A compressive creep aluminum alloy material and its preparation method and application
By adding specific elements and process to the aluminum alloy material, a high conductivity, heat and creep resistance and creep resistance aluminum alloy material was prepared, which solved the problem of reducing tensile strength and creep of aluminum conductor materials under high temperature conditions, and achieved High performance use at room temperature and high temperatures and reduces production costs.
Patent Information
- Application Number
- CN202310164921.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The tensile strength of existing aluminum conductor materials decreases under high temperature conditions, easily creeps, resulting in increased conductor sag, unable to meet safety requirements, and it is difficult to synergistically improve conductivity and other performance indicators, limiting long-distance and large capacity. Development of transmission lines.
Use compressive creep aluminum alloy materials composed of silicon, magnesium, copper, nickel, manganese, titanium, yttrium, neodymium, zirconium, scandium, strontium, vanadium and other elements, and are smelted, refined, solid solution and aging through specific alloys The treatment process was used to prepare an aluminum alloy material with high conductivity and heat resistance and creep resistance.
While maintaining creep resistance, it reduces the content requirements of scandium elements, improves the tensile strength of the material, meets the long-term use requirements under high temperature conditions, reduces production costs, and is suitable for large-scale production.
Smart Images

Figure GHA0000007508730000061 
Figure GHA0000007508730000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal materials, and in particular to a compressive creep resistant aluminum alloy material and a preparation method and application thereof. Background Art
[0002] There is a serious imbalance between regional electricity demand and electricity resources in my country. It is necessary to transmit electricity resources from rich areas to concentrated electricity load areas through long-distance and large-capacity transmission. However, as the transmission distance increases, the power loss of the transmission line increases. Among the power losses of transmission lines, the power loss caused by conductor resistance accounts for more than 80%. If the conductivity increases by 1% IACS, the average power loss per kilometer of line will be reduced by about 2,000 degrees per year. As the transmission capacity increases, the service temperature of the conductor increases, resulting in a decrease in its tensile strength. At the same time, it will also elongate and creep due to heat, which brings many problems. For example, the sag of the conductor increases significantly, causing the distance between the conductor and the ground or the distance to the crossing object to fail to meet safety requirements.
[0003] my country's UHV and long-distance power transmission technology is in the leading position in the world, but the comprehensive performance level of aluminum conductor materials for overhead transmission lines limits its development. In practical applications, the transmission capacity of the transmission line is usually restricted or the heat resistance requirements are put forward for the conductor material to ensure that the conductor material has sufficient strength residual rate and creep resistance at the service temperature. Therefore, as a conductor material for long-distance, large-capacity, and low-loss transmission lines, it is required not only to have a high conductivity at room temperature, but also to have a high conductivity at the service temperature, and to be heat-resistant and creep-resistant. However, it is difficult for existing technologies to synergistically improve conductivity and other performance indicators. Therefore, the development of high-conductivity, heat-resistant, and creep-resistant aluminum alloy conductor materials is the key to breaking through the bottleneck of further development of my country's power transmission technology.
[0004] Based on the above situation, the present invention proposes a compressive creep resistant aluminum alloy material and a preparation method and application thereof. Summary of the invention
[0005] The purpose of the present invention is to provide a compressive creep resistant aluminum alloy material and a preparation method and application thereof.
[0006] To achieve the above-mentioned purpose, the present invention provides a compressive creep resistant aluminum alloy material, which is prepared from the following raw materials in weight percentage: silicon: 0.15-0.30wt%, magnesium: 0.6-0.8wt%, copper: 0.55-0.75wt%, nickel: 0.2-0.4wt%, manganese: 0.25-0.35wt%, titanium: 0.05-0.08wt%, yttrium: 0.01-0.02wt%, neodymium: 0.05-0.15wt%, zirconium: 0.02-0.06wt%, scandium: 0.02-0.2wt%, and the balance is aluminum.
[0007] Preferably, the aluminum alloy material further includes vanadium: 0.02-0.05wt%.
[0008] Preferably, the aluminum alloy material further includes strontium: 0.03-0.04wt%.
[0009] Preferably, the aluminum alloy material is prepared from the following raw materials in weight percentage: silicon: 0.15-0.30wt%, magnesium: 0.6-0.8wt%, copper: 0.55-0.75wt%, nickel: 0.2-0.4wt%, manganese: 0.25-0.35wt%, titanium: 0.05-0.08wt%, yttrium: 0.01-0.02wt%, neodymium: 0.05-0.15wt%, zirconium: 0.02-0.06wt%, scandium: 0.02-0.04wt%, vanadium: 0.02-0.05wt%, strontium: 0.03-0.04wt%, and the balance is aluminum.
[0010] Preferably, the weight percentage of the vanadium + strontium is 0.06-0.08wt%.
[0011] Preferably, the weight percentage of scandium+vanadium+strontium is ≤0.1%wt%.
[0012] Preferably, the aluminum alloy material is prepared from the following raw materials in weight percentage: silicon: 0.30wt%, magnesium: 0.8wt%, copper: 0.75wt%, nickel: 0.4wt%, manganese: 0.35wt%, titanium: 0.08wt%, yttrium: 0.01wt%, neodymium: 0.15wt%, zirconium: 0.06wt%, scandium: 0.04wt%, vanadium: 0.02wt%, strontium: 0.04wt%, and the balance is aluminum.
[0013] Preferably, the sources of the aluminum, magnesium and neodymium are industrial pure aluminum, pure magnesium ingots and rare earth neodymium, respectively.
[0014] Preferably, the sources of the silicon, copper, nickel, manganese, titanium, yttrium, zirconium, scandium, strontium and vanadium are respectively aluminum-silicon master alloy, aluminum-copper master alloy, aluminum-nickel master alloy, aluminum-manganese master alloy, aluminum-titanium-boron master alloy, aluminum-yttrium master alloy, aluminum-zirconium master alloy, aluminum-scandium master alloy, aluminum-strontium master alloy and aluminum-vanadium master alloy.
[0015] The present invention also provides a method for preparing a compressive creep resistant aluminum alloy material, the preparation method comprising the following steps:
[0016] (1) placing industrial pure aluminum in a graphite crucible preheated to 750-770° C. for melting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in order for melting, and after one alloy raw material is fully melted, adding another alloy raw material, and after all the alloy raw materials are melted, introducing high-purity argon gas with a purity greater than 99.99% to refine the liquid alloy, the refining temperature is 750-770° C., the refining time is 50-60 min, and after the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0017] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0018] (3) subjecting the alloy casting obtained in step (2) to a solution treatment, wherein the heating temperature of the solution treatment is 460 to 480° C., the holding time is 3 to 3.5 hours, and then the alloy casting is rapidly cooled in water at 60 to 65° C., and the cooling time is 16 to 20 seconds;
[0019] (4) subjecting the alloy casting obtained in step (3) to aging treatment at a temperature of 140 to 150° C. for a holding time of 15 to 16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention can significantly reduce the content requirement of scandium in the aluminum alloy material while maintaining the creep resistance of the aluminum alloy material by adding a small amount of strontium alloy and vanadium alloy, thereby avoiding the dependence on high content requirements of a single precious metal; at the same time, the combination of strontium alloy and vanadium alloy can improve the room temperature tensile strength and high temperature tensile strength of the overall alloy material, so that the present invention application can meet the requirements of long-term use under room temperature and high temperature conditions.
[0022] 2. The raw materials of the present invention are sufficient in China and are of suitable price, so that there is no high cost restriction for large-scale production; at the same time, the preparation method is simple and the overall production cost is not high, which is conducive to large-scale industrial production. DETAILED DESCRIPTION
[0023] Example 1
[0024] Weigh the specific raw materials according to Table 1, and the specific preparation steps are as follows:
[0025] (1) placing industrial pure aluminum in a graphite crucible preheated to 750° C. for smelting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in the order of melting, and adding another alloy raw material after one alloy raw material is fully melted. After all the alloy raw materials are melted, high-purity argon gas with a purity greater than 99.99% is introduced to refine the liquid alloy. The refining temperature is 750° C. and the refining time is 60 min. After the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0026] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0027] (3) subjecting the alloy casting obtained in step (2) to a solution treatment at a heating temperature of 460° C. for a holding time of 3.5 h, and then rapidly cooling the alloy casting in water at 60° C. for a cooling time of 20 s;
[0028] (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 140° C. and a holding time of 16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0029] Example 2
[0030] Weigh the specific raw materials according to Table 1, and the specific preparation steps are as follows:
[0031] (1) placing industrial pure aluminum in a graphite crucible preheated to 770° C. for smelting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in the order of melting, and adding another alloy raw material after one alloy raw material is fully melted. After all the alloy raw materials are melted, high-purity argon gas with a purity greater than 99.99% is introduced to refine the liquid alloy. The refining temperature is 770° C. and the refining time is 50 min. After the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0032] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0033] (3) subjecting the alloy casting obtained in step (2) to a solution treatment at a heating temperature of 480° C. for a holding time of 3 h, and then rapidly cooling the alloy casting in water at 65° C. for a cooling time of 16 s;
[0034] (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 150° C. and a holding time of 15 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0035] Example 3
[0036] Weigh the specific raw materials according to Table 1, and the specific preparation steps are as follows:
[0037] (1) placing industrial pure aluminum in a graphite crucible preheated to 770° C. for smelting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in the order of melting, and adding another alloy raw material after one alloy raw material is fully melted. After all the alloy raw materials are melted, high-purity argon gas with a purity greater than 99.99% is introduced to refine the liquid alloy. The refining temperature is 770° C. and the refining time is 60 min. After the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0038] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0039] (3) subjecting the alloy casting obtained in step (2) to a solution treatment at a heating temperature of 480° C. for a holding time of 3.5 h, and then rapidly cooling the alloy casting in water at 65° C. for a cooling time of 20 s;
[0040] (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 150° C. and a holding time of 16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0041] Comparative Example 1
[0042] Specific raw materials were weighed according to Table 1. The difference from Example 3 was that no aluminum-vanadium master alloy and aluminum-strontium master alloy were added, and the content of scandium was 0.2wt%. The remaining preparation steps were the same as those in Example 3, as follows:
[0043] (1) placing industrial pure aluminum in a graphite crucible preheated to 770° C. for smelting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in the order of melting, and adding another alloy raw material after one alloy raw material is fully melted. After all the alloy raw materials are melted, high-purity argon gas with a purity greater than 99.99% is introduced to refine the liquid alloy. The refining temperature is 770° C. and the refining time is 60 min. After the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0044] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0045] (3) subjecting the alloy casting obtained in step (2) to a solution treatment at a heating temperature of 480° C. for a holding time of 3.5 h, and then rapidly cooling the alloy casting in water at 65° C. for a cooling time of 20 s;
[0046] (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 150° C. and a holding time of 16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0047] Comparative Example 2
[0048] Specific raw materials were weighed according to Table 1. The difference from Example 3 was that no aluminum-vanadium master alloy was added, and the content of strontium was 0.06wt%. The remaining preparation steps were the same as those of Example 3, as follows:
[0049] (1) placing industrial pure aluminum in a graphite crucible preheated to 770° C. for smelting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in the order of melting, and adding another alloy raw material after one alloy raw material is fully melted. After all the alloy raw materials are melted, high-purity argon gas with a purity greater than 99.99% is introduced to refine the liquid alloy. The refining temperature is 770° C. and the refining time is 60 min. After the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0050] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0051] (3) subjecting the alloy casting obtained in step (2) to a solution treatment at a heating temperature of 480° C. for a holding time of 3.5 h, and then rapidly cooling the alloy casting in water at 65° C. for a cooling time of 20 s;
[0052] (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 150° C. and a holding time of 16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0053] Comparative Example 3
[0054] The specific raw materials were weighed according to Table 1. The difference from Example 3 was that no aluminum-strontium master alloy was added, and the vanadium content was 0.06wt%. The remaining preparation steps were the same as Example 3, as follows:
[0055] (1) placing industrial pure aluminum in a graphite crucible preheated to 770° C. for smelting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in the order of melting, and adding another alloy raw material after one alloy raw material is fully melted. After all the alloy raw materials are melted, high-purity argon gas with a purity greater than 99.99% is introduced to refine the liquid alloy. The refining temperature is 770° C. and the refining time is 60 min. After the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0056] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0057] (3) subjecting the alloy casting obtained in step (2) to a solution treatment at a heating temperature of 480° C. for a holding time of 3.5 h, and then rapidly cooling the alloy casting in water at 65° C. for a cooling time of 20 s;
[0058] (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 150° C. and a holding time of 16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0059] Comparative Example 4
[0060] Specific raw materials were weighed according to Table 1. The difference from Example 3 was that no aluminum-scandium master alloy was added. The remaining preparation steps were the same as Example 3, specifically as follows:
[0061] (1) placing industrial pure aluminum in a graphite crucible preheated to 770° C. for smelting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and master alloy into the graphite crucible in the order of melting, and adding another alloy raw material after one alloy raw material is fully melted. After all the alloy raw materials are melted, high-purity argon gas with a purity greater than 99.99% is introduced to refine the liquid alloy. The refining temperature is 770° C. and the refining time is 60 min. After the refining is completed, the alloy is fully stirred and slag is removed to obtain an alloy melt;
[0062] (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5° C., casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting;
[0063] (3) subjecting the alloy casting obtained in step (2) to a solution treatment at a heating temperature of 480° C. for a holding time of 3.5 h, and then rapidly cooling the alloy casting in water at 65° C. for a cooling time of 20 s;
[0064] (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 150° C. and a holding time of 16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
[0065] Table 1
[0066]
[0067] Aluminum alloy material performance evaluation
[0068] The aluminum alloy materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used to prepare rods with a diameter of 10 mm, and room temperature tensile tests were performed according to GB / T228.1-2010; high temperature tensile tests were performed according to GB / T228.2-2015; creep coefficient tests were performed according to GB / T2039-2012; and electrical conductivity tests were performed according to GB / T 12966-2008. The test results are shown in Table 2.
[0069] Table 2
[0070]
[0071] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A compressive creep aluminum alloy material, characterized in that: The aluminum alloy material is prepared from the following raw materials in weight percentage: silicon: 0.30 wt%, magnesium: 0.8 wt%, copper: 0.75 wt%, nickel: 0.4 wt%, manganese: 0.35 wt%, titanium: 0.08 wt%, yttrium: 0.01 wt%, neodymium: 0.15 wt%, zirconium: 0.06 wt%, scandium: 0.04 wt%, vanadium: 0.02 wt%, strontium: 0.04 wt%, the remainder being aluminum; the preparation method of the aluminum alloy material comprises the following steps: (1) placing industrial pure aluminum in a graphite crucible preheated to 750-770°C for melting, and after the pure aluminum ingot is fully melted, adding pure magnesium ingot, rare earth neodymium, and intermediate alloy into the graphite crucible in the order of melting, and after one alloy raw material is fully melted, adding another alloy raw material, and after all the alloy raw materials are melted, introducing high-purity argon gas with a purity greater than 99.99% to refine the liquid alloy, the refining temperature is 750-770°C, the refining time is 50-60 min, and after the refining is completed, fully stirring and slag removal is performed to obtain an alloy melt; (2) lowering the temperature of the alloy melt obtained in step (1) to 730±5°C, casting the alloy melt into a metal mold whose inner wall is sprayed with a boron nitride (BN) release agent, and after the mold is cooled, obtaining an alloy casting; (3) subjecting the alloy casting obtained in step (2) to a solution treatment, wherein the heating temperature of the solution treatment is 460-480°C, the holding time is 3-3.5 h, and then the alloy casting is rapidly cooled in water at 60-65°C for 16-20 s; (4) The alloy casting obtained in step (3) is subjected to aging treatment at a temperature of 140-150° C. and a holding time of 15-16 h. After the aging treatment, a compressive creep aluminum alloy material is obtained.
2. The compressive creep resistant aluminum alloy material according to claim 1, characterized in that: The sources of the aluminum, magnesium and neodymium are industrial pure aluminum, pure magnesium ingot and rare earth neodymium respectively.
3. The compressive creep resistant aluminum alloy material according to claim 1, characterized in that: The sources of the silicon, copper, nickel, manganese, titanium, yttrium, zirconium, scandium, strontium and vanadium are respectively aluminum-silicon master alloy, aluminum-copper master alloy, aluminum-nickel master alloy, aluminum-manganese master alloy, aluminum-titanium-boron master alloy, aluminum-yttrium master alloy, aluminum-zirconium master alloy, aluminum-scandium master alloy, aluminum-strontium master alloy and aluminum-vanadium master alloy.