforced thermoplastic composite materials is reduced, solving the problems of material stability and high cost in the existing technology, and achieving high performance and low cost. Thermoplastic composite preparation.

CN116063776BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111277842.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-30
Publication Date
2024-10-15
Estimated Expiration
2041-10-30

AI Technical Summary

Technical Problem

It is difficult to effectively reduce the content of volatile organic compounds in existing long fiber reinforced thermoplastic composite materials at high temperatures. There are problems with adsorption balance and high cost. The existing technology cannot meet the development needs of environmentally friendly thermoplastic materials.

Method used

It adopts a multi-component material system design, including inner layer material and outer layer material. The core layer is formed by the first thermoplastic resin and the first additive, and the second thermoplastic resin layer is evenly coated on the outside of the core layer, combined with vacuuming. , adding a stripping agent to reduce the volatile organic compound content and improve the fluidity of the fibers in the resin melt.

Benefits of technology

It realizes the preparation of thermoplastic composite materials with low volatile organic compound content, improves the surface properties and application range of the materials, reduces injection molding process requirements, has low cost and wide applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116063776B_ABST
    Figure CN116063776B_ABST
Patent Text Reader

Abstract

The present invention discloses a thermoplastic composite material with a low volatile organic compound content, and a preparation method and application thereof. The thermoplastic composite material with a low volatile organic compound content comprises an inner layer material and at least one outer layer material, wherein the inner layer material is a core layer comprising a fiber bundle, a first thermoplastic resin and a first auxiliary agent, and the at least one outer layer material wraps the core layer and is a resin layer comprising a second thermoplastic resin and a second auxiliary agent, wherein the fiber bundle extends continuously from one end of the core layer to the opposite end thereof, and the first auxiliary agent and the second auxiliary agent comprise a stripping agent. The thermoplastic composite material with a low volatile organic compound content of the present invention is designed based on a multi-component material system, which can achieve a synergistic effect of performance between the components, and at the same time has excellent low VOC performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer composite materials, and in particular relates to a thermoplastic composite material with low volatile organic compound content and a preparation method and application thereof. Background Art

[0002] Long fiber reinforced thermoplastic composite is a common thermoplastic composite material, which is one of the fastest growing materials in the composite material market today. As a semi-structural material and structural material, the development target of long fiber reinforced thermoplastic composite is various fields of industry and civil use, including automobiles, equipment, entertainment, food processing, communications, electronic appliances, power tools, gardening and other fields.

[0003] The fiber length of long fiber reinforced thermoplastic materials is equivalent to the particle length, and the fiber orientation is highly consistent. It has the characteristics of low density, easy molding, high specific strength, high modulus, good fatigue resistance and non-water absorption. In addition, the material has good dimensional stability, excellent impact resistance, chemical stability (salt resistance, oil resistance, fuel resistance, etc.) and recyclability. It is especially suitable for use in occasions with frequent high and low temperature changes. It can be injection molded on ordinary injection molding machines or compression molded. It is an ideal candidate for metal replacement materials. In the total amount of long fiber reinforced thermoplastic composite materials, the application of automotive materials accounts for as much as 80%-90%.

[0004] However, with the continuous improvement of the technical level of long fiber reinforced thermoplastic composite materials and the continuous expansion of application cases, as well as the further improvement of people's awareness of health, safety and environmental protection and the continuous advancement of the automotive process, more and higher requirements have been put forward for the performance of materials. In addition to requiring materials to have excellent mechanical properties, functionalization and other requirements, they must also take into account the processing performance and the performance requirements of the parts after molding. For example, for large and complex automotive parts and high-precision electronic and electrical components, the prepared materials are required to have low volatile organic compound content (VOC), high flowability, easy molding, high dimensional stability, high surface quality and processing and molding requirements. Low volatile organic compound content is the current development trend of environmentally friendly thermoplastic materials. At present, there are many reports on the research of materials with low volatile organic compound content. Most of them use technologies such as adding adsorbents to materials, using devolatilization technology and chemical reactions to improve the emission of VOCs in the original materials.

[0005] First, use added adsorbents. This method mainly adds physical adsorbents such as activated carbon, porous silica, activated alumina, clay, bentonite, porous molecular sieves, etc. to the material, and extrude granules through a screw extruder under certain process conditions. Such as Chinese patent applications CN1727389A, CN1727390A, CN101817953A, CN101928429A, CN102020809A, etc. However, the products obtained by this method have the problem of adsorption equilibrium. At a higher temperature, the equilibrium moves in the direction of desorption, causing the volatile organic matter to continue to volatilize. Therefore, this type of method still has the hidden danger of VOC release in the later stage of the material.

[0006] Second, chemical reaction. For example, Chinese patent application CN101570612A reduces the content of volatile organic compounds by adding an inorganic photocatalyst to decompose small organic molecules, but this method has problems with photocatalytic efficiency and its effect is limited.

[0007] Third, the devolatilization method. This method mainly utilizes professional devolatilization equipment and technology to devolatilize during the polymerization and processing process. The devolatilization efficiency is high during the polymerization process, but due to the limitations of its production process and equipment, the cost is high and it is not easy to be widely used; during the processing, the devolatilization mainly utilizes a exhaust extruder to devolatilize the melt. For example, Chinese patent CN101255252B reduces the VOC of the material by adding low-molecular organic matter removers such as isopropanol / water. The low-molecular organic matter remover is mixed with other materials and then discharged from the same feed port of the extruder. This will cause the low-molecular organic matter remover to be heated and volatilized in advance in the feeding section or conveying section, thereby failing to achieve the maximum VOC removal effect, and this method has problems with compatibility and durability.

[0008] For the above-mentioned problems, the existing technology is far from meeting the needs of practical applications. Summary of the invention

[0009] In view of the above problems existing in the prior art, the present invention provides a thermoplastic composite material with low volatile organic compound content, a preparation method and application thereof. The thermoplastic composite material of the present invention is designed based on a multi-component material system, which can achieve a synergistic effect between the components, and at the same time has excellent low volatile organic compound content, and can realize the online addition of stripping agent to the thermoplastic composite material. Furthermore, the thermoplastic composite material of the present invention can also greatly improve the fluidity of the fiber in the resin melt, and the surface performance of the composite material is greatly improved, which expands the scope of application.

[0010] A first aspect of the present invention provides a thermoplastic composite material with a low volatile organic compound content, comprising an inner layer material and at least one outer layer material, wherein the inner layer material is a core layer comprising a fiber bundle, a first thermoplastic resin and a first auxiliary agent, and the at least one outer layer material wraps the core layer and is a resin layer comprising a second thermoplastic resin and a second auxiliary agent, wherein the fiber bundle extends continuously from one end of the core layer to the opposite end thereof, and the first auxiliary agent and the second auxiliary agent include a stripping agent.

[0011] The inventors of the present application have found that a first component including a first thermoplastic resin and a first auxiliary agent is used to impregnate a continuous fiber bundle to form a core layer, and a second component including a second thermoplastic resin is uniformly coated on the outside of the core layer, thereby forming a thermoplastic composite material with a low volatile organic compound content, which has a continuous fiber reinforced resin as a core layer (inner layer material) and a resin layer wrapped on the outside of the core layer as an outer layer material. A stripping masterbatch (stripping agent) is added to the thermoplastic composite material, which can be combined with a vacuum pump to ensure that the fiber bundle is fully impregnated in the thermoplastic resin, and further forcefully remove the VOC in the inner and outer layer materials. Such a thermoplastic composite material has excellent low volatile organic compound content performance, and can realize the online addition of a stripping agent to the thermoplastic composite material. In addition, by adjusting the performance and function of the first thermoplastic resin in the core layer and the second thermoplastic resin in the resin layer, the thermoplastic composite material with a low volatile organic compound content can have different performances and functions.

[0012] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the outer layer material (resin layer) can substantially continuously cover the inner layer material (core layer). Although not preferred, in the thermoplastic composite material with low volatile organic compound content of the present invention, the outer layer material (resin layer) covers at least 80% of the inner layer material (core layer), for example, 80-99%, 85-95% covers the inner layer material (core layer).

[0013] The terms "one end" and / or "opposite end" in the present invention are generally relative to the longitudinal direction of the thermoplastic composite material with a low volatile organic compound content.

[0014] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the thermoplastic composite material with low volatile organic compound content can be in strip, rod or granular form. Of course, the thermoplastic composite material with low volatile organic compound content of the present invention can also be in other shapes, such as continuous filaments. In the present invention, the thermoplastic composite material in strip, rod or granular form can be cut from the thermoplastic composite material in continuous filament form.

[0015] In some embodiments, the thermoplastic composite material with low volatile organic compound content is in the form of strips, rods or particles. The length (longitudinal dimension) of the thermoplastic composite material in the form of strips, rods or particles may be 5-30 mm, preferably 5-25 mm, and more preferably 6-15 mm.

[0016] In other embodiments, although not preferred, the thermoplastic composite material with low volatile organic compound content may also have a relatively small length dimension. For example, the thermoplastic composite material with low volatile organic compound content is in a granular form, and the particle size (length) of the granular thermoplastic composite material may also be 2-5 mm, preferably 3-4 mm.

[0017] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the present invention has no special requirements on the cross-sectional shape of the thermoplastic composite material with low volatile organic compound content. In some embodiments, the cross-sectional shape of the granular or rod-shaped thermoplastic composite material is circular or quasi-circular. In other embodiments, the cross-sectional shape of the granular or rod-shaped thermoplastic composite material can be rectangular or square.

[0018] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, and the amount of the fiber bundle is 10-110 parts by weight.

[0019] In some specific embodiments, in the inner layer material, the amount of the first thermoplastic resin can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, or a range consisting of these; and in some specific embodiments, the amount of the fiber bundle can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, or a range consisting of these.

[0020] In some preferred embodiments, in the inner layer material, the amount of the first thermoplastic resin may be 20-70 parts by weight, preferably 20-55 parts by weight, more preferably 24-45 parts by weight; and / or the amount of the fiber bundle may be 20-110 parts by weight, more preferably 25-110 parts by weight.

[0021] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, in the outer layer material, the amount of the second thermoplastic resin is 1-110 parts by weight.

[0022] In some specific embodiments, in the outer layer material, the amount of the second thermoplastic resin can be 1 part by weight, 10 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, 105 parts by weight, 110 parts by weight or a range consisting of these.

[0023] In some preferred embodiments, in the outer layer material, the amount of the second thermoplastic resin may be 10-99 parts by weight, more preferably 10-90 parts by weight, and preferably 40-90 parts by weight.

[0024] According to some specific embodiments of the thermoplastic composite material with low volatile organic compound content according to the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, preferably 20-70 parts by weight, more preferably 20-55 parts by weight, and further preferably 24-45 parts by weight; and / or the amount of the fiber bundle is 10-99 parts by weight, preferably 20-80 parts by weight, and more preferably 25-50 parts by weight.

[0025] According to other specific embodiments of the thermoplastic composite material with low volatile organic compound content according to the present invention, in the inner layer material, the amount of the first thermoplastic resin is 50-70 parts by weight, and more preferably 50-60 parts by weight; and / or the amount of the fiber bundle is 90-110 parts by weight, and more preferably 100-110 parts by weight; and / or in the outer layer material, the amount of the second thermoplastic resin is 90-110 parts by weight, and more preferably 95-105 parts by weight.

[0026] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25-6: 1. For example, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25: 1, 0.3: 1, 0.35: 1, 0.4: 1, 0.45: 1, 0.5: 1, 0.55: 1, 0.6: 1, 0.65: 1, 0.7: 1, 0.8: 1, 0.9: 1, 1: 1, 1.2: 1, 1.5: 1, 1.7: 1, 1.8: 1, 1.9: 1, 2: 1, 2.5: 1, 3: 1, 3.5: 1, 4: 1, 4.5: 1, 5: 1, 6: 1 or a range consisting of the above.

[0027] In some preferred embodiments, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin may be 0.35-4.5:1, preferably 1.7-4.5:1.

[0028] In the present invention, the dosage of the first auxiliary agent and the second auxiliary agent is not limited, in order to achieve the effects of the related auxiliary agents.

[0029] In different embodiments of the present invention, the number of layers of the outer layer material is not limited, and the outer layer material can be one layer or multiple layers. When the outer layer material is multiple layers, the multiple layers of outer layer material can be formed by one outer layer material or multiple outer layer materials.

[0030] According to some embodiments of the thermoplastic composite material with low volatile organic compound content according to the present invention, the first thermoplastic resin and the second thermoplastic resin are the same or different, and are each independently selected from at least one of polypropylene, polyethylene, polystyrene, polyvinyl chloride, polyacrylonitrile-butadiene-styrene copolymer, polyacrylonitrile-styrene copolymer, polyoxymethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polymethyl methacrylate, polycarbonate, polyphenylene ether, polyurethane, polyetheretherketone and polyphenylene sulfide and their alloy polymers.

[0031] According to a preferred embodiment of the thermoplastic composite material with low volatile organic compound content of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of polypropylene, polyethylene, polyamide (also known as nylon), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyphenylene sulfide, polyurethane and polyetheretherketone (PEEK).

[0032] According to a preferred embodiment of the thermoplastic composite material with low volatile organic compound content of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of homopolypropylene, copolymer polypropylene, a mixture of homopolypropylene and copolymer polypropylene, nylon 6 (PA6), nylon 66 (PA66), and a mixture of nylon 6 and nylon 66.

[0033] According to other embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the first thermoplastic resin and the second thermoplastic resin may also be selected from thermoplastic polyurethane elastomer (TPU) and / or high temperature nylon (PPA).

[0034] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 60-8000 g / 10 min. For example, the melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg can be 60 g / 10 min, 100 g / 10 min, 200 g / 10 min, 450 g / 10 min, 500 g / 10 min, 1000 g / 10 min, 1500 g / 10 min, 2000 g / 10 min, 3000 g / 10 min, 4000 g / 10 min, 5000 g / 10 min, 6000 g / 10 min, 7000 g / 10 min, 7500 g / 10 min, 8000 g / 10 min or a range consisting of the above.

[0035] In some preferred embodiments, the melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg may be 100-8000 g / 10 min, preferably 1000-7500 g / 10 min, and more preferably 1900-7500 g / 10 min.

[0036] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 0.1-8000 g / 10 min. For example, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg can be 0.1 g / 10 min, 1 g / 10 min, 1.5 g / 10 min, 3 g / 10 min, 10 g / 10 min, 20 g / 10 min, 30 g / 10 min, 40 g / 10 min, 45 g / 10 min, 50 g / 10 min, 55 g / 10 min, 60 g / 10 min, 70 g / 10 min, 80 g / 10 min, g / 10min, 90 g / 10min, 100 g / 10min, 450 g / 10min, 500 g / 10min, 800 g / 10min, 1000 g / 10min, 1500 g / 10min, 1900 g / 10min, 2500 g / 10min, 3000 g / 10min, 4000 g / 10min, 5000 g / 10min, 6000 g / 10min, 7000 g / 10min, 8000 g / 10min, or a range consisting of these.

[0037] In some preferred embodiments, the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg may be 3-55 g / 10 min or 450-8000 g / 10 min, preferably 3-45 g / 10 min or 1900-8000 g / 10 min.

[0038] In different embodiments of the present invention, the melt flow rates of the first thermoplastic resin and the second thermoplastic resin are not particularly specified, and the melt flow rates of the first thermoplastic resin and the second thermoplastic resin can be selected according to desired properties.

[0039] In particular, the inventors of the present application have found that according to the parameters of the present invention (e.g., melt flow rate), a thermoplastic composite material with a low volatile organic compound content having high surface quality performance and comprehensive performance can be prepared. For example, the melt flow rate of the first thermoplastic resin is higher than the melt flow rate of the second thermoplastic resin, thereby enabling the thermoplastic composite material with a low volatile organic compound content to have improved mechanical properties; conversely, the melt flow rate of the second thermoplastic resin is higher than the melt flow rate of the first thermoplastic resin, enabling the thermoplastic composite material with a low volatile organic compound content to have improved gloss.

[0040] According to some preferred embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16kg is 60-450g / 10min, for example, 60-200g / 10min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16kg is 3-55g / 10min or 450-8000g / 10min. In some specific embodiments, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16kg is 60-450g / 10min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16kg is 800-8000g / 10min.

[0041] According to other preferred embodiments of the thermoplastic composite material with low volatile organic compound content according to the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is above 450 g / 10 min, in particular greater than 450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is less than 100 g / 10 min, preferably 1.5-55 g / 10 min, and more preferably 3-50 g / 10 min.

[0042] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.05 to 12.5: 1. For example, the weight ratio of the second thermoplastic resin to the first thermoplastic resin can be 0.05: 1, 0.1: 1, 0.14: 1, 0.15: 1, 0.18: 1, 0.2: 1, 0.25: 1, 0.3: 1, 0.5: 1, 0.8: 1, 1: 1, 1.2: 1, 1.3: 1, 1.4: 1, 1.7: 1, 2: 1, 2.5: 1, 3: 1, 3.5: 1, 4: 1, 5: 1, 8: 1, 10: 1, 12.5: 1 or a range consisting of the above.

[0043] In some preferred embodiments, the weight ratio of the second thermoplastic resin to the first thermoplastic resin may be 0.1-4:1, preferably 0.14-3.5:1.

[0044] According to a preferred embodiment of the thermoplastic composite material with low volatile organic compound content of the present invention, when the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 800-8000 g / 10 min, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.25:1, preferably less than 0.18:1, and more preferably less than 0.15:1.

[0045] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, when the first thermoplastic resin and the second thermoplastic resin are selected from at least one of nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66, the viscosity of the selected nylon 6 and nylon 66 is 1.8-3.5. The viscosity of nylon in the present invention is the relative viscosity measured according to the Engler viscosity determination method GB / T266-88.

[0046] According to a specific embodiment of the thermoplastic composite material with low volatile organic compound content of the present invention, the first thermoplastic resin and the second thermoplastic resin can be homemade or commercially available.

[0047] For example, the first thermoplastic resin may be a polypropylene resin with a brand name of PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, a polypropylene resin with a brand name of M60RHC purchased from Sinopec East China Branch, or a nylon 6 with a brand name of PA6-BL3200H purchased from Sinopec Baling Branch.

[0048] For example, the second thermoplastic resin may be a polypropylene resin with a grade of PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, a polypropylene resin with a grade of PPH-T03 purchased from Sinopec Maoming Branch, a polypropylene resin with a grade of M50RH purchased from Sinopec East China Branch, a polypropylene resin with a grade of K8303 purchased from Yanshan Petrochemical Company, a polypropylene resin with a grade of PF1500 purchased from Hunan Shengjin New Materials Co., Ltd., or a polypropylene resin with a grade of PPH-Y450 purchased from Sinopec Shijiazhuang Refining and Chemical Company, or a nylon 6 with a grade of PA6-BL3200H purchased from Sinopec Baling Branch.

[0049] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the fiber bundle is selected from at least one of glass fiber, carbon fiber, basalt fiber, aromatic polyamide fiber, stainless steel fiber, synthetic resin fiber and mineral fiber.

[0050] According to a preferred embodiment of the thermoplastic composite material with low volatile organic compound content of the present invention, the glass fiber is a continuous glass fiber and / or a fixed-length glass fiber.

[0051] The fiber bundles suitable for use in the present invention can be alkali-free glass fibers with the brand name SE4805 purchased from Owens Corning (Shanghai) Glass Fiber Co., Ltd., alkali-free glass fibers with the brand name ER4301H purchased from Chongqing International Composite Materials Co., Ltd., carbon fibers with the brand name T700SC purchased from Toray Industries, Ltd. of Japan, and basalt fibers purchased from Mudanjiang Jinshi Basalt Fiber Co., Ltd.

[0052] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, on the transverse cross section of the thermoplastic composite material with low volatile organic compound content, from the inside to the outside, there are a core layer and a resin layer; the fiber bundle is oriented in the longitudinal direction of the thermoplastic composite material with low volatile organic compound content. Preferably, the length of the fiber bundle in the present invention is substantially the same as the length (longitudinal dimension) of the thermoplastic composite material with low volatile organic compound content, whereby the fiber bundle continuously extends from one end of the core layer in the longitudinal direction to the opposite end in the longitudinal direction.

[0053] In some preferred embodiments, the fiber bundle may be subjected to a dispersion treatment, which is known in the art and is not particularly limited in the present invention.

[0054] According to some embodiments of the thermoplastic composite material with a low volatile organic compound content of the present invention, the inner layer material does not contain short fibers, in particular, does not contain non-oriented short fibers.

[0055] In some specific embodiments, the inner layer material consists of a fiber bundle, a first thermoplastic resin, and a first auxiliary agent.

[0056] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the outer layer material does not contain fibers. In some preferred embodiments, the outer layer material is composed of a second thermoplastic resin and a second auxiliary agent.

[0057] According to other embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the outer layer material contains fibers, such as short fibers.

[0058] In some specific embodiments, in the outer layer material, the weight ratio of the fiber to the second thermoplastic resin is 1-50:100, preferably 5-50:100, and more preferably 20-45:100.

[0059] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the mass of the first thermoplastic resin and the second thermoplastic resin are each independently 0.5-4 parts by weight, preferably 1-4 parts by weight, more preferably 1-3.5 parts by weight, and further preferably 1-3 parts by weight.

[0060] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the stripping agent includes a foamed polymer carrier and a stripping aid supported thereon.

[0061] In the present invention, the stripping aid may be a low boiling point compound. Examples of stripping aids suitable for use in the present invention include, but are not limited to, water, ethanol, propanol, and isopropanol.

[0062] The present invention has no special restrictions on the content of the stripping agent in the stripping agent, and any known amount in the art can be used. The stripping agent can be commercially available, such as BYK-P4200 from BYK Chemicals, LDV1030 from Hefei Innovation Light Materials Co., Ltd., and LDV1030 from Yantai Xinxiu Chemical Technology Co., Ltd.

[0063] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the first thermoplastic resin and the second thermoplastic resin are 100 parts by weight, and the first auxiliary agent and the second auxiliary agent each independently include at least one of 0.5-15 parts by weight of a compatibilizer, 0.05-3 parts by weight of an antioxidant, and 0.05-2.5 parts by weight of a lubricant. Preferably, the first auxiliary agent and the second auxiliary agent each independently include at least one of 1-15 parts by weight, preferably 1-6 parts by weight, more preferably 3-6 parts by weight of a compatibilizer, 0.1-1 parts by weight, preferably 0.1-0.5 parts by weight of an antioxidant, and 0.5-2.5 parts by weight of a lubricant.

[0064] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the compatibilizer is selected from at least one of polar monomer graft-modified polymers. Preferably, the polar monomer is selected from at least one of maleic anhydride, maleic anhydride derivatives, acrylic acid and acrylate derivatives. Preferably, the polymer is selected from at least one of polyethylene, polypropylene, ethylene-α-olefin copolymer and propylene-α-olefin (α-olefin other than propylene) copolymer.

[0065] According to a specific embodiment of the thermoplastic composite material with low volatile organic compound content described in the present invention, maleic anhydride grafted polypropylene (PP-g-MAH) with a brand name of BONDYRAM 1001 purchased from Pluriram Plastic Industry Co., Ltd., maleic anhydride grafted ethylene-octene copolymer (POE-g-MAH) with a brand name of CMG9805 purchased from Shanghai Rizhisheng Technology Co., Ltd., titanate coupling agent with a brand name of NDZ12 purchased from Nanjing Shuguang Chemical Group Co., Ltd., or aluminate coupling agent with a brand name of XHY-501 purchased from Nanjing Youpu Chemical Co., Ltd. can be used as the compatibilizer.

[0066] According to some embodiments of the thermoplastic composite material with low volatile organic compound content according to the present invention, the antioxidant is selected from at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester (antioxidant 1010), tris[2,4-di-tert-butylphenyl]phosphite (antioxidant 168), β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1076), 2,2'-methylenebis(4-methyl-6-tert-butylphenol) (antioxidant 2246), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane (antioxidant CA) and bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite (antioxidant 626).

[0067] According to a specific embodiment of the thermoplastic composite material with low volatile organic compound content of the present invention, antioxidant 1010 and / or antioxidant 168 purchased from BASF can be used as the antioxidant.

[0068] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the lubricant is selected from at least one of ethylene bisstearamide, calcium stearate, polyethylene wax, pentaerythritol stearate, silicone, polyethylene glycol and fluorine-containing resin.

[0069] According to a specific embodiment of the thermoplastic composite material with low volatile organic compound content of the present invention, oxidized polyethylene wax with a brand name of XH-201 purchased from Xianghe Coatings Group can be used as the lubricant.

[0070] In different embodiments of the present invention, the first auxiliary agent may also include at least one of a lubricant, an antistatic agent and a plasticizer, and / or the second auxiliary agent may also include at least one of a lubricant, an antistatic agent, a plasticizer, a nucleating agent, a light stabilizer, a heat stabilizer, a masterbatch, an antistatic agent and a filler, and the specific types and amounts of the auxiliary agents are not limited, and a wide range of selection is possible.

[0071] A second aspect of the present invention provides a method for preparing a thermoplastic composite material with a low volatile organic compound content, the method comprising the following steps:

[0072] Step A, the first thermoplastic resin and the first auxiliary agent are mixed and then melted to obtain a first component melt; wherein the vacuum degree during melting is above -0.05 MPa, preferably above -0.08 MPa;

[0073] Step B, performing a first impregnation treatment on the continuous fiber bundle and the first component melt to form a filamentous core layer product;

[0074] Step C, the second thermoplastic resin and the second auxiliary agent are mixed and melted to obtain a second component melt; wherein the vacuum degree during melting is above -0.05 MPa, preferably above -0.08 MPa;

[0075] Step D: subjecting the filamentous core layer product to a second impregnation treatment with the second component melt to form a resin layer that continuously wraps the core layer.

[0076] According to some embodiments of the preparation method of the present invention, the preparation method can be carried out online continuously to obtain a continuous filamentary product. Such a continuous filamentary product can be directly stored and used, or cut into strips, rods or granular products with a certain length.

[0077] According to some embodiments of the preparation method of the present invention, the mixing conditions of step A include: temperature of 40-60° C., time of 0.5-20 min, preferably 1-10 min, more preferably 3-5 min.

[0078] According to some embodiments of the preparation method of the present invention, the melting temperature in step A is 200-380° C. In the present invention, the melting time can have a wide selection range, so as to fully melt the first thermoplastic resin and the first auxiliary agent to obtain a melt.

[0079] According to some embodiments of the preparation method of the present invention, preferably, in step B, before the continuous fiber is subjected to the first impregnation treatment with the first component melt, the continuous fiber is further subjected to dispersion treatment and preheating treatment, and the preheating temperature is preferably 80-250° C. The dispersion treatment process in the present invention adopts a conventional fiber dispersion treatment process in the art.

[0080] According to some embodiments of the preparation method of the present invention, the mixing conditions of step C include: temperature of 40-60° C., time of 0.5-20 min, preferably 1-10 min, more preferably 3-5 min.

[0081] According to some embodiments of the preparation method of the present invention, the melting temperature in step C is 200-380° C. In the present invention, the melting time can have a wide selection range, so as to fully melt the second thermoplastic resin and the optional second auxiliary agent.

[0082] According to some embodiments of the preparation method described in the present invention, the first impregnation treatment in step B can be carried out in a first impregnation mold, the first impregnation mold is an adjustable impregnation mold, the first impregnation mold includes a fiber inlet, a fiber outlet and a melt flow channel, and at least one first guide roller is arranged in the mold cavity of the first impregnation mold; the first guide roller can move between the fiber inlet and the fiber outlet; and / or, the first guide roller can move in a direction perpendicular to a line connecting the fiber inlet and the fiber outlet.

[0083] According to some embodiments of the preparation method described in the present invention, the first impregnation treatment in step B can be carried out in a second impregnation mold, and the second impregnation mold is a combined impregnation mold, which includes a first module, an intermediate module and a second module connected in sequence, the first module is provided with a fiber inlet and a first module flow channel, the second module is provided with a fiber outlet and a second module flow channel, and the intermediate module is provided with an intermediate module flow channel; after the first module, the intermediate module and the second module are connected in sequence, the first module flow channel, the intermediate module flow channel and the second module flow channel are connected to form a combined flow channel for the fiber to pass through.

[0084] According to some embodiments of the preparation method described in the present invention, the first impregnation treatment in step B can also be carried out in a third impregnation mold, and the third impregnation mold is a strong turbulence impregnation mold, and the third impregnation mold includes a fiber inlet channel, an impregnation outlet and a melt gap flow channel, and the fiber inlet channel, the impregnation outlet and the melt gap flow channel are all connected to the mold cavity inside the third impregnation mold; wherein, a second guide wire roller is arranged in the mold cavity of the third impregnation mold, and the second guide wire roller includes at least one active guide wire roller, and the active guide wire roller is driven to rotate by a driving device.

[0085] The first dipping mold, the second dipping mold and the third dipping mold used in the present invention are described in Chinese patent applications CN 202011193483.3, 202011191450.5 and 202011199839.4, the entire contents of which are incorporated herein by reference.

[0086] It should be noted that the first impregnation mold, the second impregnation mold and the third impregnation mold mentioned above in the present invention can be applied to any existing manufacturing system and preparation technology of thermoplastic composite materials with low volatile organic compound content, especially can be applied to any existing manufacturing system and preparation technology of continuous fiber reinforced expansion flame retardant thermoplastic composite materials.

[0087] According to some embodiments of the preparation method of the present invention, the second impregnation treatment in step D can be performed in a molding die. The molding die is composed of a core, a jacket, and a jacket mouth template. The core is located inside the jacket and forms a cavity with the jacket, and the resin melt can enter the cavity from the bottom or top or both sides of the jacket. The core can move back and forth in the jacket, and the pressure of the melt in the cavity is determined by adjusting the size of the formed cavity space. The pressure of the melt in the cavity can also be adjusted by the angle between the core and the jacket.

[0088] The working principle of the molding mold is as follows: after passing through the impregnation mold, a strip of inner layer impregnation material is formed, which is guided through the hole in the middle of the core, and then the composite structure of the inner and outer layer materials is formed in the cavity filled with mixed melt formed by the core and the outer jacket, and finally exported through the outer jacket mouth template.

[0089] According to some embodiments of the preparation method of the present invention, after step D, the method further includes drawing out, drawing, cooling, drying, and pelletizing the obtained thermoplastic composite material with a low volatile organic compound content. The process conditions for drawing out, drawing, cooling, drying, and pelletizing are not particularly limited and are within a wide selection range, with the purpose of obtaining a thermoplastic composite material with a low volatile organic compound content that meets different specifications.

[0090] According to some embodiments of the preparation method of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, and the amount of the fiber bundle is 10-110 parts by weight.

[0091] In some specific embodiments, in the inner layer material, the amount of the first thermoplastic resin can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, or a range consisting of these; and in some specific embodiments, the amount of the fiber bundle can be 1 part by weight, 10 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, 110 parts by weight, or a range consisting of these.

[0092] In some preferred embodiments, in the inner layer material, the amount of the first thermoplastic resin can be 20-70 parts by weight, preferably 20-55 parts by weight, and more preferably 24-45 parts by weight; and / or the amount of the fiber bundle can be 20-110 parts by weight, preferably 25-110 parts by weight.

[0093] According to some embodiments of the preparation method of the present invention, in the outer layer material, the amount of the second thermoplastic resin is 1-110 parts by weight.

[0094] In some specific embodiments, in the outer layer material, the amount of the second thermoplastic resin can be 1 part by weight, 10 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, 105 parts by weight, 110 parts by weight or a range consisting of these.

[0095] In some preferred embodiments, in the outer layer material, the amount of the second thermoplastic resin may be 10-90 parts by weight, preferably 40-90 parts by weight.

[0096] According to some specific embodiments of the preparation method of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight, preferably 20-70 parts by weight, more preferably 20-55 parts by weight, and further preferably 24-45 parts by weight; and / or the amount of the fiber bundle is 10-99 parts by weight, preferably 20-80 parts by weight, and more preferably 25-50 parts by weight.

[0097] According to other specific embodiments of the preparation method of the present invention, in the inner layer material, the amount of the first thermoplastic resin is 50-70 parts by weight, and more preferably 50-60 parts by weight; and / or the amount of the fiber bundle is 90-110 parts by weight, and more preferably 100-110 parts by weight; and / or in the outer layer material, the amount of the second thermoplastic resin is 90-110 parts by weight, and more preferably 95-105 parts by weight.

[0098] According to some embodiments of the preparation method of the present invention, in the inner layer material, the weight ratio of the fiber to the first thermoplastic resin is 0.25-6: 1. For example, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25: 1, 0.3: 1, 0.35: 1, 0.4: 1, 0.45: 1, 0.5: 1, 0.55: 1, 0.6: 1, 0.65: 1, 0.7: 1, 0.8: 1, 0.9: 1, 1: 1, 1.2: 1, 1.5: 1, 1.7: 1, 1.8: 1, 1.9: 1, 2: 1, 2.5: 1, 3: 1, 3.5: 1, 4: 1, 4.5: 1, 5: 1, 6: 1 or a range consisting of the above.

[0099] In some preferred embodiments, in the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin may be 0.35-4.5:1, preferably 0.43-4.5:1.

[0100] In different embodiments of the present invention, the number of layers of the outer layer material is not limited, and the outer layer material can be one layer or multiple layers. When the outer layer material is multiple layers, the multiple layers of outer layer material can be formed by one outer layer material or multiple outer layer materials.

[0101] According to some embodiments of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin are the same or different, and are independently selected from at least one of polypropylene, polyethylene, polystyrene, polyvinyl chloride, polyacrylonitrile-butadiene-styrene copolymer, polyacrylonitrile-styrene copolymer, polyoxymethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polymethyl methacrylate, polycarbonate, polyphenylene ether, polyurethane, polyetheretherketone and polyphenylene sulfide and their alloy polymers.

[0102] According to a preferred embodiment of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of polypropylene, polyethylene, polyamide (also known as nylon), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyphenylene sulfide, polyurethane and polyetheretherketone (PEEK).

[0103] According to a preferred embodiment of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin are each independently selected from at least one of homopolypropylene, copolymer polypropylene, a mixture of homopolypropylene and copolymer polypropylene, nylon 6 (PA6), nylon 66 (PA66), and a mixture of nylon 6 and nylon 66.

[0104] According to other embodiments of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin may also be selected from thermoplastic polyurethane elastomer (TPU) and / or high temperature nylon (PPA).

[0105] According to some embodiments of the preparation method of the present invention, the melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 60-8000 g / 10 min. For example, the melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg can be 60 g / 10 min, 100 g / 10 min, 200 g / 10 min, 450 g / 10 min, 500 g / 10 min, 1000 g / 10 min, 1500 g / 10 min, 2000 g / 10 min, 3000 g / 10 min, 4000 g / 10 min, 5000 g / 10 min, 6000 g / 10 min, 7000 g / 10 min, 7500 g / 10 min, 8000 g / 10 min or a range consisting of the above.

[0106] In some preferred embodiments, the melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg may be 100-8000 g / 10 min, preferably 1000-7500 g / 10 min, and more preferably 1900-7500 g / 10 min.

[0107] According to some embodiments of the preparation method of the present invention, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 0.1-8000 g / 10 min. For example, the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg can be 0.1 g / 10 min, 1 g / 10 min, 1.5 g / 10 min, 3 g / 10 min, 10 g / 10 min, 20 g / 10 min, 30 g / 10 min, 40 g / 10 min, 45 g / 10 min, 50 g / 10 min, 55 g / 10 min, 60 g / 10 min, 70 g / 10 min, 80 g / 10 min, g / 10min, 90 g / 10min, 100 g / 10min, 450 g / 10min, 500 g / 10min, 800 g / 10min, 1000 g / 10min, 1500 g / 10min, 1900 g / 10min, 2500 g / 10min, 3000 g / 10min, 4000 g / 10min, 5000 g / 10min, 6000 g / 10min, 7000 g / 10min, 8000 g / 10min, or a range consisting of these.

[0108] In some preferred embodiments, the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg may be 3-55 g / 10 min or 450-8000 g / 10 min, preferably 3-45 g / 10 min or 1900-8000 g / 10 min.

[0109] In different embodiments of the present invention, the melt flow rates of the first thermoplastic resin and the second thermoplastic resin are not particularly limited, and the melt flow rates of the first thermoplastic resin and the second thermoplastic resin can be selected according to the desired performance. In particular, the inventors of the present application have found that according to the preparation conditions (e.g., melt flow rate) of the present invention, a thermoplastic composite material with a low volatile organic compound content having high surface quality performance and comprehensive performance can be prepared. For example, the melt flow rate of the first thermoplastic resin is higher than the melt flow rate of the second thermoplastic resin, thereby enabling the thermoplastic composite material with a low volatile organic compound content to have improved mechanical properties; conversely, the melt flow rate of the second thermoplastic resin is higher than the melt flow rate of the first thermoplastic resin, which can enable the thermoplastic composite material with a low volatile organic compound content to have improved gloss.

[0110] According to some preferred embodiments of the preparation method of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16kg is 60-450g / 10min, for example, 60-200g / 10min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16kg is 3-55g / 10min or 450-8000g / 10min. In some specific embodiments, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16kg is 60-450g / 10min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16kg is 800-8000g / 10min.

[0111] According to other preferred embodiments of the preparation method of the present invention, the melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is above 450 g / 10 min, in particular greater than 450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is less than 100 g / 10 min, preferably 1.5-55 g / 10 min, and more preferably 3-50 g / 10 min.

[0112] According to some embodiments of the preparation method of the present invention, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.05 to 12.5: 1. For example, the weight ratio of the second thermoplastic resin to the first thermoplastic resin can be 0.05: 1, 0.1: 1, 0.14: 1, 0.15: 1, 0.18: 1, 0.2: 1, 0.25: 1, 0.3: 1, 0.5: 1, 0.8: 1, 1: 1, 1.2: 1, 1.3: 1, 1.4: 1, 1.7: 1, 2: 1, 2.5: 1, 3: 1, 3.5: 1, 4: 1, 5: 1, 8: 1, 10: 1, 12.5: 1 or a range consisting of the above.

[0113] In some preferred embodiments, the weight ratio of the second thermoplastic resin to the first thermoplastic resin may be 0.14-4:1, preferably 0.14-3.5:1.

[0114] According to a preferred embodiment of the preparation method of the present invention, when the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is 800-8000 g / 10 min, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.25:1, preferably less than 0.18:1, and more preferably less than 0.15:1.

[0115] According to some embodiments of the preparation method of the present invention, when the first thermoplastic resin and the second thermoplastic resin are selected from at least one of nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66, the viscosity of the selected nylon 6 and nylon 66 is 1.8-3.5.

[0116] According to a specific embodiment of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin can be homemade or commercially available.

[0117] For example, the first thermoplastic resin may be a polypropylene resin with a brand name of PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, a polypropylene resin with a brand name of M60RHC purchased from Sinopec East China Branch, or a nylon 6 with a brand name of PA6-BL3200H purchased from Sinopec Baling Branch.

[0118] For example, the second thermoplastic resin may be a polypropylene resin with a grade of PPB-M100-GH purchased from Sinopec Yangzi Petrochemical Company, a polypropylene resin with a grade of PPH-T03 purchased from Sinopec Maoming Branch, a polypropylene resin with a grade of M50RH purchased from Sinopec East China Branch, a polypropylene resin with a grade of K8303 purchased from Yanshan Petrochemical Company, a polypropylene resin with a grade of PF1500 purchased from Hunan Shengjin New Materials Co., Ltd., or a polypropylene resin with a grade of PPH-Y450 purchased from Sinopec Shijiazhuang Refining and Chemical Company, or a nylon 6 with a grade of PA6-BL3200H purchased from Sinopec Baling Branch.

[0119] According to some embodiments of the preparation method of the present invention, the fiber bundle is selected from at least one of glass fiber, carbon fiber, basalt fiber, aromatic polyamide fiber, stainless steel fiber, synthetic resin fiber and mineral fiber.

[0120] According to a preferred embodiment of the preparation method of the present invention, the glass fiber is a continuous glass fiber and / or a fixed-length glass fiber.

[0121] According to some embodiments of the preparation method of the present invention, based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the amount of the stripping agent is independently 0.5-4 parts by weight, preferably 1-4 parts by weight, more preferably 1-3.5 parts by weight, and further preferably 1-3 parts by weight.

[0122] According to some embodiments of the thermoplastic composite material with low volatile organic compound content of the present invention, the stripping agent includes a foamed polymer carrier and a stripping aid supported thereon.

[0123] In the present invention, the stripping aid may be a low boiling point compound. Examples of stripping aids suitable for use in the present invention include, but are not limited to, water, ethanol, propanol, and isopropanol.

[0124] The present invention has no special restrictions on the content of the stripping agent in the stripping agent, and any known amount in the art can be used. The stripping agent can be commercially available, such as BYK-P4200 from BYK Chemicals, LDV1030 from Hefei Innovation Light Materials Co., Ltd., and LDV1030 from Yantai Xinxiu Chemical Technology Co., Ltd.

[0125] According to some embodiments of the preparation method of the present invention, the first thermoplastic resin and the second thermoplastic resin are 100 parts by weight, and the first auxiliary agent and the second auxiliary agent each independently include at least one of 0.5-15 parts by weight of a compatibilizer, 0.05-3 parts by weight of an antioxidant, and 0.05-2.5 parts by weight of a lubricant. Preferably, the first auxiliary agent and the second auxiliary agent each independently include at least one of 1-15 parts by weight, preferably 1-6 parts by weight, more preferably 3-6 parts by weight of a compatibilizer, 0.1-1 parts by weight, preferably 0.1-0.5 parts by weight of an antioxidant, and 0.5-2.5 parts by weight of a lubricant.

[0126] According to some embodiments of the preparation method of the present invention, the compatibilizer is selected from at least one of polar monomer graft-modified polymers. Preferably, the polar monomer is selected from at least one of maleic anhydride, maleic anhydride derivatives, acrylic acid and acrylate derivatives. Preferably, the polymer is selected from at least one of polyethylene, polypropylene, ethylene-α-olefin copolymer and propylene-α-olefin (α-olefin other than propylene).

[0127] According to some embodiments of the preparation method of the present invention, the lubricant is selected from at least one of ethylene bisstearamide, calcium stearate, polyethylene wax, pentaerythritol stearate, silicone, polyethylene glycol and fluorine-containing resin.

[0128] In different embodiments of the present invention, the first auxiliary agent may also include at least one of a lubricant, an antistatic agent and a plasticizer, and the second auxiliary agent may also include at least one of a lubricant, an antistatic agent, a plasticizer, a nucleating agent, a light stabilizer, a flame retardant, a heat stabilizer, a masterbatch, an antistatic agent and a filler, and the specific types and amounts of the auxiliary agents are not limited, and the amounts can be selected within a wider range.

[0129] In some embodiments of the present invention, the preparation method of the present invention is as follows Figure 2 or Figure 3The process is carried out in the thermoplastic composite material manufacturing system with low volatile organic compound content shown in the figure. The specific structure and connection method of the thermoplastic composite material manufacturing system with low volatile organic compound content are described in the detailed implementation section.

[0130] The third aspect of the present invention provides the application of the above-mentioned thermoplastic composite material with low volatile organic compound content, and the thermoplastic composite material with low volatile organic compound content obtained by the above-mentioned preparation method in the fields of automobile industry, machinery manufacturing, electronic appliances, chemical environmental protection, aerospace communications and construction industry, preferably in large automobile parts and / or high-precision electronic and electrical components, more preferably in automobile front-end modules and / or all-plastic tailgate inner panels. But it is not limited thereto.

[0131] Beneficial effects of the present invention:

[0132] 1. The thermoplastic composite material with low volatile organic compound content prepared by the present invention has a composite structure of a core layer and an outer layer. The composite system design based on the multiple materials can achieve a synergistic effect of the performance between different components between the inner layer material and the outer layer material, can effectively improve the processing performance of the thermoplastic composite material with low volatile organic compound content and the lubricity between the fiber and the resin matrix during injection molding, and improve the fluidity of the fiber in the resin matrix melt, thereby improving the bonding state between the two, reducing the separation state between the two, and improving the fluidity of the entire material system, so that the comprehensive performance and surface quality of the prepared thermoplastic composite material are greatly improved, while reducing the requirements for the injection molding process, expanding the application range of the thermoplastic composite material with low volatile organic compound content, and having broad application prospects and economic significance.

[0133] 2. The thermoplastic composite material of the present invention can quickly remove residual VOC in the polymer melt under vacuum conditions by using a stripping agent, and has excellent low volatile organic compound content performance.

[0134] 3. The thermoplastic composite material with low volatile organic compound content of the present invention has low cost, short injection molding cycle, high dimensional stability of the product, high material strength, no need for secondary mixing during use, and functional materials can be added to the first component and / or the second component, especially the second component (resin layer), and has wide applicability. Further, the outer layer material of the thermoplastic composite material with low volatile organic compound content of the present invention can be fiber-free, has the advantages of good surface quality performance, no floating fibers on the surface, and has improved glossiness. BRIEF DESCRIPTION OF THE DRAWINGS

[0135] The accompanying drawings are used to further understand the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0136] Figure 1 This is a schematic diagram of the structure of a thermoplastic composite material with low volatile organic compound content according to an embodiment of the present invention;

[0137] Figure 2 It is a schematic structural diagram of a thermoplastic composite material manufacturing system with low volatile organic compound content in one embodiment of the present invention;

[0138] Figure 3 It is a schematic structural diagram of a thermoplastic composite material manufacturing system with low volatile organic compound content in another embodiment of the present invention;

[0139] Figure 4 A cross-sectional view of a first impregnation mold in one embodiment of the present invention;

[0140] Figure 5 A cross-sectional view of a second impregnation mold in one embodiment of the present invention;

[0141] Figure 6 is a cross-sectional view of a third dipping mold in one embodiment of the present invention;

[0142] Figure 7 A schematic diagram of a second immersion treatment in one embodiment of the present invention;

[0143] Figure 8 This is a cross-sectional view of a molding die used in the second dipping process according to one embodiment of the present invention.

[0144] Description of reference numerals:

[0145] 0-1, core layer; 0-2, fiber bundle; 0-3, resin layer;

[0146] 1. Fiber rack and fiber guide device; 2. Fiber pretreatment device; 3. First impregnation mold; 4. Melt plasticization feeding device; 5. Forming mold; 6. Cooling water tank; 7. Dryer; 8. Tractor; 9. Pelletizer; 10. Collection box;

[0147] A300, first impregnation die head; A1, fiber inlet; A2, second chute; A3, melt flow channel; A4, first chute; A5, upper die cover; A6, fiber outlet; A7, impregnation die body; A8, first guide roller;

[0148] B300, second impregnation die head; B1, fiber inlet; B2, melt flow channel; B3, first module; B31, first module flow channel; B4, combined flow channel; B5, standardized joint; B6, middle module; B61, middle module flow channel; B7, second module; B71, second module flow channel; B8, fiber outlet;

[0149] C300, the third impregnation die head; C1, the melt gap flow channel; C2, the impregnation die outer body; C3, the fiber inlet channel; C4, the active guide roller; C5, the driven guide roller; C6, the impregnation outlet;

[0150] 4-1, extruder I; 4-2, extruder II;

[0151] 5-1, core; 5-2, outer jacket; 5-3, outer jacket opening template; 5-4, material strip; 5-5, second resin inlet. DETAILED DESCRIPTION

[0152] In order to make the present invention more easily understood, the present invention will be described in detail below in conjunction with embodiments. These embodiments are only for illustration and are not intended to limit the application scope of the present invention.

[0153] The test method of the present invention and the equipment used in the test are as follows:

[0154] (1) The tensile strength test was carried out in accordance with ISO527-2 standard, with a tensile speed of 5 mm / min.

[0155] (2) The bending strength test was carried out in accordance with ISO178 standard, with a bending speed of 2 mm / min.

[0156] (3) Notched impact strength test is carried out according to ISO179 standard.

[0157] (4) The surface gloss test is carried out in accordance with ISO2813 standard.

[0158] (5) VOC testing is carried out in accordance with VDA277 standard.

[0159] Some of the reagents used in the present invention are from:

[0160] (1) PPB-M100-GH, melt flow rate of 100 g / 10 min, test conditions of 230 °C, 2.16 kg load, produced by Sinopec Yangzi Petrochemical Company.

[0161] (2) PF1500, melt flow rate 1500 g / 10 min, produced by Hunan Shengjin New Materials Co., Ltd.

[0162] (3) PPH-Y450, melt flow rate 450 g / 10 min, produced by Sinopec Shijiazhuang Refining and Chemical Company.

[0163] (4) BL3200H, viscosity 1.8, produced by Sinopec Baling Branch.

[0164] (5) SE4805, alkali-free glass fiber, diameter 17 μm, linear density 2400 tex, produced by Owens Corning (Shanghai) Glass Fiber Co., Ltd.

[0165] (6) ER4301H, alkali-free glass fiber, diameter 17 μm, linear density 2400 tex, produced by Chongqing International Composite Materials Co., Ltd.

[0166] (7) T700SC, carbon fiber, tow 1200-50C, produced by Toray Industries, Japan.

[0167] (8) Basalt fiber, single fiber diameter 12 μm, produced by Mudanjiang Jinshi Basalt Fiber Co., Ltd.

[0168] (9) PP-g-MAH brand is BONDYRAM 1001, produced by BONDYRAM Plastics Industries Ltd.

[0169] (10) POE-g-MAH brand is CMG9805, produced by Shanghai Rizhisheng Technology Co., Ltd.

[0170] (11) NDZ12, produced by Nanjing Shuguang Chemical Group Co., Ltd.

[0171] (12) XHY-501, produced by Nanjing Youpu Chemical Co., Ltd.

[0172] (13) Antioxidant 1010, produced by BASF.

[0173] (14) Antioxidant 168, produced by BASF.

[0174] (15) Stripping agent, BYK-P4200, produced by BYK Chemical Company of Germany.

[0175] (16) XH-201, produced by Xianghe Paint Group.

[0176] The present invention will be further described below in conjunction with the accompanying drawings.

[0177] Figure 1 The structure of the thermoplastic composite material with low volatile organic compound content of the present invention is shown. Figure 1As shown, the cross-section of the thermoplastic composite material with low volatile organic compound content of the present invention is circular, and includes a core layer 0-1 and a resin layer 0-3 from the inside to the outside, and the core layer 0-1 is distributed with fiber bundles 0-2 oriented in the longitudinal direction, and the fiber bundles 0-2 are uniformly dispersed in the core layer 0-1.

[0178] like Figure 2 and Figure 3 As shown, the manufacturing system of the present invention includes a fiber rack and fiber guide device 1, a fiber pretreatment device 2, a first impregnation mold 3, a melt plasticizing feeding device 4, a molding mold 5, a cooling water trough 6, a dryer 7, a traction machine 8, a pelletizer 9, a collection box 10 and an electronic control system (not shown in the figure) connected in sequence.

[0179] In the manufacturing system, the molding die 5 is used for molding the composite material of the inner and outer layer composite structure, and its structure is as follows: Figure 8 shown.

[0180] In the manufacturing system, the first impregnation mold 3 is used for impregnation of the fiber with the resin melt.

[0181] like Figure 4 As shown, in one embodiment, the first impregnation mold is an impregnation device with adjustable godet roller position, including a first impregnation mold die head A300, and the first impregnation mold die head A300 includes an impregnation mold body A7, a fiber inlet A1, a fiber outlet A6, and a melt flow channel A3. At least one first godet roller A8 is arranged in the mold cavity, wherein the first godet roller A8 can move between the fiber inlet A1 and the fiber outlet A6, or the first godet roller A8 can move in a direction perpendicular to the line connecting the fiber inlet A1 and the fiber outlet A6; or the first godet roller A8 can move both between the fiber inlet A1 and the fiber outlet A6 and in a direction perpendicular to the line connecting the fiber inlet A1 and the fiber outlet A6.

[0182] Taking the rectangular first dipping mold die A300 as an example, a plurality of first guide rollers A8 are arranged in the first dipping mold die A300, and the axial direction of each first guide roller A8 is the width direction of the first dipping mold die A300. Therefore, each first guide roller A8 can move along the length direction of the first dipping mold die A300, and can also move along the height direction, thereby changing the position of the first guide roller A8 in the first dipping mold die A300.

[0183] It can be understood that the axial direction of the first guide roller A8 can also be the length direction of the first dipping mold die A300. At this time, each first guide roller A8 can move along the width direction of the first dipping mold die A300, and can also move along the height direction of the first dipping mold die A300, thereby changing the position of the first guide roller A8 in the first dipping mold die A300.

[0184] Since the fiber (fiber bundle) needs to bypass the first wire guide roller A8 in the mold cavity in sequence when walking in the mold cavity of the first impregnation mold die head A300, the walking path of the fiber in the mold cavity can be changed by changing the position (horizontal position, longitudinal position, etc.) of the first wire guide roller A8 in the first impregnation mold die head A300, so that when the impregnation conditions required by the fiber change, there is no need to replace a new mold and only need to adjust the position of the first wire guide roller A8 in the first impregnation mold die head A300, thereby improving production efficiency and production continuity. At the same time, the number of first impregnation mold die heads A300 can be reduced, saving production costs.

[0185] Specifically, the inventive concept of the present invention is to achieve the purpose of adjusting the position of the first guide roller A8 by means of grooving the inner wall of the mold cavity of the first impregnation mold die head A300.

[0186] A first chute A4 is provided on the first inner wall of the first impregnation die head A300. The first chute A4 extends between the fiber inlet A1 and the fiber outlet A6 (i.e. Figure 4 The first wire guide roller A8 moves along the first slide groove A4 to change its horizontal position in the first impregnation mold die head A300.

[0187] Furthermore, a second chute A2 is also provided on the first inner wall of the first impregnation mold die head A300, and the second chute extends in a direction perpendicular to the first chute A4 (ie Figure 4 The first wire guide roller A8 moves along the second slide groove A2 to change its vertical position in the die head.

[0188] It should be noted that the first chute A4 and the second chute A2 can be connected. Thus, the first wire guide roller A8 can be moved arbitrarily in the longitudinal direction or the transverse direction, so that its position can be changed.

[0189] The cross-sections of the first slide groove A4 and the second slide groove A2 may be trapezoidal, circular, arc-shaped or rectangular, etc., which is not limited in the present invention.

[0190] Both ends of the first guide roller A8 are provided with adjustment devices (not shown in the figure), which are used to adjust the axial length of the first guide roller A8, wherein the minimum axial length of the first guide roller A8 is smaller than the distance between the first inner wall and the second inner wall, and the maximum axial length of the first guide roller A8 is larger than the distance between the first inner wall and the second inner wall.

[0191] like Figure 5As shown, in another embodiment of the present invention, the second impregnation mold is a combined impregnation mold, including a second impregnation mold die head B300, and the second impregnation mold die head B300 includes a first module B3, an intermediate module B6, and a second module B7 connected in sequence. Among them, the first module B3 is provided with a fiber inlet B1 and a first module flow channel B31, the second module B7 is provided with a fiber outlet B8 and a second module flow channel B71, and the intermediate module B6 is provided with an intermediate module flow channel B61.

[0192] After the first module B3, the middle module B6 and the second module B7 are connected in sequence, the first module flow channel B31, the middle module flow channel B61 and the second module flow channel B71 are connected to form a combined flow channel B4 for the fiber to pass through, wherein the number of the middle module B6 is at least one. That is, the first module B3 is the head module, the second module B7 is the tail module, and there are one or more middle modules B6 between the two. It should be noted that these middle modules B6 are also connected in sequence.

[0193] That is to say, the number of intermediate modules B6 can be increased or decreased as needed, so that when the impregnation requirements change, different intermediate modules B6 can be combined to form a combined second impregnation mold die head B300, thereby improving production continuity and production efficiency and saving the cost of additional mold opening.

[0194] Furthermore, by selecting different intermediate modules B6, the shape parameters (such as curvature, etc.) of the formed combined flow channel B4 can be changed, thereby changing the flow path of the fiber and the melt. The fiber impregnation angle and fiber tension in different stations of the mold can be changed, ultimately achieving the purpose of adjusting and optimizing the entire fiber impregnation process, and improving the adaptability of the second impregnation mold die head B300 to different resin matrices and fibers.

[0195] The first module B3, the middle module B6 and the second module B7 are placed in a mold frame, and are brought into close contact with each other through the restraining effect of the mold frame, thereby ensuring the sealing of the formed combined flow channel B4.

[0196] like Figure 5 As shown, an embodiment with two intermediate modules B6 is shown. Figure 5 In the illustrated embodiment, the downstream end of the first module flow channel B31 is connected to the upstream end of one of the intermediate module flow channels B61, the two intermediate module flow channels B61 are connected to each other, and the downstream section of the other intermediate module flow channel B61 is connected to the upstream end of the second intermediate module flow channel B71, thereby forming a combined flow channel B4 extending from the fiber inlet B1 to the fiber outlet B8.

[0197] It can be understood that by selecting different intermediate modules B6, different combined flow channels B4 can be obtained.

[0198] like Figure 5 As shown, the downstream end of the first module flow channel B31, the upstream end of the second module flow channel B71, and both ends of the middle module flow channel B61 are all located in the same plane, and are configured with standardized joints B5. In other words, the connections between the first module flow channel B31, the middle module flow channel B61, and the second module B71 are connected through standardized joints B5. Since the standardized joints B5 are all located in the same plane, and the shapes and sizes of the standardized joints B5 are the same, it is convenient to combine and connect different modules.

[0199] like Figure 6 As shown, in another embodiment of the present invention, the third impregnation mold is a strong turbulence impregnation mold, including a third impregnation mold head C300, the third impregnation mold head C300 includes an impregnation mold outer body C2, and the impregnation mold outer body C2 is provided with a fiber inlet channel C3, an impregnation outlet C6 and a melt gap flow channel C1, and the fiber inlet channel C3, the impregnation outlet C6 and the melt gap flow channel C1 are all connected with the mold cavity inside the impregnation mold outer body C2.

[0200] Among them, a second wire guide roller is arranged in the mold cavity of the impregnation mold outer body C2, and the second wire guide roller includes at least one active wire guide roller C4, and the active wire guide roller C4 is driven to rotate by a driving device (not shown in the figure). Since the rotation of the active wire guide roller C4 is driven by the driving device instead of being driven by the traction of the fiber, when the fiber passes through the active wire guide roller C4, the actively rotating active wire guide roller C4 helps to reduce the traction tension of the fiber and the friction between the fiber and the active wire guide roller C4, thereby reducing the amount of fiber breakage, ensuring the integrity of the fiber, and avoiding the situation where the fiber is pulled apart, thereby improving the mechanical properties of the material. Preferably, the second wire guide roller also includes at least one driven wire guide roller C5, and the driven wire guide roller C5 is driven by the fiber passing through the active wire guide roller C4; or the driven wire guide roller C5 is connected to the active wire guide roller C4 through a belt mechanism, a gear mechanism or a chain mechanism. Figure 6 As shown, an example with one active godet roller C4 and two driven godet rollers C5 is shown, wherein the two driven godet rollers C5 are arranged one above the other to extend the impregnation path of the fibers passing through them. The active godet roller C4 and the driven godet roller C5 may be at the same or different heights in the mold cavity.

[0201] Furthermore, the driving device may be a device such as a motor, a hydraulic mechanism or a reduction box that can drive the active guide roller C4 to rotate.

[0202] According to the traveling speed v1 of the fiber entering the mold cavity of the impregnation mold outer body C2, the corresponding tangential speed v2 of the active guide roller C4 can be selected. For example, the tangential speed v2 of the active guide roller C4 can be made the same as the traveling speed v1 of the fiber, that is, v1=v2, so as to achieve the purpose of reducing fiber breakage and wear, thereby ensuring the integrity of the fiber, promoting the degree of fiber impregnation, shortening the impregnation time, and improving production efficiency.

[0203] like Figure 2 As shown, the melt-plasticizing feeding device 4 is composed of a twin-screw extruder for melt-plasticizing materials. The twin-screw extruder is a co-rotating twin-screw extruder with a screw diameter of 25 mm-95 mm and an aspect ratio of 36:1-65:1. When the melt-plasticizing feeding device 4 is composed of one extruder 4, the melt-plasticized melt in the extruder is divided by a melt distributor and enters the impregnation mold and the molding mold respectively, and the melt flow control valve is used to control the respective flow rates.

[0204] like Figure 3 As shown, when the melt-plasticizing feeding device 4 is composed of two extruders 4-1 and 4-2, the melts that are melted and plasticized are respectively fed into the impregnation mold and the molding mold through the extruder I 4-1 and the extruder II 4-2. In this embodiment, the melt-plasticizing feeding device is composed of two extruders, namely, the extruder I 4-1 and the extruder II 4-2, and the melts that are melted and plasticized are respectively fed into the first impregnation mold 3 and the molding mold 5 through the extruder I 4-1 and the extruder II 4-2. The extruder I 4-1 and the extruder II 4-2 can be fed with the same or different materials, so that a composite material with the same or different materials for the inner layer and the outer layer can be prepared.

[0205] The fiber pretreatment device 2 is composed of a tension roller and a hot drying tunnel. This combination allows the tension on the fiber to be released to a certain extent when entering the hot drying tunnel, so as to adapt to fibers of different strengths and avoid the breakage of fibers with lower strength before entering the impregnation die. The surface of the tension roller in the fiber pretreatment device 2 needs to be plated with ceramic to increase the surface roughness and reduce the friction on the fiber.

[0206] In the manufacturing system, the fiber rack and fiber guide device 1 are used for fiber derivation and untwisting. The device is equipped with an automatic control untwisting device, which is linked with the traction machine 8 and electrically connected to the electric control system (such as a PLC control device).

[0207] In the manufacturing system, the cooling water tank 6, the dryer 7, the traction machine 8, the pelletizer 9, and the collecting box 10 are conventional equipment or devices known to those skilled in the art, and will not be described in detail here.

[0208] Figure 7 A schematic diagram showing a second dipping process using a forming die is shown, Figure 8 A cross-sectional view of a molding die used in the second dipping process is shown.

[0209] like Figure 8 As shown, in one embodiment, the molding die 5 is composed of a core 5-1, a jacket 5-2, and a jacket mouth template 5-3. The core 5-1 is located inside the jacket 5-2, and forms a cavity with the jacket 5-2. The resin melt can enter the cavity from the bottom or top or both sides of the jacket 5-2. The core 5-1 can move forward and backward in the jacket 5-2, and the pressure of the melt in the cavity is determined by adjusting the size of the formed cavity space. The pressure of the melt in the cavity can also be adjusted by the angle between the core 5-1 and the jacket 5-2. The working principle of the molding die 5 is: after passing through the impregnation mold 3, the material strip of the inner layer impregnation material is formed, and it is guided through the hole in the middle of the core 5-1, and then, the composite structure of the inner and outer layer materials is formed in the cavity filled with mixed melt formed by the core 5-1 and the jacket 5-2, and finally guided out through the jacket mouth template 5-3.

[0210] like Figure 7 As shown, the material strip 5-4 enters a cavity filled with a second component melt formed by a core (not shown) and a jacket 5-2 for processing, wherein the second component melt is fed into the cavity from a second resin inlet 5-5.

[0211] In the following examples and comparative examples, Figure 3 The manufacturing system shown is used to prepare a thermoplastic composite material with low volatile organic compound content, wherein the first impregnation treatment is selected from Figure 4 The first dipping mold shown, the second dipping process uses Figure 8 The molding die shown.

[0212] [Example 1]

[0213] (1) Weigh 50 parts by weight of dry PPB-M100-GH polypropylene resin (melt flow rate of 100 g / 10 min), 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1.75 parts by weight of BYK-P4200 and 0.5 parts by weight of XH-201, stir in a high-speed mixer at 50° C. for 3 min, keep the vacuum degree of the vacuum system of the equipment above -0.08 MPa, obtain a first component melt, and feed it into a first impregnation mold.

[0214] (2) 30 parts by weight of glass fiber SE4805 enters the first impregnation mold under the action of a traction machine, where it is infiltrated and dispersed with the first component melt to form a material strip, which is used as the inner layer material.

[0215] (3) Weigh 49 parts by weight of dry PPH-Y450 polypropylene resin (melt flow rate: 450 g / 10 min), 2.5 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 0.51 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0216] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0217] (5) The coating amount of the outer layer material is adjusted by adjusting the extrusion rate of the extruder for the outer layer material and the die outlet diameter of the die, so that the coating is carried out according to the amount specified in step (3), and the cutting speed of the pelletizer is adjusted so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 61.1 mm. In the composite material, the glass fiber SE4805 accounts for 21.6% by weight.

[0218] (6) The polypropylene composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0219] [Example 2]

[0220] (1) Weigh 20 parts by weight of dry self-made high-flow polypropylene (melt flow rate of 1000 g / 10 min), 0.6 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.05 parts by weight of antioxidant 168, 0.35 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min to obtain a first component melt, keep the vacuum degree of the equipment vacuum system above -0.08 MPa, and feed it into a first impregnation mold.

[0221] (2) 50 parts by weight of glass fiber SE4805 enters the first impregnation mold under the action of a traction machine, where it is infiltrated and dispersed with the melt to form a material strip, which is used as the inner layer material.

[0222] (3) Weigh 59 parts by weight of dry PPH-T03 polypropylene resin (melt flow rate 3 g / 10 min), 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1.2 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0223] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0224] (5) The coating amount of the outer layer material is adjusted by adjusting the extrusion amount of the outer layer material extruder and the die outlet diameter of the die, so that the coating is performed according to the amount specified in step (3), and the cutting speed of the pelletizer is adjusted so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 15 mm. In the composite material, the glass fiber SE4805 accounts for 36.8% by weight.

[0225] (6) The polypropylene composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0226] [Example 3]

[0227] (1) Weigh 20 parts by weight of dry self-made high-flow polypropylene (melt flow rate 7500 g / 10 min), 0.6 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.05 parts by weight of antioxidant 168, 0.35 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir in a high-speed mixer at 50° C. for 3 min, keep the vacuum degree of the vacuum system of the equipment above -0.08 MPa, obtain a first component melt, and feed it into a first impregnation mold.

[0228] (2) 80 parts by weight of glass fiber SE4805 enters the first impregnation mold under the action of a traction machine, where it is infiltrated and dispersed with the melt to form a material strip, which is used as the inner layer material.

[0229] (3) Weigh 69 parts by weight of dry K8303 polypropylene resin (melt flow rate 1.5 g / 10 min), 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 0.36 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0230] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0231] (5) The coating amount of the outer layer material is adjusted by adjusting the extrusion rate of the extruder for the outer layer material and the diameter of the die outlet, so that the coating is carried out according to the amount specified in step (3), and the cutting speed of the pelletizer is adjusted so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 18 mm. In the composite material, the glass fiber SE4805 accounts for 45.6% by weight.

[0232] (6) The polypropylene composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0233] [Example 4]

[0234] (1) Weigh 70 parts by weight of dry PPB-M100-GH (melt flow rate 100 g / 10 min), 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1.84 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir in a high-speed mixer at 50° C. for 3 min, keep the vacuum degree of the equipment vacuum system above -0.08 MPa, obtain a first component melt, and feed it into a first impregnation mold.

[0235] (2) 25 parts by weight of glass fiber SE4805 enters the first impregnation mold under the action of a traction machine, where it is infiltrated and dispersed with the melt to form a strip, which is used as the inner layer material.

[0236] (3) Weigh 10 parts by weight of dry self-made high-flow polypropylene (melt flow rate 1900 g / 10 min), 0.5 parts by weight of BONDYRAM 1001, 0.05 parts by weight of antioxidant 1010, 0.01 parts by weight of antioxidant 168, 0.21 parts by weight of BYK-P4200, and 0.25 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0237] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0238] (5) The coating amount of the outer layer material is adjusted by adjusting the extrusion amount of the outer layer material extruder and the die outlet diameter of the die, so that the coating is performed according to the amount specified in step (3), and the cutting speed of the pelletizer is adjusted so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 5 mm. In the composite material, the glass fiber SE4805 accounts for 22.4% by weight.

[0239] (6) The polypropylene composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0240] [Example 5]

[0241] (1) Weigh 57 parts by weight of dry M60RHC polypropylene resin (melt flow rate 60 g / 10 min), 2.5 parts by weight of BONDYRAM 1001, 0.5 parts by weight of NDZ12, 0.1 parts by weight of antioxidant 168, 0.5 parts by weight of BYK-P4200, and 0.25 parts by weight of XH-201, stir in a high-speed mixer at 50° C. for 3 min, maintain the vacuum degree of the equipment vacuum system above -0.08 MPa, obtain a first component melt, and feed it into a first impregnation mold.

[0242] (2) 40 parts by weight of glass fiber SE4805 enters the first impregnation mold under the action of a traction machine, where it is infiltrated and dispersed with the melt to form a strip, which is used as the inner layer material.

[0243] (3) Weigh 97 parts by weight of dry M50RH polypropylene resin (melt flow rate 50 g / 10 min), 4 parts by weight of BONDYRAM 1001, 0.8 parts by weight of NDZ12, 0.1 parts by weight of antioxidant 168, 2 parts by weight of BYK-P4200, and 0.8 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the equipment vacuum system above -0.08 MPa, to obtain a second component melt.

[0244] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0245] (5) The coating amount of the outer layer material is adjusted by adjusting the extrusion rate of the extruder for the outer layer material and the die outlet diameter of the die, so that the coating is carried out according to the amount specified in step (3), and the cutting speed of the pelletizer is adjusted so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 10 mm. In the composite material, the glass fiber SE4805 accounts for 19.4% by weight.

[0246] (6) The polypropylene composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0247] [Example 6]

[0248] (1) Weigh 57 parts by weight of dry PA6-BL3200H, 3 parts by weight of CMG9805, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 2 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min to obtain a first component melt, keep the vacuum degree of the equipment vacuum system above -0.08 MPa, and feed it into the first impregnation mold.

[0249] (2) ER4301H enters the first impregnation mold under the action of the traction machine, where it is infiltrated and dispersed with the first component melt to form a material strip, which is used as the inner layer material.

[0250] (3) Weigh 97 parts by weight of dry PA6-BL3200H, 3 parts by weight of CMG9805, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1 part by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0251] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0252] (5) adjusting the coating amount of the outer layer material by adjusting the extrusion rate of the extruder for the outer layer material and the die outlet diameter of the die, so that the coating is carried out according to the amount specified in step (3), and adjusting the cutting speed of the pelletizer so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 12 mm. In the composite material, ER4301H accounts for 40% by weight.

[0253] (6) The long glass fiber reinforced PA6 composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0254] [Example 7]

[0255] (1) Weigh 57 parts by weight of dry PPB-M100-GH, 3 parts by weight of BONDYRAM 1001, 0.5 parts by weight of XHY-501, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1 part by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 minutes to obtain a first component melt, keep the vacuum degree of the equipment vacuum system above -0.08 MPa, and feed it into a first impregnation mold.

[0256] (2) The continuous basalt fiber enters the first impregnation mold under the action of the traction machine, where it is infiltrated and dispersed with the first component melt to form a material strip, which is used as the inner layer material.

[0257] (3) Weigh 97 parts by weight of dry PPB-M100-GH, 3 parts by weight of BONDYRAM 1001, 0.5 parts by weight of XHY-501, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1 part by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0258] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0259] (5) adjusting the coating amount of the outer layer material by adjusting the extrusion rate of the extruder for the outer layer material and the diameter of the die outlet of the die, so that the coating is carried out according to the amount specified in step (3), and adjusting the cutting speed of the pelletizer so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 12 mm. In the composite material, the continuous basalt fiber accounts for 40% by weight.

[0260] (6) The basalt fiber reinforced PP composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0261] [Example 8]

[0262] (1) Weigh 57 parts by weight of dry PA6-BL3200H, 3 parts by weight of BONDYRAM 1001, 0.5 parts by weight of NDZ12, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1 part by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min to obtain a first component melt, keep the vacuum degree of the equipment vacuum system above -0.08 MPa, and feed it into a first impregnation mold.

[0263] (2) The continuous carbon fiber enters the first impregnation mold under the action of the traction machine, where it is infiltrated and dispersed with the first component melt to form a material strip, which is used as the inner layer material.

[0264] (3) Weigh 97 parts of dry PA6-BL3200H, 3 parts by weight of BONDYRAM 1001, 0.5 parts by weight of NDZ12, 0.1 parts by weight of antioxidant 1010, 1 part by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0265] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0266] (5) adjusting the coating amount of the outer layer material by adjusting the extrusion rate of the extruder for the outer layer material and the diameter of the die outlet of the die, so that the coating is carried out according to the amount specified in step (3), and adjusting the cutting speed of the pelletizer so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 12 mm. In the composite material, the continuous carbon fiber accounts for 40% by weight.

[0267] (6) The long carbon fiber reinforced PA6 composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0268] [Example 9]

[0269] The preparation process is the same as that of Example 1, except that 70 parts by weight of PPB-M100-GH are weighed in step (1), and 85 parts by weight of PPH-Y450 are weighed in step (3). The prepared composite material is subjected to performance tests, and the test results are shown in Table 1. In the composite material, the glass fiber SE4805 accounts for 15.4% by weight.

[0270] [Example 10]

[0271] The preparation process is the same as that of Example 1, except that: in step (1), 45 parts by weight of PPB-M100-GH, 2.5 parts by weight of BONDYRAM 1001, 0.08 parts by weight of antioxidant 1010, and 0.4 parts by weight of XH-201 are weighed, and in step (3), 65 parts by weight of PPH-Y450 are weighed. The prepared composite material is subjected to performance tests, and the test results are shown in Table 1. In the composite material, glass fiber SE4805 accounts for 20% by weight.

[0272] [Example 11]

[0273] The preparation process is the same as that of Example 1, except that: in step (1), 25 parts by weight of PPB-M100-GH, 1.5 parts by weight of BONDYRAM 1001, 0.05 parts by weight of antioxidant 1010, and 0.25 parts by weight of XH-201 are weighed, and in step (3), 45 parts by weight of PPH-Y450 are weighed. The prepared composite material is subjected to performance tests, and the test results are shown in Table 1. In the composite material, glass fiber SE4805 accounts for 27.3% by weight.

[0274] [Example 12]

[0275] The preparation process is the same as that of Example 1, except that: 55 parts by weight of PPB-M100-GH are weighed in step (1), and 70 parts by weight of PPH-Y450 are weighed in step (3). The prepared composite material is subjected to performance tests, and the test results are shown in Table 1. In the composite material, the glass fiber SE4805 accounts for 18.2% by weight.

[0276] [Example 13]

[0277] (1) Weigh 50 parts by weight of dry PPB-M100-GH polypropylene resin (melt flow rate of 100 g / 10 min), 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 1.75 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min to obtain a first component melt, keep the vacuum degree of the equipment vacuum system above -0.08 MPa, and feed them into a first impregnation mold.

[0278] (2) 30 parts by weight of glass fiber SE4805 enters the first impregnation mold under the action of a traction machine, where it is infiltrated and dispersed with the first component melt to form a material strip, which is used as the inner layer material.

[0279] (3) Weigh 49 parts by weight of dry M60RHC polypropylene resin (melt flow rate: 60 g / 10 min), 20 parts by weight of short glass fibers cut from glass fiber SE4805 with a length of 3 mm, 2.5 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, 0.1 parts by weight of antioxidant 168, 0.51 parts by weight of BYK-P4200, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, use them as the outer layer material, and feed them into a twin-screw extruder connected to a molding die, keeping the vacuum degree of the vacuum system of the equipment above -0.08 MPa, to obtain a second component melt.

[0280] (4) The inner layer material enters the molding die under the action of the traction machine, is guided through the hole in the middle of the core, and is formed in the cavity formed by the core and the outer shell, which is filled with the second component melt, to achieve the molding of the composite structure of the inner and outer layer materials, and is finally discharged through the mold outlet.

[0281] (5) The coating amount of the outer layer material is adjusted by adjusting the extrusion rate of the extruder for the outer layer material and the diameter of the die outlet, so that the coating is carried out according to the amount specified in step (3), and the cutting speed of the pelletizer is adjusted so that the pelletizing length of the prepared thermoplastic composite material with low volatile organic compound content is controlled to be 6.1 mm. In the composite material, the glass fiber SE4805 accounts for 32% by weight.

[0282] (6) The polypropylene composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0283] [Comparative Example 1]

[0284] (1) Weigh 57 parts by weight of dry PPB-M100-GH, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 minutes to obtain a melt, which is then fed into a dipping mold.

[0285] (2) SE4805 enters the impregnation mold under the action of the traction machine, where it is infiltrated and dispersed with the melt. The content of SE4805 in the composite material is adjusted by selecting the size of the impregnation mold molding die (6 mm) to control the content of SE4805 to 22% by weight. The cutter speed of the pelletizer is adjusted to control the pelletizing length of the prepared polypropylene composite material to 12 mm.

[0286] (3) The polypropylene composite material prepared by the above method was injection molded into a standard specimen and the performance was tested. The test results are shown in Table 1.

[0287] [Comparative Example 2]

[0288] (1) Weigh 50 parts by weight of dry PPB-M100-GH polypropylene resin (melt flow rate of 100 g / 10 min), 30 parts by weight of short glass fibers cut from glass fiber SE4805 with a length of 3 mm, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201, and stir them in a high-speed mixer at 50° C. for 3 min to obtain the inner layer resin;

[0289] (2) Weigh 49 parts by weight of dry M60RHC polypropylene resin (melt flow rate: 60 g / 10 min), 20 parts by weight of short glass fibers cut from glass fiber SE4805 with a length of 3 mm, 3 parts by weight of BONDYRAM 1001, 0.1 parts by weight of antioxidant 1010, and 0.5 parts by weight of XH-201, stir them in a high-speed mixer at 50° C. for 3 min, and use them as the outer layer material;

[0290] (3) The inner layer material is added to the No. 1 extruder, and the outer layer material is added to the No. 2 extruder. The two extruders extrude the raw materials at the same time, and extrude through a die head with an inner and outer layer structure to obtain a continuous wire material having an inner layer of a short glass fiber resin layer and an outer layer of a short glass fiber resin layer, and pelletize to obtain a comparative example raw material. The performance test is shown in Table 1.

[0291] Table 1

[0292]

[0293]

[0294] Note: in Table 1, D1 and D2 are Comparative Example 1 and Comparative Example 2, respectively, and S1-S13 are Examples 1-13.

[0295] By comparing Examples 1-5 and Examples 9-13 with Comparative Examples 1-2, it is found that the tensile strength, flexural strength, simply supported beam notched impact strength and surface gloss of the long glass fiber reinforced polypropylene material prepared by the present invention are significantly higher than those of the material prepared in Comparative Example 1, and the surface quality of the product is higher.

[0296] According to Examples 6-8 of the present invention, the preparation method proposed in the present invention is not only applicable to long glass fiber reinforced polypropylene composites, but also applicable to the preparation of continuous glass fiber reinforced PA6, continuous basalt fiber reinforced polypropylene, and continuous carbon fiber reinforced PA6 composites.

[0297] Furthermore, it can be seen from the data in Table 1 that the thermoplastic composite material of the present invention has a low VOC content, and the melt flow rate of the thermoplastic resin of the inner layer material and the outer layer material is selected so that the prepared composite material has an ideal surface gloss.

[0298] The preparation method of the present invention is simple to operate, can realize online continuous production, can ensure higher production capacity and lower energy consumption, and is suitable for industrial production and application.

[0299] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this field, under the technical enlightenment provided by the present invention, as common knowledge in the field, other equivalent variations and improvements can also be made, which should also be regarded as the protection scope of the present invention.

Claims

1. A thermoplastic composite material with a low volatile organic compound content, comprising an inner layer material and at least one outer layer material, wherein the inner layer material is a core layer comprising a fiber bundle, a first thermoplastic resin and a first auxiliary agent, and the at least one outer layer material wraps the core layer and is a resin layer comprising a second thermoplastic resin and a second auxiliary agent, wherein: The fiber bundle extends continuously from one end of the core layer to the opposite end thereof, and the first auxiliary agent and the second auxiliary agent include a stripping agent; On the transverse cross section of the thermoplastic composite material, there are a core layer and a resin layer from the inside to the outside; the first thermoplastic resin and the second thermoplastic resin are of the same type; The first thermoplastic resin has a melt flow rate of 60-8000 g / 10 min at 230° C. and a load of 2.16 kg; The melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 0.1-8000 g / 10 min; The melt flow rate of the first thermoplastic resin is higher than the melt flow rate of the second thermoplastic resin; or, the melt flow rate of the second thermoplastic resin is higher than the melt flow rate of the first thermoplastic resin; In the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight; the amount of the fiber bundle is 10-110 parts by weight; In the outer layer material, the amount of the second thermoplastic resin is 1-110 parts by weight.

2. The thermoplastic composite material with low volatile organic compound content according to claim 1, characterized in that: The thermoplastic composite material with low volatile organic compound content is in the form of strips, rods or particles.

3. The thermoplastic composite material with low volatile organic compound content according to claim 2, characterized in that: The length of the strip-shaped, rod-shaped or granular thermoplastic composite material resistant to heat and oxygen aging is 5-30 mm.

4. The thermoplastic composite material with low volatile organic compound content according to claim 3, characterized in that: The length of the strip-shaped, rod-shaped or granular thermoplastic composite material resistant to heat and oxygen aging is 5-25 mm.

5. The thermoplastic composite material with low volatile organic compound content according to claim 4, characterized in that: The length of the strip-shaped, rod-shaped or granular thermoplastic composite material resistant to heat and oxygen aging is 6-15 mm.

6. The thermoplastic composite material with low volatile organic compound content according to claim 1, characterized in that: In the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.25-6:

1.

7. The thermoplastic composite material with low volatile organic compound content according to claim 6, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-70 parts by weight; and / or, In the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.35-4.5:1; and / or, in the outer layer material, the amount of the second thermoplastic resin is 10-99 parts by weight.

8. The thermoplastic composite material with low volatile organic compound content according to claim 7, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-55 parts by weight; and / or, In the inner layer material, the weight ratio of the fiber bundle to the first thermoplastic resin is 0.43-4.5:1; and / or, in the outer layer material, the amount of the second thermoplastic resin is 40-90 parts by weight.

9. The thermoplastic composite material with low volatile organic compound content according to claim 8, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 24-45 parts by weight.

10. The thermoplastic composite material with low volatile organic compound content according to claim 6, characterized in that: The amount of the fiber bundle is 20-110 parts by weight.

11. The thermoplastic composite material with low volatile organic compound content according to claim 10, characterized in that: The amount of the fiber bundle is 25-110 parts by weight.

12. The thermoplastic composite material with low volatile organic compound content according to claim 6, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 1-90 parts by weight; and / or the amount of the fiber bundle is 10-99 parts by weight, or, In the inner layer material, the amount of the first thermoplastic resin is 50-70 parts by weight; and / or, the amount of the fiber bundle is 90-110 parts by weight; and / or, in the outer layer material, the amount of the second thermoplastic resin is 90-110 parts by weight.

13. The thermoplastic composite material with low volatile organic compound content according to claim 12, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-70 parts by weight; and / or, the amount of the fiber bundle is 20-80 parts by weight, or, In the inner layer material, the amount of the first thermoplastic resin is 50-60 parts by weight; and / or, the amount of the fiber bundle is 100-110 parts by weight; and / or, in the outer layer material, the amount of the second thermoplastic resin is 95-105 parts by weight.

14. The thermoplastic composite material with low volatile organic compound content according to claim 13, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 20-55 parts by weight; and / or the amount of the fiber bundle is 25-50 parts by weight.

15. The thermoplastic composite material with low volatile organic compound content according to claim 14, characterized in that: In the inner layer material, the amount of the first thermoplastic resin is 24-45 parts by weight.

16. The thermoplastic composite material with low volatile organic compound content according to any one of claims 1 to 15, characterized in that The inner layer material does not contain non-oriented short fibers.

17. The thermoplastic composite material with low volatile organic compound content according to claim 16, characterized in that The inner layer material consists of a fiber bundle, a first thermoplastic resin and a first auxiliary agent.

18. The thermoplastic composite material with low volatile organic compound content according to any one of claims 1 to 15, characterized in that The outer layer material does not contain fibers; or the outer layer material contains fibers.

19. The thermoplastic composite material with low volatile organic compound content according to claim 18, characterized in that The outer layer material is composed of a second thermoplastic resin and a second auxiliary agent; or, the outer layer material contains short fibers.

20. The thermoplastic composite material with low volatile organic compound content according to claim 19, characterized in that In the outer layer material, the weight ratio of the fiber to the second thermoplastic resin is 1-50:

100.

21. The thermoplastic composite material with low volatile organic compound content according to claim 20, characterized in that In the outer layer material, the weight ratio of the fiber to the second thermoplastic resin is 5-50:

100.

22. The low volatile organic compound content thermoplastic composite material according to claim 21, characterized in that In the outer layer material, the weight ratio of the fiber to the second thermoplastic resin is 20-45:

100.

23. The low volatile organic compound content thermoplastic composite material according to claim 1, characterized in that: The first thermoplastic resin and the second thermoplastic resin are selected from at least one of polypropylene, polyethylene, polystyrene, polyvinyl chloride, polyacrylonitrile-butadiene-styrene copolymer, polyacrylonitrile-styrene copolymer, polyoxymethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polymethyl methacrylate and alloy polymers thereof; and / or, The fiber bundle is selected from at least one of carbon fiber, stainless steel fiber, synthetic resin fiber and mineral fiber.

24. The low volatile organic compound content thermoplastic composite material according to claim 23, characterized in that: The first thermoplastic resin and the second thermoplastic resin are selected from polypropylene, polyethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate; and / or, The fiber bundle is selected from at least one of glass fiber, basalt fiber and aromatic polyamide fiber.

25. The low volatile organic compound content thermoplastic composite material according to claim 24, characterized in that The first thermoplastic resin and the second thermoplastic resin are at least one selected from homopolypropylene, copolymer polypropylene, a mixture of homopolypropylene and copolymer polypropylene, nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66.

26. The low volatile organic compound content thermoplastic composite material according to claim 1, characterized in that: The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 100-8000 g / 10 min; the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 3-55 g / 10 min or 450-8000 g / 10 min.

27. The low volatile organic compound content thermoplastic composite material according to claim 26, characterized in that The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 1000-7500 g / 10 min or the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 3-45 g / 10 min.

28. The low volatile organic compound content thermoplastic composite material according to claim 27, characterized in that The first thermoplastic resin has a melt flow rate of 1900-7500 g / 10 min at 230° C. and a load of 2.16 kg.

29. The low volatile organic compound content thermoplastic composite material according to claim 26, characterized in that: The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 60-450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 3-55 g / 10 min or 450-8000 g / 10 min.

30. The low volatile organic compound content thermoplastic composite material according to claim 29, characterized in that The first thermoplastic resin has a melt flow rate of 60-200 g / 10 min at 230° C. and a load of 2.16 kg.

31. The low volatile organic compound content thermoplastic composite material according to claim 30, characterized in that The melt flow rate of the first thermoplastic resin at 230° C. and a load of 2.16 kg is 60-450 g / 10 min, and the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 800-8000 g / 10 min; or The melt flow rate of the first thermoplastic resin at 230°C and a load of 2.16 kg is above 450 g / 10 min; the melt flow rate of the second thermoplastic resin at 230°C and a load of 2.16 kg is less than 100 g / 10 min; and / or the weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.05-12.5:

1.

32. The low volatile organic compound content thermoplastic composite material according to claim 31, characterized in that The first thermoplastic resin has a melt flow rate greater than 450 g / 10 min at 230° C. and a load of 2.16 kg.

33. The low volatile organic compound content thermoplastic composite material according to claim 32, characterized in that The second thermoplastic resin has a melt flow rate of 1.5-55 g / 10 min at 230° C. and a load of 2.16 kg.

34. The low volatile organic compound content thermoplastic composite material according to claim 33, characterized in that The second thermoplastic resin has a melt flow rate of 3-50 g / 10 min at 230° C. and a load of 2.16 kg.

35. The low volatile organic compound content thermoplastic composite material according to claim 34, characterized in that The weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.1-4:

1.

36. The low volatile organic compound content thermoplastic composite material according to claim 35, characterized in that The weight ratio of the second thermoplastic resin to the first thermoplastic resin is 0.14-3.5:

1.

37. The low volatile organic compound content thermoplastic composite material of claim 26, wherein: When the melt flow rate of the second thermoplastic resin at 230° C. and a load of 2.16 kg is 800 to 8000 g / 10 min, the weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.25:1; and / or, When the first thermoplastic resin and the second thermoplastic resin are selected from at least one of nylon 6, nylon 66, and a mixture of nylon 6 and nylon 66, the viscosity of nylon 6 and nylon 66 is 1.8-3.

5.

38. The low volatile organic compound content thermoplastic composite material according to claim 37, characterized in that The weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.18:

1.

39. The low volatile organic compound content thermoplastic composite material according to claim 38, characterized in that The weight ratio of the second thermoplastic resin to the first thermoplastic resin is less than 0.15:

1.

40. The low volatile organic compound content thermoplastic composite material of claim 1, wherein: Based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the amount of the stripping agent is independently 0.5-4 parts by weight; And / or, the stripping agent comprises a foaming polymer carrier and a stripping aid loaded thereon; the stripping aid is selected from one or more of water, ethanol, propanol and isopropanol; and / or, based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the first auxiliary agent and the second auxiliary agent each independently include at least one of 0.5-15 parts by weight of a compatibilizer, 0.05-3 parts by weight of an antioxidant, and 0.05-2.5 parts by weight of a lubricant; and / or, The compatibilizer is selected from at least one of the polar monomer graft-modified polymers; and / or, The antioxidant is at least one selected from tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, tris[2,4-di-tert-butylphenyl]phosphite, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane and bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite; and / or, The lubricant is selected from at least one of ethylene bisstearamide, calcium stearate, polyethylene wax, pentaerythritol stearate, silicone, polyethylene glycol and fluorine-containing resin; and / or, The first auxiliary agent further comprises at least one of a lubricant, an antistatic agent and a plasticizer; and / or, The second auxiliary agent also includes at least one of a lubricant, an antistatic agent, a plasticizer, a nucleating agent, a light stabilizer, a flame retardant, a heat stabilizer, a masterbatch and a filler.

41. The low volatile organic compound content thermoplastic composite material according to claim 40, characterized in that Based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the amount of the stripping agent is independently 1-4 parts by weight; and / or, based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the first auxiliary agent and the second auxiliary agent each independently include 1-15 parts by weight of a compatibilizer, 0.1-1 parts by weight of an antioxidant and 0.5-2.5 parts by weight of a lubricant; and / or, The polar monomer is selected from at least one of maleic anhydride, maleic anhydride derivatives, acrylic acid and acrylate derivatives; and / or the polymer is selected from at least one of polyethylene, polypropylene, ethylene-α-octene copolymer and propylene-α-olefin copolymer.

42. The low volatile organic compound content thermoplastic composite material according to claim 41, characterized in that Based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the amount of the stripping agent is independently 1-3.5 parts by weight; And / or, the first auxiliary agent and the second auxiliary agent each independently include at least one of 1-6 parts by weight of a compatibilizer, 0.1-0.5 parts by weight of an antioxidant and 0.5-2.5 parts by weight of a lubricant.

43. The low volatile organic compound content thermoplastic composite material according to claim 42, characterized in that Based on 100 parts by weight of the first thermoplastic resin and the second thermoplastic resin, the amount of the stripping agent is independently 1-3 parts by weight; And / or, the first auxiliary agent and the second auxiliary agent each independently include at least one of 3-6 parts by weight of a compatibilizer, 0.1-0.5 parts by weight of an antioxidant and 0.5-2.5 parts by weight of a lubricant.

44. The method for preparing a thermoplastic composite material with low volatile organic compound content according to any one of claims 1 to 43, characterized in that: The method comprises the following steps: Step A, a first thermoplastic resin and a first auxiliary agent are mixed and then melted to obtain a first component melt; wherein the vacuum degree during melting is above -0.05 MPa; Step B, performing a first impregnation treatment on the continuous fiber bundle and the first component melt to form a filamentous core layer product; Step C, the second thermoplastic resin and the second auxiliary agent are mixed and melted to obtain a second component melt; wherein the vacuum degree during melting is above -0.05 MPa; Step D: subjecting the filamentous core layer product to a second impregnation treatment with the second component melt to form a resin layer wrapping the core layer.

45. The preparation method according to claim 44, characterized in that: The mixing conditions of step A include: temperature of 40-60°C, time of 0.5-20 min; melting temperature of step A of 200-380°C; and / or, The vacuum degree during melting in step A is above -0.08 MPa; and / or, The vacuum degree during melting in step C is above -0.08 MPa; and / or, The mixing conditions of step C include: temperature of 40-60° C., time of 0.5-20 min; and melting temperature of step C of 200-380° C.

46. ​​The preparation method according to claim 45, characterized in that The mixing conditions of step A include: the time is 1-10 min; and / or, the mixing conditions of step C include: the time is 1-10 min.

47. The preparation method according to claim 46, characterized in that The mixing conditions of step A include: the mixing time is 3-5 min; and / or, the mixing conditions of step C include: the mixing time is 3-5 min.

48. The preparation method according to any one of claims 44 to 47, characterized in that: In step B, the first impregnation treatment is carried out in a first impregnation mold, which is an adjustable impregnation mold. The first impregnation mold includes a fiber inlet, a fiber outlet and a melt flow channel, and at least one first guide roller is arranged in the mold cavity of the first impregnation mold; the first guide roller can move between the fiber inlet and the fiber outlet; and / or the first guide roller can move in a direction perpendicular to the line connecting the fiber inlet and the fiber outlet.

49. The preparation method according to any one of claims 44 to 47, characterized in that: In step B, the first impregnation treatment is carried out in a second impregnation mold, and the second impregnation mold is a combined impregnation mold, which includes a first module, an intermediate module and a second module connected in sequence, the first module is provided with a fiber inlet and a first module flow channel, the second module is provided with a fiber outlet and a second module flow channel, and the intermediate module is provided with an intermediate module flow channel; after the first module, the intermediate module and the second module are connected in sequence, the first module flow channel, the intermediate module flow channel and the second module flow channel are connected to form a combined flow channel for the fiber to pass through.

50. The preparation method according to any one of claims 44 to 47, characterized in that: In step B, the first impregnation treatment is carried out in a third impregnation mold, and the third impregnation mold is a strong turbulence impregnation mold. The third impregnation mold includes a fiber inlet channel, an impregnation outlet and a melt gap flow channel, and the fiber inlet channel, the impregnation outlet and the melt gap flow channel are all connected to the mold cavity inside the third impregnation mold; wherein a second guide wire roller is arranged in the mold cavity of the third impregnation mold, and the second guide wire roller includes at least one active guide wire roller, and the active guide wire roller is driven to rotate by a driving device.

51. Application of the thermoplastic composite material with low volatile organic compound content as claimed in any one of claims 1 to 43 or the thermoplastic composite material with low volatile organic compound content obtained by the preparation method as claimed in any one of claims 44 to 50 in the fields of automobile industry, machinery manufacturing, electronic appliances, chemical industry and environmental protection, aerospace communication and construction industry.

52. The use according to claim 51, characterized in that The application is application in large automobile parts and / or high-precision electronic and electrical components.