A water-based environmentally friendly solar cell welding silver paste and preparation method thereof
By using water as a solvent in solar cell welding silver paste, combined with silver powder, glass powder and water-soluble resin, the problem of organic solvent emission pollution in traditional welding silver paste is solved, and high-performance, low-cost environmentally friendly water properties are achieved The preparation of silver paste has broad market prospects.
Patent Information
- Application Number
- CN202211315154.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-10-26
AI Technical Summary
The problem of organic emission pollution caused by the use of organic solvents in the preparation method of traditional solar cell welding silver paste has not been effectively solved.
The silver paste is welded by water-based environmentally friendly solar cells, composed of silver powder, glass powder, water-soluble resin, thixotropic agent and surfactant, and deionized water is used as solvent. The particle size and density of silver powder and glass powder are evenly distributed, through Three rollers grinding and mixing and adhesively preparing high-performance aqueous silver paste.
It realizes the use of water as a solvent, reduces the volatility of organic solvents, reduces environmental pollution, and meets the performance requirements of crystalline silicon solar cell welding silver paste, providing a new green and environmentally friendly conductive paste.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application belongs to the field of chemical technology, and specifically relates to an aqueous environment-friendly solar cell welding silver paste and a preparation method thereof. Background Art
[0002] In the industrial production of solar cells, soldering silver paste is one of the indispensable electrode metallization materials. Soldering silver paste is generally composed of silver powder, glass powder, organic resin, organic solvent and additives, among which the weight of organic solvent in the paste accounts for 30-50%. During the use of paste printing, drying and sintering, the organic solvent is completely volatilized and discharged into the air, which will cause air pollution.
[0003] Patent CN 105551568 A discloses a water-based environmentally friendly and efficient conductive silver paste for crystalline silicon solar cells and its preparation method. However, from the perspective of the paste composition, the silver paste contains 1-6% of an environmentally friendly solvent, and does not use water as a solvent. Patent CN 104036844 A discloses an environmentally friendly water-soluble solar cell positive electrode silver paste and its preparation method. The silver paste contains 1-15% propylene glycol, and does not use water alone as a solvent, which also produces organic emissions. Summary of the invention
[0004] The present application provides an aqueous environment-friendly solar cell soldering silver paste and a preparation method thereof, so as to solve the technical problem of generating organic emissions in the traditional preparation method.
[0005] To solve the above technical problems, a technical solution adopted in the present application is: comprising the following components and their mass percentages: 45-65% silver powder; 2-5% glass powder; 2-5% water-soluble resin; 0.5-5% thixotropic agent; 30-50% deionized water; and 0.1-1.5% surfactant.
[0006] Furthermore, the particle size of the silver powder is 0.1-1.5 μm, and the tap density of the silver powder is 2.5-4.5 g / cm 3 .
[0007] Furthermore, the glass powder is metallic glass, and the particle size of the glass powder is 0.2-2.0 μm.
[0008] Furthermore, the water-soluble resin is one or more of hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose and hydroxypropyl methyl cellulose.
[0009] Furthermore, the thixotropic agent is one or more of water-based polyethylene wax and water-based polyamide wax.
[0010] Furthermore, the surfactant is one or more of sodium alkyl sulfonate, sodium fatty alcohol ether sulfate, alkyl phosphate, and fatty acid salt.
[0011] Another technical solution adopted in the present application is: a method for preparing an aqueous environmentally friendly solar cell soldering silver paste, comprising the following steps:
[0012] The surfactant, thixotropic agent, deionized water and adhesive are mixed in proportion, stirred evenly, and then glass powder and silver powder are added, and then stirred sufficiently to make the glass powder and silver powder dispersed evenly to obtain the initial silver paste; the initial silver paste is three-roll ground for 3-5 times, and then stirred and adjusted to obtain the water-based environmentally friendly solar cell welding silver paste.
[0013] Furthermore, the preparation method of the adhesive comprises:
[0014] The resin powder is added into deionized water, stirred at room temperature until the resin is completely dissolved in the water, and passed through a 400-mesh sieve to obtain the adhesive.
[0015] Furthermore, the method for preparing the glass powder comprises the following steps:
[0016] A plurality of metal oxides are mixed, stirred evenly and placed in a plain quartz crucible, melted at a high temperature of 1000-1200°C and kept warm for 30-60min to obtain a glass liquid; the glass liquid is quenched with deionized water to obtain a glass crystal state, the glass crystal state is dried and crushed and then wet-ball milled, and stearic acid or stearate is added as a surface modifier during the ball milling process to modify the surface of the glass powder to obtain the glass powder.
[0017] The beneficial effects of the present application are as follows: the present application uses water as a solvent alone to replace the organic solvent in the traditional preparation method, thereby reducing the volatilization of the solvent, reducing environmental pollution while meeting the performance requirements of the crystalline silicon solar cell welding silver paste. It is a new type of green and environmentally friendly conductive paste with broad market prospects. DETAILED DESCRIPTION
[0018] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0019] The present application provides an aqueous environment-friendly solar cell soldering silver paste, wherein the components and weight percentages are: silver powder 45-65%; glass powder 2-5%; water-soluble resin 2-5%; thixotropic agent 0.5-5%; deionized water 30-50%; surfactant 0.1-1.5%.
[0020] The particle size of the silver powder is 0.1-1.5 μm, and the tap density of the silver powder is 2.5-4.5 g / cm 3 One or more of .
[0021] The glass powder is metallic glass, and the particle size of the glass powder is 0.2-2.0 μm. The glass powder is a glass system containing copper-manganese-bismuth or copper-manganese-lead.
[0022] The water-soluble resin is one or more of hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose and hydroxypropyl methyl cellulose. The resin plays a film-forming role in the slurry. The reason for selecting such resins is that they have good solubility in water, strong film-forming ability, low carbon residue during high-temperature sintering, and little effect on the conductivity and welding performance of the silver paste.
[0023] The thixotropic agent is one or more of water-based polyethylene wax and water-based polyamide wax.
[0024] The surfactant is one or more of sodium alkyl sulfonate, sodium fatty alcohol ether sulfate, alkyl phosphate, and fatty acid salt.
[0025] Example 1
[0026] The present application provides a method for preparing an aqueous environment-friendly solar cell soldering silver paste, comprising the following steps:
[0027] S1. Preparation of adhesive.
[0028] Specifically, according to the above specific proportions, the resin powder is added to deionized water, stirred at room temperature until the resin is completely dissolved in the water, and passed through a 400-mesh sieve to obtain the adhesive.
[0029] S2. Prepare glass powder.
[0030] Specifically, a plurality of metal oxides and other compounds are mixed, stirred evenly, placed in a plain quartz crucible, melted at a high temperature of 1000-1200° C. and kept warm for 30-60 min to obtain glass liquid.
[0031] Subsequently, the glass liquid is quenched with deionized water to obtain a glass crystal state. The glass crystal state is dried and crushed and then wet-ball milled. During the ball milling process, stearic acid or stearate is added as a surface modifier to modify the surface of the glass powder to obtain the glass powder.
[0032] S4. Mix the surfactant, thixotropic agent, deionized water and adhesive according to the above proportions, stir evenly, add glass powder and silver powder, and stir thoroughly to make the glass powder and silver powder evenly dispersed to obtain an initial silver paste.
[0033] S5. The initial silver paste is ground by three rollers for 3-5 times, and then stirred and adjusted to obtain the above-mentioned water-based environmentally friendly solar cell welding silver paste.
[0034] Example 2
[0035] The silver paste formula used in this embodiment is 50% silver powder, 2.5% glass powder, 2.2% water-soluble resin, 1% thixotropic agent, 0.5% surfactant, and 43.8% deionized water. The silver powder particle size is 0.26 μm and the tap density is 2.8 g / cm 3 The glass powder is a glass system containing copper-manganese-bismuth, and the particle size is 0.8 μm; the resin is hydroxymethyl cellulose; the thixotropic agent is water-based polyethylene wax; and the surfactant is sodium alkyl sulfonate.
[0036] The above materials were prepared according to the preparation method of Example 1 to obtain silver paste No. 1.
[0037] Example 3
[0038] The silver paste formula used in this embodiment is 65% silver powder, 4% glass powder, 3% water-soluble resin, 4.5% thixotropic agent, 1.5% surfactant, and 22% deionized water. The silver powder particle size is 0.8 μm and the tap density is 3.8 g / cm 3 The glass powder is a glass system containing copper-manganese-bismuth, and the particle size is 0.8 μm; the resin is hydroxyethyl cellulose; the thixotropic agent is water-based polyamide wax; and the surfactant is sodium fatty alcohol ether sulfate.
[0039] The above materials were prepared according to the preparation method of Example 1 to obtain silver paste No. 2.
[0040] Example 4
[0041] The silver paste formula used in this embodiment is 45% silver powder, 5% glass powder, 4.5% water-soluble resin, 3% thixotropic agent, 1% surfactant, and 41.5% deionized water. The silver powder has a particle size of D50 = 0.15 μm and a tap density of 2.6 g / cm 3 The particle size is 1.1 μm and the tap density is 4.2 g / cm 3 The weight ratio of coarse and fine silver powder is 1:4; the glass powder is a glass system containing copper-manganese-bismuth, and the particle size D50 is 1.6 μm; the resin is hydroxypropyl methylcellulose; the thixotropic agent is water-based polyethylene wax; and the surfactant is sodium alkyl sulfonate.
[0042] The above materials were prepared according to the preparation method of Example 1 to obtain No. 3 silver paste.
[0043] Example 5
[0044] The silver paste formula used in this embodiment is 54% silver powder, 3.6% glass powder, 3.2% water-soluble resin, 1% thixotropic agent, 0.6% surfactant, and 37.6% deionized water. The silver powder has a particle size of 0.2 μm and a tap density of 2.9 g / cm 3 The particle size is 1 μm and the tap density is 4.5 g / cm 3 The weight ratio of coarse and fine silver powder is 2:3; the glass powder is a glass system containing copper-manganese-lead, and the particle size is 0.9 μm; the resin is a mixture of hydroxyethyl cellulose and hydroxypropyl cellulose in a weight ratio of 1:1; the thixotropic agent is water-based polyamide wax; and the surfactant is alkyl phosphate.
[0045] The above materials were prepared according to the preparation method of Example 1 to obtain No. 4 silver paste.
[0046] Example 6
[0047] The silver paste formula used in this embodiment is 59% silver powder, 3% glass powder, 3.6% water-soluble resin, 2.5% thixotropic agent, 0.6% surfactant, and 31.3% deionized water. The silver powder has a particle size of 0.35 μm and a tap density of 3.1 g / cm 3 The particle size is 0.7 μm and the tap density is 4 g / cm 3 The weight ratio of coarse and fine silver powder is 3:2. The glass powder is a glass system containing copper-manganese-lead, and the particle size is 0.6 μm; the resin is a mixture of hydroxymethyl cellulose and hydroxypropyl cellulose in a weight ratio of 2:1; the thixotropic agent is a mixture of water-based polyethylene wax and water-based polyamide wax in a weight ratio of 1:2; and the surfactant is a mixture of fatty acid salts.
[0048] The above materials were prepared according to the preparation method of Example 1 to obtain No. 5 silver paste.
[0049] Comparative Example 1
[0050] The comparative example is a commercially available product of Nantong Tiansheng New Energy Co., Ltd. The model of the product is 203D, and the actual measured solid content of the silver paste is 62.6%.
[0051] The welding tensile test results of the silver paste products of Examples 2-6 and Comparative Example 1 are shown in Table 1, where the peak tensile force of each 2×5 mm PAD point is taken as the welding tensile force. The minimum, maximum and average values in the table are statistically calculated based on the results of 30 PAD points.
[0052] Table 1 Welding tensile test results
[0053]
[0054]
[0055] It can be seen from Table 1 that the silver paste welding strength of Examples 2-6 is greater than that of Comparative Example 1, indicating that this type of welding silver paste has a better welding effect.
[0056] The present application provides a low-cost, high-performance, environmentally friendly water-based solar cell welding silver paste using water alone as a solvent and a preparation method thereof, wherein the water solvent replaces the organic solvent in the traditional preparation method, thereby reducing the volatilization of the solvent and reducing environmental pollution while meeting the performance requirements of the crystalline silicon solar cell welding silver paste. The present application is a new type of green and environmentally friendly conductive paste with broad market prospects.
[0057] The above descriptions are merely embodiments of the present application and are not intended to limit the patent scope of the present application. Any use of the present application specification directly or indirectly in other related technical fields shall be included in the patent protection scope of the present application.
Claims
1. A water-based environmentally friendly solar cell welding silver paste, It is characterized in that The invention comprises the following components and their mass percentages: 45-65% silver powder; 2-5% glass powder; 2-5% water-soluble resin; 0.5-5% thixotropic agent; 30-50% deionized water; 0.1-1.5% surfactant; wherein the glass powder is metallic glass, and the particle size of the glass powder is 0.2-2.0 μm; the water-soluble resin is one or more of hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and hydroxypropyl methyl cellulose; the thixotropic agent is one or more of water-based polyethylene wax or water-based polyamide wax; the surfactant The agent is one or more of sodium alkyl sulfonate, sodium fatty alcohol ether sulfate, alkyl phosphate, and fatty acid salt; the glass powder is obtained by mixing the metal oxides, stirring them evenly, placing them in a plain quartz crucible, melting them at a high temperature of 1000-1200°C and keeping them warm for 30-60 minutes to obtain glass liquid; quenching the glass liquid with deionized water to obtain a glass crystal state, drying and crushing the glass crystal state, and then wet ball milling, adding stearic acid or stearate as a surface modifier during the ball milling process to modify the surface of the glass powder to obtain the glass powder.
2. The water-based environmentally friendly solar cell soldering silver paste according to claim 1, It is characterized in that The particle size of the silver powder is 0.1-1.5 μm, and the tap density of the silver powder is 2.5-4.5 g / cm 3 .
3. A method for preparing an aqueous environment-friendly solar cell soldering silver paste as claimed in claim 1 or 2, It is characterized in that The following steps are involved: The surfactant, thixotropic agent, deionized water and adhesive are mixed in proportion, and after being stirred evenly, glass powder and silver powder are added, and then stirred sufficiently to make the glass powder and silver powder evenly dispersed to obtain an initial silver paste; The initial silver paste is ground by three rollers for 3-5 times, and then stirred to adjust the viscosity to obtain the water-based environment-friendly solar cell welding silver paste.
4. The preparation method according to claim 3, It is characterized in that The preparation method of the adhesive comprises: The resin powder is added into deionized water, stirred at room temperature until the resin is completely dissolved in the water, and passed through a 400-mesh sieve to obtain the adhesive.