Positive electrode active material, preparation method thereof, lithium ion battery, battery module, battery pack and electric device comprising the same
By coating the surface of the cathode active material of the lithium-ion battery with a second lithium salt coating layer of fluorine and phosphorus elements to form a CEI film, the problems of high oxidation activity and slow solid-phase lithium ion transmission in lithium-ion batteries are solved, significantly improving Battery power performance and cycle life.
Patent Information
- Application Number
- CN202111291132.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-02
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2041-11-02
AI Technical Summary
The high oxidation activity of lithium-ion batteries and the slow transmission speed of solid-phase lithium ions cause the electrolyte to be oxidized and decomposed on the surface of the positive electrode during the battery cycle, consuming active lithium and reducing power performance and cycle life.
The surface of the positive electrode active material is coated with a second lithium salt coating layer containing fluorine and phosphorus elements to form a CEI film, which blocks electrolyte corrosion and improves the film structure, reduces active lithium consumption, and increases the lithium ion transmission rate.
Significantly improves the power performance and cycle life of lithium-ion batteries, reduces side reactions and extends battery life.
Smart Images

Figure CN116072829B
Abstract
Description
Technical Field
[0001] This application relates to the field of electrochemistry, and more particularly to a positive electrode active material, a lithium-ion battery containing the same, a battery module, a battery pack, and an electrical device. Background Art
[0002] With the rapid development of the new energy field, lithium-ion batteries, with their excellent electrochemical performance, lack of memory effect, and low environmental pollution, are widely used in various large-scale power devices, energy storage systems, and consumer products, especially in the field of new energy vehicles such as pure electric vehicles and hybrid electric vehicles. This places higher demands on the comprehensive improvement of the lifespan and fast-charging performance of lithium-ion batteries. Summary of the Invention
[0003] This application is made in view of the above-mentioned issues, and aims to provide a positive electrode active material that enables lithium-ion batteries to have both excellent power performance and cycle life.
[0004] This application provides a positive electrode active material, including a matrix and a coating layer located on the surface of the matrix. The matrix includes a first lithium salt, the first lithium salt being selected from layered structures such as LiAO2 and Li[Ni]. a Co b Mn c O2, and lithium-rich manganese-based xLi2MnO3·(1-x)LiMn y B 1-y At least one of O2, wherein A is Ni, Co, Mn or Al, and B is selected from one or two metal ions selected from Ni, Co or Al, and 0.1≤x≤0.9, 0.1≤y≤0.9, wherein 0<a<1, 0<b<1, 0<c<1, a+b+c=1. The coating layer includes a second lithium salt containing fluorine, phosphorus and oxygen simultaneously, wherein the oxygen in the second lithium salt contains a lone pair of electrons.
[0005] In any embodiment, based on the total mass of the positive electrode active material, the mass percentage of the second lithium salt is 0.1% to 20%, optionally 1% to 10%.
[0006] In any embodiment, the thickness of the positive electrode active material coating layer is 10–100 nm, and can be selected as 20–60 nm.
[0007] In any embodiment, the second lithium salt is selected from at least one of lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, and lithium tetrafluorooxalate phosphate.
[0008] In any embodiment, the positive electrode active material consists of first particles with a volume average particle size Dv50 of 2 to 8 μm and second particles with a volume average particle size Dv50 of 13 to 22 μm.
[0009] In any embodiment, the mass ratio of the first particles to the second particles is 2.3 to 9:1.
[0010] In any embodiment, the first and / or second particles simultaneously include both single crystal and polycrystalline crystal forms, and the mass ratio of the single crystal particles to the polycrystalline particles is 0.1 to 1:1, optionally 0.23 to 0.67:1.
[0011] The second aspect of the present application provides a method for preparing a positive electrode active material, including the following steps:
[0012] S1: Dry and dehydrate the first lithium salt to obtain the dried first lithium salt;
[0013] S2: Dissolve the second lithium salt in an organic solvent to obtain a second lithium salt organic solution;
[0014] S3: Add the dried first lithium salt to the second lithium salt organic solution and mix evenly;
[0015] S4: Filter the uniformly mixed mixture and perform heat treatment on the filtered solid particles to obtain the positive electrode active material; wherein, it includes a matrix and a coating layer located on the surface of the substrate,
[0016] The matrix includes a first lithium salt, and the first lithium salt is selected from at least one of spinel-structured LiAO4, layered-structured LiBO2, and lithium-rich manganese-based xLi2MnO3·(1-x)LiCO2, wherein A is Ni or Co, B is Ni, Co, Mn or Al, C is selected from Ni, Co or Mn and 0.1 < x < 0.9; the coating layer includes a second lithium salt containing both fluorine and phosphorus.
[0017] In any embodiment, before step S1, there is also step S0, and step S0 includes the step of preparing single crystal type first lithium salt and / or polycrystalline type first lithium salt.
[0018] In any embodiment, there is also step S5, and step S5 is to adjust the volume average particle size Dv50 of the positive electrode active material to obtain first particles with a volume average particle size Dv50 of 2 to 8 μm and second particles with a volume average particle size Dv50 of 13 to 22 μm.
[0019] In any embodiment, there is also step S6, and step S6 includes mixing the first particles and the second particles according to a predetermined mass ratio to obtain the positive electrode active material.
[0020] In any embodiment, in S1, the temperature range for drying and dehydrating the first lithium salt is 100 - 200 °C; and / or,
[0021] In S2, the organic solvent is an ether, carboxylic acid ester, or carbonate organic solvent; and / or,
[0022] In S3, the method of uniform mixing is to stir and disperse at 50–100°C for 4–8 hours; and / or,
[0023] In step S4, the heat treatment is performed in an air atmosphere at 200-250°C for 5-10 hours.
[0024] The third aspect of this application provides a lithium-ion battery, including the high-nickel ternary cathode active material described in the first aspect of this application or the high-nickel ternary cathode active material prepared by the preparation method in the second aspect of this application.
[0025] This application provides a fourth aspect of a battery module, including the lithium-ion battery of the third aspect of this application. The battery module can be fabricated using methods known in the prior art for fabricating battery modules.
[0026] This application provides a battery pack, including one or more of the lithium-ion battery of the third aspect of this application or the battery module of the fourth aspect of this application. The battery pack can be manufactured using methods known in the prior art for manufacturing battery packs.
[0027] A sixth aspect of this application provides an electrical device comprising one or more of the following: a lithium-ion battery according to the third aspect of this application, a battery module according to the fourth aspect of this application, or a battery pack according to the fifth aspect of this application. The lithium-ion battery, the battery module, or the battery pack serves as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device can be manufactured using methods known in the prior art for manufacturing electrical devices.
[0028] [Beneficial Effects]
[0029] This application, by coating the surface of the first lithium salt with a coating layer containing a second lithium salt, can, on the one hand, prevent the electrolyte from corroding and decomposing the first lithium salt, thereby reducing the occurrence of side reactions; on the other hand, it can enable the second lithium salt to form a CEI (cathode electrolyte interface) film in situ on the surface of the first lithium salt particles, thereby improving the film structure and preventing the decomposition of the effective components in the electrolyte; furthermore, the second lithium salt contains both fluorine and phosphorus elements, so that the composition of the formed film is as consistent as possible with the CEI film composition of lithium hexafluorophosphate (electrolyte) in the electrolyte, thereby reducing the consumption of active lithium in the electrolyte; the positive electrode active material of this application can significantly improve the power performance and cycle life of the battery.
[0030] The battery module, battery pack, and power device of this application include the lithium-ion battery provided in this application, and therefore have at least the same advantages as the lithium-ion battery. Attached Figure Description
[0031] Figure 1 This is a schematic diagram of the structure of the positive electrode active material of this application;
[0032] Figure 2 These are SEM images (Figure A) of the positive electrode active material of one embodiment of this application and SEM images (Figure B) of the positive electrode active material of Comparative Example 1 of this application.
[0033] Figure 3 This is a schematic diagram of a lithium-ion battery according to one embodiment of this application;
[0034] Figure 4 yes Figure 2 An exploded view of a lithium-ion battery according to an embodiment of this application is shown.
[0035] Figure 5 This is a schematic diagram of a battery module according to one embodiment of this application;
[0036] Figure 6 This is a schematic diagram of a battery pack according to one embodiment of this application;
[0037] Figure 7 yes Figure 5 An exploded view of a battery pack according to one embodiment of this application is shown;
[0038] Figure 8 This is a schematic diagram of an electrical device according to one embodiment of this application.
[0039] Explanation of reference numerals in the attached figures:
[0040] 1 battery pack;
[0041] 2 upper box;
[0042] 3 lower box;
[0043] 4 battery modules;
[0044] 5. Lithium-ion batteries;
[0045] 51. Shell;
[0046] 52 electrode assembly;
[0047] 53 Top cover assembly. Detailed Implementation
[0048] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the positive electrode active material, its manufacturing method, positive electrode sheet, secondary battery, battery module, battery pack, and electrical device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0049] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0050] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0051] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0052] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0053] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0054] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0055] It should be noted that the term "coating layer" refers to a portion that covers the surface of the substrate. This portion may, but does not necessarily, completely cover the "substrate". The use of "coating layer" is merely for ease of description and is not intended to limit this application.
[0056] For a series of positive electrode active materials for lithium-ion batteries, especially the nickel-cobalt-manganese ternary system, there are two major unavoidable drawbacks that are detrimental to electrical performance: 1) high oxidation activity; 2) slow solid-phase lithium-ion transport speed. High oxidation activity leads to continuous oxidative decomposition of the electrolyte on the positive electrode surface during battery cycling, consuming the limited active lithium in the positive electrode. The decomposition products deposited on the positive electrode surface significantly increase the diffusion resistance of lithium ions at the interface, thereby deteriorating the battery's power performance and cycle life. Therefore, it is necessary to modify the positive electrode active materials to overcome these drawbacks.
[0057] The continuous oxidation and decomposition of the electrolyte on the positive electrode surface is actually a process in which the solvent, electrolyte, additives, and other components in the electrolyte decompose and form a CEI (cathode electrolyte interface) film on the positive electrode surface. Therefore, if the positive electrode active material can be modified by in-situ coating with the effective components of the pre-formed CEI film, allowing the effective components of the pre-formed CEI film to form an in-situ film on the surface of the positive electrode active material, the probability of electrolyte oxidation will be significantly reduced, and the consumption of active lithium and the deposition of electrolyte decomposition byproducts will not occur, thereby significantly improving the battery's power and cycle performance.
[0058] Some lithium salts containing both fluorine and phosphorus, such as lithium difluorophosphate, are generally added to electrolytes as additives to improve battery cycle performance. However, they are difficult to dissolve in electrolytes and have low utilization rates. Furthermore, lithium difluorophosphate has low conductivity in electrolytes, and even a 1% addition will severely deteriorate the conductivity, thus hindering the battery's power performance.
[0059] Therefore, this application solves the aforementioned problems by using lithium salts such as lithium difluorophosphate as modifiers in the modification of positive electrode active materials, and significantly improves the power and cycle performance of lithium-ion batteries.
[0060] [Positive electrode active material]
[0061] This application provides a positive electrode active material, which includes a matrix and a coating layer located on the surface of the matrix.
[0062] The matrix includes a first lithium salt, which is selected from layered LiAO2 and Li[Ni] 2, etc. a Co b Mn c O2, and lithium-rich manganese-based xLi2MnO3·(1-x)LiMn y B 1-y At least one of O2, wherein A is Ni, Co, Mn or Al, and B is selected from one or two metal ions selected from Ni, Co or Al, and 0.1≤x≤0.9, 0.1≤y≤0.9, wherein 0<a<1, 0<b<1, 0<c<1, a+b+c=1. The coating layer includes a second lithium salt containing fluorine, phosphorus and oxygen, wherein the oxygen in the second lithium salt contains a lone pair of electrons.
[0063] This application, by coating the surface of the first lithium salt with a coating layer containing a second lithium salt, can, on the one hand, prevent the electrolyte from corroding and decomposing the first lithium salt in the matrix, thereby reducing the occurrence of side reactions; on the other hand, it can enable the second lithium salt to form a CEI film in situ on the surface of the first lithium salt particles, thereby improving the film structure and increasing the transport rate of lithium ions in the positive electrode active material; furthermore, the second lithium salt contains both fluorine and phosphorus elements, so that the composition of the formed film is as consistent as possible with the composition of the CEI film formed by lithium hexafluorophosphate (electrolyte) in the electrolyte, thereby reducing the consumption of active lithium in the electrolyte; in summary, the positive electrode active material of this application can significantly improve the power performance and cycle life of the battery.
[0064] In some embodiments, the second lithium salt is selected from at least one of lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, and lithium tetrafluoro(oxalate) phosphate.
[0065] The structural formulas of lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, and lithium tetrafluorooxalate phosphate are as follows:
[0066]
[0067] In addition to enabling in-situ synthesis of a CEI film and optimization of the film structure on the surface of the first lithium salt, the aforementioned second lithium salt structure also possesses oxygen lone pairs. These oxygen lone pairs in the second lithium salt allow lithium difluorophosphate to adhere tightly to the surface of the first lithium salt through complexation with transition metal ions in the first lithium salt, forming a uniform coating layer (see reference). Figure 2 .B, The surface of the untreated positive electrode active material particles is smooth; Reference Figure 2 A. The surface of the positive electrode active material of this application after modification treatment has a rough layer and the surface of the rough layer has protruding aggregate particles, which can not only prevent the coating layer from falling off the substrate, but also effectively prevent the dissolution of transition metals in the first lithium salt, thereby preventing the reduction of battery performance.
[0068] Furthermore, the second lithium salt can be lithium tetrafluorooxalate phosphate. A second lithium salt with a higher fluorine content can increase the stability of the formed CEI film, thus further improving battery performance. Experiments showed that, under the same conditions, using lithium tetrafluorooxalate phosphate as the second lithium salt as the positive electrode active material improved cycle performance by approximately 5% and reduced battery DCR by approximately 10%.
[0069] Furthermore, the surface of the coating layer of the positive electrode active material of this application has protruding aggregate particles formed by the second lithium salt.
[0070] The coating layer of the positive electrode active material in this application consists of a relatively flat layer and protruding aggregate particles on the surface of the layer. The second lithium salt is uniformly distributed in the relatively flat layer, thereby improving the microstructure of the CEI film on the surface of the positive electrode active material and increasing the transport rate of lithium ions in the positive electrode active material. On the other hand, the protruding aggregate particles, composed of the second lithium salt, are beneficial for replenishing the battery with additional lithium salt after long-term cycling, increasing the amount of active lithium in the electrolyte, and thus improving battery life.
[0071] In some embodiments, the mass percentage of the second lithium salt is 0.1% to 20% based on the total mass of the positive electrode active material, and can be selected as 1% to 10%.
[0072] When the mass percentage of the second lithium salt in the positive electrode is less than 0.1%, it cannot form an effective coating layer and cannot effectively hinder the contact between the positive electrode active material and the electrolyte, that is, it cannot effectively suppress the side reactions of the electrolyte at the positive electrode interface. When the mass percentage of the second lithium salt in the positive electrode is greater than 10%, it cannot further improve the effect, but instead increases the cost and also hinders the transport of lithium ions.
[0073] In some embodiments, the thickness of the coating layer of the positive electrode active material is 10–100 nm, and can be selected as 20–60 nm.
[0074] By keeping the coating thickness within a reasonable range, the effectiveness of the second lithium salt can be maintained while preventing a reduction in power performance due to obstructed lithium-ion transport.
[0075] In some embodiments, the positive electrode active material consists of first particles with a volume average particle size Dv50 of 2 to 8 μm and second particles with a volume average particle size Dv50 of 13 to 22 μm.
[0076] In some embodiments, the positive electrode active material is composed of a first particle and a second particle, with a mass ratio of 2.3 to 9:1.
[0077] The adaptive pairing of the first and second particles enables the presence of more positive electrode active material per unit thickness of the positive electrode film, thereby increasing the material compaction density and ultimately improving the battery energy density.
[0078] Furthermore, when the mass ratio of the first particle to the second particle is greater than 9:1, the presence of more large particles in the material prolongs the path of lithium ions in solid-phase transport, which has a certain impact on the power performance of the battery. When the mass ratio of large to small particles is less than 2.3:1, the presence of more small particles in the positive electrode active material results in a larger specific surface area of the material, which may lead to uneven coating of the coating layer, thereby affecting the effectiveness of the second lithium salt.
[0079] The particle size of the cathode material can be achieved through existing pulverization processes. For example, a mechanical pulverizer can be used to obtain first particles of 2–8 μm, and an air jet mill can be used to obtain second particles of 13–22 μm.
[0080] In some implementations, the first and / or second particles may include both single-crystal and polycrystalline forms.
[0081] In this application, single crystals have long ion transport paths but low specific surface areas and fewer side reactions, while polycrystalline materials have large specific surface areas and many side reactions, but short lithium-ion transport paths and better power performance. Combining the two can integrate the advantages of both.
[0082] This application provides a method for preparing a positive electrode active material, which includes the following steps:
[0083] S1: Dry and dehydrate the first lithium salt to obtain the dried first lithium salt;
[0084] S2: Dissolve the second lithium salt in an organic solvent to obtain an organic solution of the second lithium salt;
[0085] S3: Add the dried first lithium salt to the second lithium salt organic solution and mix thoroughly;
[0086] S4: Filter the homogeneous mixture and heat-treat the filtered solid particles to obtain the positive electrode active material; wherein, it includes a matrix and a coating layer located on the surface of the matrix.
[0087] The matrix includes a first lithium salt, which is selected from layered LiAO2 and Li[Ni] 2, etc. a Co b Mn c O2, and lithium-rich manganese-based xLi2MnO3·(1-x)LiMn y B 1-y At least one of O2, wherein A is Ni, Co, Mn or Al, and B is selected from one or two metal ions selected from Ni, Co or Al, and 0.1≤x≤0.9, 0.1≤y≤0.9, wherein 0<a<1, 0<b<1, 0<c<1, a+b+c=1. The coating layer includes a second lithium salt containing both fluorine and phosphorus.
[0088] In some embodiments, step S0 is included before step S1, which includes the steps of preparing a single-crystal first lithium salt and / or a polycrystalline first lithium salt.
[0089] In some embodiments, the method further includes step S5, which involves adjusting the volume average particle size Dv50 of the positive electrode active material to obtain first particles with a volume average particle size Dv50 of 2 to 8 μm and second particles with a volume average particle size Dv50 of 13 to 22 μm.
[0090] In some embodiments, the method further includes step S6, which involves mixing the first particle and the second particle in a predetermined mass ratio to obtain the positive electrode active material.
[0091] In some embodiments, in step S1, the temperature range for drying and dehydrating the first lithium salt is 100–200°C.
[0092] In some embodiments, in step S2, the organic solvent is an ether, a carboxylic acid ester, or a carbonate organic solvent.
[0093] In some embodiments, in step S3, the mixing is achieved by stirring and dispersing at 50–100°C for 4–8 hours; and / or,
[0094] In some embodiments, in step S4, the heat treatment is performed in an air atmosphere at 200-250°C for 5-10 hours.
[0095] [Positive electrode plate]
[0096] This application provides a positive electrode sheet, which includes the positive electrode active material of this application.
[0097] The positive electrode includes a positive current collector and a positive electrode material disposed on at least one surface of the positive current collector. As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode material is disposed on either or both of the two opposite surfaces of the positive current collector.
[0098] In the lithium-ion battery of this application, the positive electrode current collector can be a metal foil or a composite current collector. For example, aluminum foil can be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), 1,3-propanesulfonate lactone (PS), polyethylene (PE), etc.), but this application is not limited to these materials.
[0099] The cathode material may optionally include a conductive agent. However, there is no specific limitation on the type of conductive agent, and those skilled in the art can select it according to actual needs. As an example, the conductive agent used in the cathode material may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0100] In this application, the positive electrode sheet can be prepared according to methods known in the art. As an example, the positive active material, conductive agent and binder of this application can be dispersed in a solvent (e.g., N-methylpyrrolidone (NMP)) to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet is obtained.
[0101] [Negative electrode plate]
[0102] The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer including a negative electrode active material.
[0103] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0104] In the lithium-ion battery of this application, the negative electrode current collector can be a metal foil or a composite current collector. For example, copper foil can be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.), but this application is not limited to these materials.
[0105] In the negative electrode sheet of this application, the negative electrode film layer typically comprises a negative electrode active material and optional binders, optional conductive agents, and other optional additives, and is usually formed by coating and drying a negative electrode slurry. The negative electrode slurry is typically formed by dispersing the negative electrode active material, optional conductive agents, and binders in a solvent and stirring until homogeneous. The solvent can be N-methylpyrrolidone (NMP) or deionized water.
[0106] As an example, the conductive agent may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0107] In the negative electrode sheet of this application, the negative electrode film layer, in addition to the negative electrode active material, may optionally include other commonly used negative electrode active materials. Examples of other commonly used negative electrode active materials include artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from one or more of elemental tin, tin oxide compounds, and tin alloys.
[0108] [Electrolytes]
[0109] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be selected from at least one of solid electrolytes and liquid electrolytes (i.e., electrolyte solutions).
[0110] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0111] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).
[0112] In some embodiments, the solvent may be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butyl carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).
[0113] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature performance.
[0114] [Isolation membrane]
[0115] Lithium-ion batteries using electrolytes, as well as some lithium-ion batteries using solid electrolytes, also include a separator. The separator is disposed between the positive and negative electrodes, serving a separating function. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected. In some embodiments, the separator material can be selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0116] [Lithium-ion battery]
[0117] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly by a winding process or a stacking process, wherein the positive electrode includes the lithium iron phosphate positive electrode active material of this application.
[0118] In some embodiments, the lithium-ion battery may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte described above.
[0119] In some implementations, the outer packaging of a lithium-ion battery can be a rigid shell, such as a hard plastic shell, aluminum shell, or steel shell. The outer packaging of a lithium-ion battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0120] This application does not impose any particular limitation on the shape of the lithium-ion battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 2 This is an example of a square-structured lithium-ion battery 5.
[0121] In some implementations, refer to Figure 3The outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be placed over the opening to close the receiving cavity. A positive electrode sheet, a negative electrode sheet, and a separator can be formed into an electrode assembly 52 via a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The lithium-ion battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific needs.
[0122] [Battery Module]
[0123] In some implementations, lithium-ion batteries can be assembled into battery modules, and the number of lithium-ion batteries contained in a battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0124] Figure 4 This is battery module 4, used as an example. (See reference...) Figure 4 In battery module 4, multiple lithium-ion batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple lithium-ion batteries 5 can be fixed in place using fasteners.
[0125] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple lithium-ion batteries 5 are housed.
[0126] [Battery Pack]
[0127] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be selected by those skilled in the art based on the application and capacity of the battery pack.
[0128] Figure 5 and Figure 6 This is battery pack 1 as an example. (See reference...) Figure 5 and Figure 6 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0129] [Electrical appliances]
[0130] In addition, this application also provides an electrical device, which includes one or more of the lithium-ion battery, battery module, or battery pack provided in this application. The lithium-ion battery, battery module, or battery pack can be used as a power source for the device or as an energy storage unit for the device. The device can be, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0131] As the electrical device, a lithium-ion battery, battery module, or battery pack can be selected according to its usage requirements.
[0132] Figure 7 This is an example device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the device's requirements for high power and high energy density lithium-ion batteries, a battery pack or battery module can be used.
[0133] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use lithium-ion batteries as their power source.
[0134] Example
[0135] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the art or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products commonly used in the art and available commercially. Unless otherwise specified, the content of each component in the embodiments of this application is by mass.
[0136] Example
[0137] Example 1
[0138] Preparation of positive electrode active materials
[0139] Preparation of S0: Single-crystal / polycrystalline first lithium salt LiNi0.8Co0.1Mn0.1O2
[0140] S01): Preparation of single-crystal LiNi0.8Co0.1Mn0.1O2
[0141] The precursor Ni0.8Co0.1Mn0.1(OH)2 and lithium carbonate were added to a mortar and ground continuously for 10-15 min until homogeneous. The molar ratio of Li to the sum of transition metals was 1.2-1.25. The mixture was then placed in a tube furnace, and the air was first purged with nitrogen. Then oxygen was introduced and the temperature was raised to 820-900℃ and calcined for 12 h. The initial heating rate was 10℃ / min and the final cooling rate was 10℃ / min. After cooling, the mixture was ground again in a mortar and sieved to obtain single crystal LiNi0.8Co0.1Mn0.1O2.
[0142] SO2): The precursor Ni0.8Co0.1Mn0.1(OH)2 and lithium carbonate were added to a mortar and ground continuously for 10-15 min until they were uniformly mixed. The molar ratio of Li to the sum of the transition metals was 1.0-1.15. The mixture was then placed in a tube furnace, and the air was first purged with nitrogen. Then oxygen was introduced and the temperature was raised to 600-800℃ and calcined for 12 h. The initial heating rate was 10℃ / min and the final cooling rate was 10℃ / min. After cooling, the mixture was ground again in a mortar and sieved to obtain polycrystalline LiNi0.8Co0.1Mn0.1O2.
[0143] S1: Single-crystal LiNi0.8Co0.1Mn0.1O2 and polycrystalline LiNi0.8Co0.1Mn0.1O2 are uniformly mixed at a mass ratio of 0.4:1 and dried at 150℃ for 2 hours to obtain the dried first lithium salt;
[0144] S2: Dissolve the second lithium salt, lithium difluorophosphate, in 1,2-dimethoxyethane (to make the mass fraction of lithium difluorophosphate 15%).
[0145] S3: The dried first lithium salt is added to the 1,2-dimethoxyethane solution of the second lithium salt. The amount of the first lithium salt added is 90% of the sum of the masses of the first lithium salt and the second lithium salt, and the mixture is stirred and dispersed at 30°C for 4 hours.
[0146] S4: The above uniformly mixed mixture is filtered, and the filtered solid particles are treated in an air atmosphere at 200°C for 5 hours to obtain a positive electrode active material that is a mixture of single crystal and polycrystalline forms.
[0147] S5: Preparation of the first / second particle
[0148] The positive electrode active material obtained in step S4 is pulverized in a mechanical pulverizer at a specific frequency to obtain first particles with a particle size of 5 μm; the positive electrode active material obtained in step S4 is pulverized in an air jet pulverizer at a specific frequency to obtain second particles with a particle size of 15 μm.
[0149] S6: Mix the first particle and the second particle at a mass ratio of 3:1 to obtain the positive electrode active material of Example 1.
[0150]
Positive Electrode
[0151] The positive electrode active material from Example 1, the conductive agent Super P, and the binder polyvinylidene fluoride (PVDF) were used to prepare a positive electrode slurry in N-methylpyrrolidone (NMP). The solid content of the positive electrode slurry was 50 wt%, and the mass ratio of the positive electrode active material, Super P, and PVDF in the solid components was 8:1:1. The positive electrode slurry was coated onto a current collector aluminum foil and dried at 85°C, followed by cold pressing. Then, the foil was trimmed, cut into sheets, and slit. Finally, it was dried under vacuum at 85°C for 4 hours to produce a positive electrode sheet.
[0152] [Negative electrode plate]
[0153] Graphite, used as the negative electrode active material, was mixed evenly with conductive agent Super P, thickener CMC, and binder styrene-butadiene rubber (SBR) in deionized water to prepare a negative electrode slurry. The solid content of the negative electrode slurry was 30 wt%, and the mass ratio of graphite, Super P, CMC, and binder styrene-butadiene rubber (SBR) in the solid components was 80:15:3:2. The negative electrode slurry was coated onto a current collector copper foil and dried at 85°C. Then, it was cold-pressed, trimmed, cut into sheets, and slit. Finally, it was dried under vacuum at 120°C for 12 hours to prepare the negative electrode sheet.
[0154] Electrolyte
[0155] EC:DEC:DMC were mixed in a volume ratio of 1:1:1, and LiPF6 was added to form an electrolyte. The concentration of LiPF6 in the electrolyte was 1 mol / L.
[0156]
Isolation Film
[0157] Polyethylene separator film.
[0158] [Preparation of Lithium-ion Batteries]
[0159] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. After being wound into a square bare cell, it is placed in an aluminum-plastic film, injected with the appropriate non-aqueous electrolyte, and sealed. After processes such as standing, hot and cold pressing, formation, clamping, and capacity testing, a lithium-ion battery is obtained.
[0160] Comparative Example 1
[0161] The product used is a commercially available LiNi0.8Co0.1Mn0.1O2, model number HAH101, purchased from Hunan Bangpu Recycling Technology Co., Ltd.
[0162] The other preparation process is the same as in Example 1.
[0163] Example 2
[0164] In the preparation of the positive electrode active material, in step S1, the first lithium salt used is LiNiO2 and the second lithium salt is lithium difluorobis(oxalato)phosphate; in step S3, the amount of the first lithium salt added is 91% of the sum of the mass of the first lithium salt and the second lithium salt; in step S5, the particle size of the first particle is prepared to be 7 μm and the particle size of the second particle is prepared to be 16 μm; other preparation processes are the same as in Example 1.
[0165] Example 3
[0166] In the preparation of the positive electrode active material, in step S1, the first lithium salt used is LiMnO2 and the second lithium salt is lithium tetrafluorooxalate phosphate; in step S3, the amount of the first lithium salt added is 91% of the sum of the mass of the first lithium salt and the second lithium salt; in step S6, the mixing mass ratio of the first particle to the second particle is 4:1; other preparation processes are the same as in Example 1.
[0167] Example 4
[0168] In the preparation of the positive electrode active material, in step S1, the first lithium salt used is 0.5Li2MnO3·0.5LiMn0.3Co0.7O2; the other preparation processes are the same as in Example 1.
[0169] Examples 5 to 15
[0170] In the preparation of the positive electrode active material, in step S1 and step S3, the amount of the first lithium salt added is 1.8% of the sum of the mass of the first lithium salt and the second lithium salt, respectively.
[0171] 5%, 15%, 20%, 0.9%, 30%, 0.10%, 5%, 20%, 0.01%, 25%; other preparation processes are the same as in Example 1.
[0172] Examples 16-20
[0173] In the preparation of the positive electrode active material, in step S5, the particle sizes of the first particles are prepared as 2μm, 4μm, 8μm, 1μm, and 10μm, respectively, and the other preparation processes are the same as in Example 1.
[0174] Examples 21-25
[0175] In the preparation of the positive electrode active material, in step S5, the particle sizes of the second particles are prepared as 13μm, 18μm, 22μm, 10μm, and 25μm, respectively; the other preparation processes are the same as in Example 1.
[0176] Examples 26-30
[0177] In the preparation of the positive electrode active material, in step S6, the mixing mass ratio of the first particle to the second particle is 2.3:1, 4:1, 9:1, 1.8:1, and 9.5:1, respectively, and the other preparation processes are the same as in Example 1.
[0178] Example 31
[0179] In the preparation of the positive electrode active material, step S0 does not include step S02, which involves the preparation of a polycrystalline first lithium salt; the other processes are similar to those in Example 1.
[0180] [Testing of Relevant Parameters for Positive Electrode Active Materials]
[0181] 1. Composition and mass percentage of the second lithium salt in the positive electrode active material (taking lithium difluorophosphate as an example)
[0182] The content of the second lithium salt was tested according to the general rules of ion chromatography analysis in JY / T 020-1996.
[0183] 2. Volume average particle size Dv50 test
[0184] D50 test shall be performed in accordance with GB / T19077-2016.
[0185] 3. Coating thickness test
[0186] An IB-19500CP ion polishing system was used. After cleaning the sample preparation tools, the sample preparation adhesive (a gel-like substance formed by dispersing PVDF in NMP, with a PVDF mass content of 8%) was mixed with the sample powder (approximately 5 times the weight of the powder) and evenly applied to copper foil. The sample was then dried at 60°C for 30 minutes. The prepared sample was cut into 6mm × 6mm pieces using scissors, fixed on the sample stage, and placed in the ion polishing system (model: IB-19500CP) for cutting. According to JBT9352-1999, the cut samples were then subjected to thickness measurement using a FEITecnai G2 transmission electron microscope (USA).
[0187] [Battery Performance Test]
[0188] 1. Initial discharge capacity
[0189] At 25℃, a lithium-ion battery is charged at a constant current of 1C to 4.25V, then charged at a constant voltage to a current of 0.05C. After the battery is fully charged, it is left to stand for 5 minutes, then discharged at 1C for 30 minutes (the battery has a state of charge of 50%), left to stand for 5 minutes, and the temperature is adjusted to 25℃. After standing for 1 hour, the battery voltage V1 is recorded. After discharging at 0.4C for 15 seconds, the voltage V2 after the pulse discharge is recorded. Then, the DCR of the battery at 50% SOC is (V1-V2) / I, where I = 0.4C.
[0190] 2. Cyclic capacity retention
[0191] At 25°C, charge-discharge tests were performed on all lithium-ion batteries used in the examples and comparative examples. One charge-discharge cycle was as follows: constant current charging at 1C to 4.25V, then constant voltage charging at 4.25V until the current ≤0.05mA, resting for 5 minutes, and then constant current discharging at 1C to 2.8V. The battery capacity at this point was recorded as C1. This constitutes one charge-discharge cycle. The above process was repeated 200 times, and the battery capacity at this point was recorded as C200. Therefore, the cycle capacity retention rate = C200 / C1 × 100%.
[0192] The product parameters of the positive electrode active materials and the lithium-ion battery performance parameters of the examples and comparative examples are shown in Tables 1 to 6.
[0193]
[0194]
[0195]
[0196]
[0197]
[0198]
[0199]
Claims
1. A positive electrode active material, characterized in that: It comprises a substrate and a coating layer located on the surface of the substrate, The matrix includes a first lithium salt, which is selected from the group consisting of LiAO2, Li[Ni a Co b Mn c ]O2, and lithium-rich manganese-based xLi2MnO3·(1-x)LiMn y B 1-y O2, wherein A is Ni, Co, Mn or Al, B is selected from one or two metal ions of Ni, Co or Al, and 0.1≤x≤0.9, 0.1≤y≤0.9, 0<a<1, 0<b<1, 0<c<1, a+b+c=1, The coating layer includes a second lithium salt containing fluorine, phosphorus and oxygen simultaneously, wherein oxygen in the second lithium salt contains a lone electron pair.
2. The positive electrode active material according to claim 1, characterized in that The coating layer has protruding accumulation particles formed by the second lithium salt on its surface.
3. The positive electrode active material according to claim 1 or 2, characterized in that: Based on the total mass of the positive electrode active material, the mass proportion of the second lithium salt is 0.1% to 20%.
4. The positive electrode active material according to claim 3, characterized in that Based on the total mass of the positive electrode active material, the mass proportion of the second lithium salt is 1% to 10%.
5. The positive electrode active material according to claim 1, characterized in that The thickness of the coating layer is 10-100 nm.
6. The positive electrode active material according to claim 5, characterized in that The thickness of the coating layer is 20-60 nm.
7. The positive electrode active material according to claim 1, characterized in that The second lithium salt is selected from at least one of lithium difluorophosphate, lithium difluorobisoxalate phosphate, and lithium tetrafluorooxalate phosphate.
8. The positive electrode active material according to claim 1, characterized in that The positive electrode active material consists of first particles with a volume average particle size Dv50 of 2 to 8 μm and second particles with a volume average particle size Dv50 of 13 to 22 μm.
9. The positive electrode active material according to claim 8, characterized in that The mass ratio of the first particles to the second particles is 2.3-9:
1.
10. The positive electrode active material according to claim 9, characterized in that The first and / or second particles include two crystal forms: single crystal and polycrystalline, and the mass ratio of single crystal particles to polycrystalline particles is 0.1-1:
1.
11. The positive electrode active material according to claim 10, characterized in that The mass ratio of the single crystal particles to the polycrystalline particles is 0.23-0.67:
1.
12. A method for preparing a positive electrode active material, characterized in that: The steps include: S1: drying and dehydrating the first lithium salt to obtain a dried first lithium salt; S2: dissolving the second lithium salt in an organic solvent to obtain a second lithium salt organic solution; S3: adding the dried first lithium salt to the second lithium salt organic solution and mixing them evenly; S4: filtering the uniformly mixed mixture and heat-treating the filtered solid particles to obtain the positive electrode active material; wherein the positive electrode active material comprises a substrate and a coating layer located on the surface of the substrate, The matrix includes a first lithium salt, which is selected from the group consisting of LiAO2, Li[Ni a Co b Mn c ]O2, and lithium-rich manganese-based xLi2MnO3·(1-x)LiMn y B 1-y O2, wherein A is Ni, Co, Mn or Al, B is selected from one or two metal ions of Ni, Co or Al, and 0.1≤x≤0.9, 0.1≤y≤0.9, 0<a<1, 0<b<1, 0<c<1, a+b+c=1; the coating layer includes a second lithium salt containing both fluorine and phosphorus, The oxygen in the second lithium salt contains a lone electron pair.
13. The preparation method according to claim 12, characterized in that: Before step S1, step S0 is also included, and step S0 includes the step of preparing a single-crystal first lithium salt and / or a polycrystalline first lithium salt.
14. The preparation method according to claim 12 or 13, characterized in that: The invention also includes step S5, wherein the volume average particle size Dv50 of the positive electrode active material is adjusted to obtain first particles with a volume average particle size Dv50 of 2 to 8 μm and second particles with a volume average particle size Dv50 of 13 to 22 μm.
15. The preparation method according to claim 14, characterized in that: The method further includes step S6, wherein the step S6 includes mixing the first particles and the second particles according to a predetermined mass ratio to obtain the positive electrode active material.
16. The preparation method according to claim 12, characterized in that: In S1, the temperature range of drying and dehydrating the first lithium salt is 100-200° C.; and / or, In S2, the organic solvent is an ether, carboxylate, or carbonate organic solvent; and / or, In said S3, the uniform mixing is carried out by stirring and dispersing at 50-100° C. for 4-8 hours; and / or, In S4, the heat treatment is performed in an air atmosphere at 200-250° C. for 5-10 hours.
17. A lithium-ion battery, comprising a positive electrode sheet, a separator and a negative electrode sheet, characterized in that: The positive electrode sheet comprises the positive electrode active material according to any one of claims 1 to 11 or the positive electrode active material prepared by the preparation method according to any one of claims 12 to 16.