A kind of folding-resistant high-peeling aluminum-coated fabric and preparation method thereof

By etching, applying coupling agent and conductive adhesive on the aluminum foil fabric, and forming an aluminum film on the fabric, the problem of easy breakage of aluminum foil fabric during folding and friction is solved, and folding resistance and high peeling performance are achieved. Improved and maintained protective performance.

CN116080189BActive Publication Date: 2024-12-03NANTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211391807.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-08
Publication Date
2024-12-03
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

Existing aluminum foil fabrics are prone to frictional damage and peeling during use, resulting in a degradation of protective performance, especially in case of repeated folding and friction.

Method used

Plasma etching of the aluminum foil surface is used to form an etching surface, and a coupling agent and conductive adhesive are applied to form an outer protective body. Then, vacuum-plated aluminum on the first fabric to form an aluminum film, and with the second fabric Sew together to form a multi-layer structure to improve fold resistance and high peeling properties.

Benefits of technology

Through the dual protection mechanism of the outer aluminum foil and the inner aluminum film, the folding and friction resistance of the fabric is enhanced, the gaps in the damage of the aluminum foil are filled, the protective performance is maintained, and the cushioning effect is provided through the fabric connection, which significantly improves the fracture strength and High peeling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116080189B_ABST
    Figure CN116080189B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of aluminum foil fabrics, in particular to a folding-resistant and highly peelable aluminum-coated fabric and a preparation method thereof. The following scheme is proposed, which comprises the following steps: Step 1: using plasma to etch the surface of the aluminum foil to form an etched surface, applying a coupling agent on the etched surface to form a coupling agent layer, applying a conductive adhesive on the coupling agent layer to form an adhesive layer, and pressing a first fabric on the adhesive layer to obtain an outer protective body; Step 2: vacuum-plating aluminum on one side of the first fabric to form an aluminum film, pasting a second fabric on one side of the aluminum film, and sewing the first fabric and the second fabric together to obtain an aluminum-coated fabric. The present invention achieves the folding-resistant and friction-resistant performance of the aluminum-coated fabric through the protective form of an outer protective body (aluminum foil) + an inner protective body (aluminum film).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aluminum foil fabrics, in particular to a folding-resistant and highly peelable aluminum-coated fabric and a preparation method thereof. Background Art

[0002] Electromagnetic pollution has become the fourth largest pollution source after air pollution, water pollution and noise pollution, and it has attracted people's attention day by day. The urgent demand for electromagnetic wave shielding and protection has promoted the research and development of shielding conductive materials.

[0003] Aluminum foil has the characteristics of good conductivity and excellent thermal insulation performance. It is usually compounded with flexible fabrics and used in the fields of thermal protection, electromagnetic shielding, etc., and plays an important role. However, the surface bonding performance of aluminum foil is poor. The bonding strength between the aluminum film layer and the fabric is an important indicator of the aluminum foil fabric during use. The fabric will always be damaged by external factors to a certain extent during use. For example, after repeated use, the aluminum film layer will be damaged by friction. After repeated folding, it is easy to be damaged and easy to peel off from the fabric, resulting in a decrease in the protective performance of the composite fabric, thereby affecting the shielding performance of the fabric. For this reason, the present invention proposes a folding-resistant high-peeling aluminum-coated fabric and a preparation method thereof. Summary of the invention

[0004] In order to solve the problems in the prior art, the present invention provides a folding-resistant and highly peelable aluminum-coated fabric and a preparation method thereof.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a folding-resistant and highly peelable aluminum-coated fabric comprises the following steps:

[0007] Step 1: using plasma to etch the surface of the aluminum foil to form an etched surface, applying a coupling agent on the etched surface to form a coupling agent layer, applying a conductive adhesive on the coupling agent layer to form an adhesive layer, and pressing the first fabric on the adhesive layer to obtain an outer protective body;

[0008] Step 2: vacuum-plating aluminum on one side of the first fabric to form an aluminum film, pasting a second fabric on one side of the aluminum film, and sewing the first fabric and the second fabric together to obtain an aluminum-coated fabric.

[0009] In some embodiments, the aluminum foil is immersed in a 1%-3% sodium hydroxide solution for 20-40 minutes.

[0010] In some embodiments, the plasma etches the surface of the aluminum foil at a speed of 3-6 cm / s and an input power of 200-500 W.

[0011] In some embodiments, the aluminum foil is left to stand in air for 1-2 hours after being plasma etched before being coated with a coupling agent.

[0012] In some embodiments, the first fabric is a polyester fabric roughened with NaOH, ethylenediamine or alcohol solution.

[0013] In some embodiments, the conductive adhesive is formed by melt-mixing a hot-melt adhesive composed of a thermoplastic resin with a conductive filler and an additive.

[0014] In some embodiments, the thermoplastic resin includes modified polyurethane with a melting point of 90° C.-100° C., the conductive filler includes at least one of 5-60 nm nanoscale carbon black, carbon nanotubes, carbon fibers, and graphene, and the additive includes acrylic acid.

[0015] In some embodiments, the fabric density of the first fabric is (80-90)×(70-80) strands / inch.

[0016] In some embodiments, the modified polyurethane comprises a resin obtained by melting and mixing 70% by weight of ethylene-methacrylate copolymer and 30% by weight of thermoplastic polyurethane.

[0017] The aluminum-coated fabric prepared by the above preparation method.

[0018] Beneficial effects of the present invention:

[0019] The aluminum foil on the surface of the aluminum-coated fabric of the present invention is damaged after being rubbed and folded, but there is still an aluminum film inside the aluminum-coated fabric. Since the aluminum film is vacuum-plated on the surface of the first fabric, aluminum particles are dispersed into the gaps of the first fabric. Even if the aluminum foil is folded and damaged, the internal aluminum film has good protective performance, so it can fill the gap of the aluminum foil at the damaged part.

[0020] The protective form of the outer protective body (aluminum foil) + inner protective body (aluminum film) mentioned above achieves the folding and friction resistance of the aluminum-coated fabric, and the outer aluminum foil has a certain buffering effect when it is pulled by connecting the first fabric and the second fabric together, and because it has a strong breaking strength, it has a high peeling performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic structural diagram of the aluminum-coated fabric of the present invention.

[0022] Numbers in the figure: 1 thin wire, 2 second fabric, 3 aluminum film, 4 first fabric, 5 adhesive layer, 6 coupling agent layer, 7 aluminum foil. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0024] Three samples were prepared according to the following examples or comparative examples.

[0025] Example 1

[0026] (1) placing an aluminum foil with a thickness of 0.1 mm and a size of 20 cm*20 cm in a container containing a sodium hydroxide solution with a mass percentage concentration of 1% and immersing it for 20 minutes to remove impurities from the surface of the aluminum foil. After the impurities are removed, the aluminum foil is washed three times with deionized water and dried;

[0027] (2) The upper surface of the dried aluminum foil was etched using arc plasma. After etching, it was placed in the air for 1 hour so that the surface of the etched aluminum foil was oxidized by oxygen to form a protective film. The etching parameters were set as follows: Ar was used as the working gas with a flow rate of 20 sccm. A trapezoidal columnar graphite target with a purity of 99.999% and diameters of φmax70mm and φmin60mm was used. The arc source magnetic coil (SM) current, bending magnetic coil (BM) current and output magnetic coil (OM) current were set to 2.0, 4.5, and 4.5A respectively. The positive bias voltage of the bend was 10V. The cathode power supply was turned on to generate arc plasma. A negative bias voltage of 450V was applied to the substrate. The etching speed was 3cm / s and the input power was 200w.

[0028] (3) coating the silane coupling agent solution with a mass percentage concentration of 0.5% on the surface of the etched aluminum foil, and drying it at 40° C. for 10 minutes to form a coupling agent layer;

[0029] (4) preparing a molten conductive adhesive: 70 g of ethylene-methacrylate copolymer and 30 g of thermoplastic polyurethane were mixed and melted to obtain a modified polyurethane, and then extruded and granulated to obtain polyurethane particles, 20 g of acrylic acid and 10 g of 5 nm graphene were mixed, and the mixed solution was mixed and melted with 100 g of the modified polyurethane particles at 200° C. to obtain a conductive adhesive;

[0030] (5) applying a molten conductive adhesive to the coupling agent layer of the aluminum foil at 100° C. to a thickness of 1 mm to form a molten conductive adhesive layer;

[0031] (6) placing a polyester fabric with a fabric density of 80×70 strands / inch in a sodium hydroxide solution with a mass percentage concentration of 2% for 10 minutes to perform a roughening treatment, and then washing and drying the polyester fabric with deionized water; using a pressing roller to press the dried polyester fabric onto the conductive adhesive layer, so that part of the conductive adhesive seeps out of the surface of the polyester fabric, and drying at 80° C. for 30 minutes to obtain an outer protective body;

[0032] (7) The surface of the polyester fabric is electroplated by vacuum evaporation to form an aluminum film with a thickness of 0.05 mm. The coated outer protective body is placed at 100° C., the cloth fabric (second fabric) is coated with the aluminum film, and the cloth fabric (second fabric) is sewn together with the first fabric by needle and thread to obtain an aluminum-coated fabric that is resistant to folding and high peeling.

[0033] Example 2

[0034] (1) placing an aluminum foil with a thickness of 0.1 mm and a size of 20 cm*20 cm in a container containing a sodium hydroxide solution with a mass percentage concentration of 2% and immersing it for 30 minutes to remove impurities from the surface of the aluminum foil. After the impurities are removed, the aluminum foil is washed three times with deionized water and dried;

[0035] (2) The upper surface of the dried aluminum foil was etched by arc plasma. After etching, it was placed in air for 1.5 hours so that the surface of the etched aluminum foil was oxidized by oxygen to form a protective film. The etching parameters were set as follows: Ar was used as the working gas with a flow rate of 20 sccm. A trapezoidal columnar graphite target with a purity of 99.999% and a diameter of φmax70mm and φmin60mm was used. The arc source magnetic coil (SM) current, bending magnetic coil (BM) current and output magnetic coil (OM) current were set to 2.0, 4.5, and 4.5A respectively. The positive bias voltage of the bending tube was 10V. The cathode power supply was turned on to generate arc plasma. A negative bias voltage of 450V was applied to the substrate. The etching speed was 5cm / s and the input power was 300w.

[0036] (3) coating the silane coupling agent solution with a mass percentage concentration of 0.5% on the surface of the etched aluminum foil, and drying it at 40° C. for 10 minutes to form a coupling agent layer;

[0037] (4) preparing a molten conductive adhesive: 70 g of ethylene-methacrylate copolymer and 30 g of thermoplastic polyurethane were mixed and melted to obtain a modified polyurethane, and then extruded and granulated to obtain polyurethane particles, 20 g of acrylic acid and 10 g of 20 nm graphene were mixed, and the mixed solution was mixed and melted with 100 g of the modified polyurethane particles at 200° C. to obtain a conductive adhesive;

[0038] (5) applying a molten conductive adhesive to the coupling agent layer of the aluminum foil at 100° C. to a thickness of 1 mm to form a molten conductive adhesive layer;

[0039] (6) placing a polyester fabric with a fabric density of 85×75 strands / inch in a sodium hydroxide solution with a mass percentage concentration of 2% for 10 minutes to perform a roughening treatment, and then washing and drying the polyester fabric with deionized water; using a pressing roller to press the dried polyester fabric onto the conductive adhesive layer, so that part of the conductive adhesive seeps out of the surface of the polyester fabric, and drying at 80° C. for 30 minutes to obtain an outer protective body;

[0040] (7) The surface of the polyester fabric is electroplated by vacuum evaporation to form an aluminum film with a thickness of 0.05 mm. The coated outer protective body is placed at 100° C., the cloth fabric (second fabric) is coated with the aluminum film, and the cloth fabric (second fabric) is sewn together with the first fabric by needle and thread to obtain an aluminum-coated fabric that is resistant to folding and high peeling.

[0041] Example 3

[0042] (1) placing an aluminum foil with a thickness of 0.1 mm and a size of 20 cm*20 cm in a container containing a sodium hydroxide solution with a mass percentage concentration of 3% and immersing it for 40 minutes to remove impurities from the surface of the aluminum foil, and then washing the aluminum foil three times with deionized water and drying it;

[0043] (2) The upper surface of the dried aluminum foil was etched by arc plasma. After etching, it was placed in the air for 2 hours so that the surface of the etched aluminum foil was oxidized by oxygen to form a protective film. The etching parameters were set as follows: Ar was used as the working gas with a flow rate of 20 sccm. A trapezoidal columnar graphite target with a purity of 99.999% and a diameter of φmax70mm and φmin60mm was used. The arc source magnetic coil (SM) current, bending magnetic coil (BM) current and output magnetic coil (OM) current were set to 2.0, 4.5, and 4.5A respectively. The positive bias voltage of the bending tube was 10V. The cathode power supply was turned on to generate arc plasma. A negative bias voltage of 450V was applied to the substrate. The etching speed was 3cm / s and the input power was 500w.

[0044] (3) coating the silane coupling agent solution with a mass percentage concentration of 0.5% on the surface of the etched aluminum foil, and drying it at 40° C. for 10 minutes to form a coupling agent layer;

[0045] (4) preparing a molten conductive adhesive: 70 g of ethylene-methacrylate copolymer and 30 g of thermoplastic polyurethane were mixed and melted to obtain a modified polyurethane, and then extruded and granulated to obtain polyurethane particles, 20 g of acrylic acid and 10 g of 5 nm graphene were mixed, and the mixed solution was mixed and melted with 100 g of the modified polyurethane particles at 200° C. to obtain a conductive adhesive;

[0046] (5) applying a molten conductive adhesive to the coupling agent layer of the aluminum foil at 100° C. to a thickness of 1 mm to form a molten conductive adhesive layer;

[0047] (6) placing a polyester fabric with a fabric density of 90×80 strands / inch in a sodium hydroxide solution with a mass percentage concentration of 2% for 10 minutes to perform a roughening treatment, and then washing and drying the polyester fabric with deionized water; using a pressing roller to press the dried polyester fabric onto the conductive adhesive layer, so that part of the conductive adhesive seeps out of the surface of the polyester fabric, and drying at 80° C. for 30 minutes to obtain an outer protective body;

[0048] (7) The surface of the polyester fabric is electroplated by vacuum evaporation to form an aluminum film with a thickness of 0.05 mm. The coated outer protective body is placed at 100° C., the cloth fabric (second fabric) is coated with the aluminum film, and the cloth fabric (second fabric) is sewn together with the first fabric by needle and thread to obtain an aluminum-coated fabric that is resistant to folding and high peeling.

[0049] Figure 1 2 is a schematic diagram of the structure of the aluminum-coated fabric of the present invention. A coupling agent layer 6 is adhered to one side of the aluminum foil 7, an adhesive layer 5 is coated on one side of the coupling agent layer 6, a first fabric 4 is adhered to one side of the adhesive layer 5, an aluminum film 3 is plated on one side of the first fabric 4, a second fabric 2 is provided on one side of the aluminum film 3, a thin wire 1 is sequentially passed through the second fabric 2, the aluminum film 3, and the first fabric 4, and the first fabric 4 and the second fabric 2 are sewn together, and the second fabric 2 mainly plays the role of bearing force.

[0050] Comparative Example 1

[0051] Compared with Example 1, vacuum aluminum plating is not performed, and the roughened cloth fabric (second fabric) is directly covered on the adhesive layer, which specifically includes the following steps:

[0052] (1) placing an aluminum foil with a thickness of 0.1 mm and a size of 20 cm*20 cm in a container containing a sodium hydroxide solution with a mass percentage concentration of 1% and immersing it for 20 minutes to remove impurities from the surface of the aluminum foil. After the impurities are removed, the aluminum foil is washed three times with deionized water and dried;

[0053] (2) The upper surface of the dried aluminum foil was etched using arc plasma. After etching, it was placed in the air for 1 hour so that the surface of the etched aluminum foil was oxidized by oxygen to form a protective film. The etching parameters were set as follows: Ar was used as the working gas with a flow rate of 20 sccm. A trapezoidal columnar graphite target with a purity of 99.999% and diameters of φmax70mm and φmin60mm was used. The arc source magnetic coil (SM) current, bending magnetic coil (BM) current and output magnetic coil (OM) current were set to 2.0, 4.5, and 4.5A respectively. The positive bias voltage of the bend was 10V. The cathode power supply was turned on to generate arc plasma. A negative bias voltage of 450V was applied to the substrate. The etching speed was 3cm / s and the input power was 200w.

[0054] (3) coating the silane coupling agent solution with a mass percentage concentration of 0.5% on the surface of the etched aluminum foil, and drying it at 40° C. for 10 minutes to form a coupling agent layer;

[0055] (4) preparing a molten adhesive: 70 g of ethylene-methacrylate copolymer and 30 g of thermoplastic polyurethane were mixed and melted to obtain a modified polyurethane, and then extruded and granulated to obtain polyurethane particles, 20 g of acrylic acid and 10 g of 5 nm graphene were mixed, and the mixed solution was mixed and melted with 100 g of the modified polyurethane particles at 200° C. to obtain a conductive adhesive;

[0056] (5) applying a molten conductive adhesive to the coupling agent layer of the aluminum foil at 100° C. to a thickness of 1 mm to form a molten conductive adhesive layer;

[0057] (6) Lay the cloth fabric (second fabric) on the conductive adhesive layer, use a pressing roller to compact the cloth fabric (second fabric) and the conductive adhesive layer, and then place them at 80° C. for drying to obtain an aluminum-coated fabric.

[0058] Test analysis

[0059] 1. Breaking strength test

[0060] Fabric breaking strength was tested according to GB / T3923.1-1997 standard using a YG(B)26D-500 electronic fabric strength tester on the aluminum-coated fabrics prepared in Examples 1-3 and Comparative Example 1. Sample strips of 15 cm × 5 cm were prepared along the warp and weft directions. The test results are shown in Table 1

[0061] Table 1 Breaking strength test results of aluminum-coated fabrics

[0062]

[0063] It can be seen from the data in Table 1 that the breaking strength of the aluminum-coated fabrics prepared by the methods of Examples 1-3 is relatively large, and is much greater than the breaking strength of the aluminum-coated fabric of Comparative Example 1, indicating that the aluminum-coated fabrics prepared by the method of the present invention have high strength, good toughness and high peelability.

[0064] 2. Friction the aluminum-covered fabric

[0065] The flat grinding method was adopted, and the aluminum foil surface of the aluminum-coated fabric prepared in Implementation 1 and Comparative Example 1 was rubbed using a YG522N disc-type fabric wear machine in accordance with GB / T 21196.4-2007 standard. A circular test sample was prepared with reference to the sample template, and after ensuring that the surface of the fabric was flat, the cloth clamping ring was used to tighten it, and the sample was subjected to a certain tension. The dust collection device was placed on the flat grinder, and the dust collection switch was turned on. Press the power button, and the working disc drove the fabric to perform a constant speed circular motion, and the aluminum foil surface was rubbed. When the counter was 20, the switch was paused, and the radiation protection performance of the aluminum-coated fabric after friction was tested.

[0066] 3. Folding resistance test

[0067] The aluminum-coated fabrics prepared in Implementation Example 1 and Comparative Example 1 were folded in half three times respectively, and each aluminum-coated fabric was folded 10 times repeatedly. The radiation protection performance of the folded aluminum-coated fabrics was tested.

[0068] 4. Radiation protection performance test

[0069] Referring to GB / T 23463-2009 standard, the N998B electromagnetic radiation detector was used to conduct electromagnetic radiation shielding tests on two fabrics, and also on the computer, the first fabric, and the second fabric. Turn on the power switch of the instrument, select the high frequency (High) button as required, and gradually approach the object to be measured with the handheld instrument to start the measurement. The specific steps are: first use the electromagnetic radiation detector to aim at the computer screen to measure the computer radiation value, and then use the first fabric, the second fabric, and the aluminum-covered fabric to block the computer screen in turn, and measure the computer radiation value at this time.

[0070] The above test results are shown in Table 2;

[0071] Table 2 Test results of radiation protection performance of aluminum-coated fabrics (unit: mG)

[0072]

[0073] By observing the data in Table 2, it can be seen that the radiation protection performance of the aluminum-coated fabric of Comparative Example 1 is significantly reduced after friction, while the radiation protection performance of the aluminum-coated fabric of Example 1 is almost unchanged. The reason is that the aluminum foil on the surface of the aluminum-coated fabric is damaged after friction, resulting in reduced radiation protection performance of the aluminum-coated fabric. The aluminum-coated fabric of Comparative Example 1 has only an aluminum foil protective layer, while the aluminum-coated fabric of Example 1 has an aluminum film inside in addition to the aluminum foil protective layer, so it can fill the gap of the aluminum foil at the damaged part.

[0074] After folding, the radiation protection performance of the aluminum-clad fabric of comparative example 1 is significantly reduced, while the radiation protection performance of the aluminum-clad fabric of embodiment 1 is almost unchanged. The reason is that after folding, the aluminum foil on the surface of the aluminum-clad fabric is damaged, resulting in reduced radiation protection performance of the aluminum-clad fabric. The aluminum-clad fabric of comparative example 1 has only an aluminum foil protective layer, while the aluminum-clad fabric of embodiment 1 has an aluminum film inside in addition to the aluminum foil protective layer. Since the aluminum film is vacuum-plated on the surface of the first fabric, aluminum particles are dispersed into the gaps of the first fabric. Even if the aluminum foil is folded and damaged, the aluminum film inside has good protection performance, so it can fill the gap of the aluminum foil at the damaged part.

[0075] The protective form of the outer protective body (aluminum foil) + inner protective body (aluminum film) mentioned above achieves the folding and friction resistance of the aluminum-coated fabric, and the outer aluminum foil has a certain buffering effect when it is pulled by connecting the first fabric and the second fabric together, and because it has a strong breaking strength, it has a high peeling performance.

[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a folding-resistant and highly peelable aluminum-coated fabric, characterized in that: The steps include: Step 1: using plasma to etch the surface of the aluminum foil to form an etched surface, applying a coupling agent on the etched surface to form a coupling agent layer, applying a conductive adhesive on the coupling agent layer to form an adhesive layer, and pressing the first fabric on the adhesive layer to obtain an outer protective body; The conductive adhesive is formed by melting and mixing a hot-melt adhesive composed of a thermoplastic resin with a conductive filler and an additive; The thermoplastic resin includes a modified polyurethane with a melting point of 90°C-100°C, and the modified polyurethane includes a resin obtained by mixing and melting 70% of an ethylene-methyl acrylate copolymer and 30% of a thermoplastic polyurethane; The conductive filler includes at least one of 5-60nm nano-scale carbon black, carbon nanotubes, carbon fibers, and graphene, and the auxiliary agent includes acrylic acid; The first fabric is a polyester fabric that has been roughened with NaOH, ethylenediamine or alcohol solution; Step 2: vacuum-plating aluminum on one side of the first fabric to form an aluminum film, pasting a second fabric on one side of the aluminum film, sewing the first fabric and the second fabric together to obtain an aluminum-coated fabric, wherein the second fabric is a cloth fabric.

2. The method for preparing a folding-resistant and highly peelable aluminum-coated fabric according to claim 1, characterized in that: The aluminum foil is immersed in a 1%-3% sodium hydroxide solution for 20-40 minutes.

3. The method for preparing a folding-resistant and highly peelable aluminum-coated fabric according to claim 2, characterized in that: The plasma etches the surface of the aluminum foil at a speed of 3-6 cm / s and an input power of 200-500 W.

4. The method for preparing a folding-resistant and highly peelable aluminum-coated fabric according to claim 1, characterized in that: After the aluminum foil is plasma etched, it is left to stand in the air for 1-2 hours before being coated with a coupling agent.

5. The method for preparing a folding-resistant and highly peelable aluminum-coated fabric according to claim 1, characterized in that: The fabric density of the first fabric is (80-90)×(70-80) strands / inch.

6. Aluminum-coated fabric prepared by the preparation method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Recoverable fabric sleeve

    US4877660A

  • Transdermal pharmaceutical composition

    US5523094A