Silicon wafer retaining ring grinding liquid and preparation method thereof

By controlling the ratio and particle size of alumina and silica sol, combined with chemical etching and mechanical grinding, the prepared silicon wafer retaining ring polishing fluid solves the problems of scratches and poor dispersion of the silicon wafer retaining ring, achieving efficient polishing effects and environmentally friendly properties , suitable for the industrial production of silicon wafer retaining rings.

CN116082961BActive Publication Date: 2024-10-15NINGBO PINGHENG ELECTRONICS MATERIALS CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202211532466.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2024-10-15
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

The existing silicon wafer retaining ring polishing fluid has the problems of poor dispersion, high cost, not suitable for polishing PPS silicon wafer retaining rings, and cannot effectively eliminate scratches on the silicon wafer retaining rings, affecting the polishing quality.

Method used

By controlling the ratio and particle size of alumina and silica sol, combined with chemical etching and mechanical grinding, a silicon wafer retaining ring polishing fluid without adding oxidant was prepared, the pH value was adjusted to 3.9-4.1, and deionized water, dispersant and Bactericide, forming a green and environmentally friendly grinding fluid with excellent grinding effect.

Benefits of technology

It can effectively eliminate scratches on the silicon wafer retaining ring, improve flatness and surface gloss, reduce abrasive settling speed, avoid hardening, improve production efficiency, reduce costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a silicon wafer retaining ring grinding liquid and a preparation method thereof. The silicon wafer retaining ring grinding liquid is composed of the following raw materials in terms of mass percentage: 34-80wt% deionized water, 2.3-10wt% alumina, 1.5-5wt% dispersant, 16-50wt% silica sol, and 0.2-1wt% bactericide; the total mass percentage of the raw materials is 100%; and a pH regulator is used to adjust the pH value of the silicon wafer retaining ring grinding liquid to 3.9-4.1. The present invention controls the ratio and particle size of abrasive alumina and silica sol, and the obtained silicon wafer retaining ring grinding liquid can effectively improve the flatness and surface gloss of the silicon wafer retaining ring, while avoiding the caking phenomenon of the silicon wafer retaining ring grinding liquid when it is placed for a long time, and the grinding liquid has good dispersibility; in addition, no additives such as oxidants are added, and it has the characteristics of green environmental protection and low raw material cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical mechanical polishing, and in particular to a silicon wafer retaining ring grinding liquid and a preparation method thereof. Background Art

[0002] Chemical mechanical polishing (CMP) technology is a technology that combines chemical etching and mechanical grinding. By applying pressure to the polishing liquid, the polishing workpiece is forced to reciprocate relative to the polishing pad. With the help of the grinding effect of nanoparticles, a high-quality smooth surface is formed on the surface of the polished workpiece. Compared with chemical polishing, it is not easy to produce surface unevenness and poor polishing consistency, and compared with mechanical polishing, it will not cause defects such as surface damage.

[0003] In chemical mechanical polishing equipment, a silicon wafer retaining ring is usually used to fix the silicon wafer to the bottom end of the grinding head. The lower surface of the silicon wafer faces the grinding pad. The grinding liquid flows through the retaining ring to the interface between the grinding pad and the silicon wafer. When the retaining ring rotates, the silicon wafer is also driven to rotate, so that the lower surface of the silicon wafer rotates relative to the surface of the grinding pad and is ground and polished. Since the retaining ring is also polished together with the silicon wafer, it is very easy to produce scratches on the surface of the silicon wafer retaining ring.

[0004] CN 211103391U discloses a chemical mechanical grinding ring, comprising a first annular portion and a second annular portion, wherein the material of the first annular portion may be stainless steel, and the material of the second annular portion may be high-grade plastic, such as PPS (polyphenylene sulfide). The second annular portion comprises an inner annular surface, an outer annular surface and a lower surface, wherein the lower surface is located between the inner annular surface and the outer annular surface. The second annular portion further comprises a plurality of drainage grooves, each of which has an inner opening, an outer opening, a lower opening and a groove bottom surface, wherein the inner opening is located on the inner annular surface, the outer opening is located on the outer annular surface, the lower opening is located on the lower surface, the groove bottom surface is relative to the lower opening, wherein the width of the cross section of each drainage groove gradually expands from the lower opening toward the groove bottom surface. The grinding ring disclosed in the utility model can ensure the efficiency of the discharge of the grinding liquid, but the friction scratches generated on the surface of the grinding ring cannot be effectively eliminated, which will further reduce the polishing quality of the silicon wafer.

[0005] CN 107717639A provides a method for controlling the flatness of a retaining ring, a retaining ring produced, and a semiconductor manufacturing system. The method comprises the following steps: turning the base disc surface of the retaining ring, and then grinding the base disc surface; turning the resin surface of the retaining ring, and then grinding the resin surface. It can be seen that the present invention increases the grinding of the base disc surface of the retaining ring, so that before the resin surface of the retaining ring is processed, the flatness of the base disc surface as the base is basically consistent, and then the resin surface is turned, so that the flatness of the finished resin surface after turning meets the flatness requirements of semiconductor consumables. The invention controls the flatness of the retaining ring by machining methods, and cannot effectively solve surface damage and scratches.

[0006] Silicon wafer retaining rings are usually made of standard special engineering plastic PPS. Most PPS grinding fluids have the problem of poor dispersibility, and the addition of additives containing metal ions will reduce the polishing quality. At the same time, the existing PPS grinding fluids are mostly used for polishing ordinary PPS products and are not suitable for polishing PPS silicon wafer retaining rings.

[0007] In view of the shortcomings of the existing technology, it is necessary to provide a silicon wafer retaining ring grinding liquid with good grinding effect, good dispersibility, green environmental protection and low cost. Summary of the invention

[0008] The purpose of the present invention is to provide a silicon wafer retaining ring grinding liquid and a preparation method thereof. Based on the perspective of mechanical and chemical balance, the silicon wafer retaining ring grinding liquid is prepared by controlling the ratio and particle size of the abrasive without adding any additional oxidant. The obtained grinding liquid is green, environmentally friendly, has good dispersibility, and has excellent grinding effect.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In the first aspect, the present invention provides a silicon wafer retaining ring grinding liquid, which is composed of the following raw materials in terms of mass percentage: 34-80wt% deionized water, 2.3-10wt% alumina, 1.5-5wt% dispersant, 16-50wt% silica sol, and 0.2-1wt% bactericide; the total mass percentage of the raw materials is 100%; and the pH value of the silicon wafer retaining ring grinding liquid is adjusted to 3.9-4.1 by using a pH adjuster.

[0011] The silicon wafer retaining ring grinding liquid provided by the present invention selects a suitable ratio of aluminum oxide to silica sol, cooperates with chemical corrosion, and performs grinding and repairing simultaneously. Textures are ground out by aluminum oxide, and the surface is repaired by silica sol. Chemical additives accelerate the reaction process. The prepared silicon wafer retaining ring grinding liquid can effectively eliminate scratches on the silicon wafer retaining ring, improve its flatness and surface gloss, and at the same time does not add additives such as oxidants. It has the characteristics of being green and environmentally friendly. In addition, the raw material cost is low, and it is suitable for large-scale industrial production.

[0012] The mass percentage of deionized water in the silicon wafer retaining ring grinding liquid is 34-80wt%, for example, it can be 34wt%, 47wt%, 60wt%, 70wt% or 80wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] The mass percentage of aluminum oxide in the silicon wafer retaining ring grinding liquid is 2.3-10wt%, for example, it can be 2.3wt%, 3wt%, 5wt%, 8wt% or 10wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] The mass percentage of the dispersant in the silicon wafer retaining ring grinding liquid is 1.5-5wt%, for example, it can be 1.5wt%, 1.7wt%, 2.5wt%, 4.2wt% or 5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] The mass percentage of silica sol in the silicon wafer retaining ring grinding liquid is 16-50wt%, for example, it can be 16wt%, 25wt%, 32wt%, 40wt% or 50wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] The mass percentage of the bactericide in the silicon wafer retaining ring grinding liquid is 0.2-1wt%, for example, it can be 0.2wt%, 0.3wt%, 0.5wt%, 0.8wt% or 1wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] The pH value of the silicon wafer retaining ring grinding liquid is adjusted to 3.9-4.1, for example, it can be 3.9, 3.95, 4, 4.05 or 4.1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] Preferably, the total mass percentage of the aluminum oxide and the silica sol is 20-60wt%, for example, 20wt%, 30wt%, 40wt%, 50wt% or 60wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] When the total mass percentage of the alumina and the silica sol is within a reasonable range, the obtained silicon wafer retaining ring grinding liquid has a better grinding effect. If the total mass percentage is too high or too low, the surface gloss and flatness of the silicon wafer retaining ring will be reduced, thereby reducing the grinding effect.

[0020] Preferably, the particle size of the silica sol is 80-140 nm, for example, 80 nm, 90 nm, 100 nm, 120 nm or 140 nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0021] Preferably, the particle size of the aluminum oxide is 0.95-1.05 μm, for example, 0.95 μm, 0.98 μm, 1 μm, 1.02 μm or 1.05 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] By selecting lower particle sizes of silica sol and alumina, the settling speed of the abrasive is reduced, and the abrasive liquid of the silicon wafer retaining ring is prevented from being hardened when placed for a long time. The steps of pure water washing are reduced, the production efficiency is improved and the cost is reduced.

[0023] Preferably, the dispersant comprises alkyl aryl phosphate and / or sodium polyacrylate.

[0024] Preferably, the fungicide comprises 2-methyl-4-isothiazoline-3-one and / or 1,2-phenylisothiazoline-3-one.

[0025] Preferably, the concentration of the pH regulator is 1-2 mol / L, for example, 1 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L or 2 mol / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the pH adjuster comprises any one of nitric acid, hydrochloric acid or oxalic acid or a combination of at least two thereof, and typical but non-limiting combinations include a combination of nitric acid and hydrochloric acid, a combination of hydrochloric acid and oxalic acid, or a combination of nitric acid, hydrochloric acid and oxalic acid.

[0027] In a second aspect, the present invention provides a method for preparing the silicon wafer retaining ring grinding liquid as described in the first aspect, the preparation method comprising the following steps:

[0028] Alumina and deionized water are uniformly mixed to obtain an alumina solution; a dispersant is added to the obtained alumina solution for a first mixing, and then silica sol is added for a second mixing, and then a bactericide is added for a third mixing, and a pH adjuster is used to adjust the pH value of the solution to 3.9-4.1. The obtained mixed solution is filtered and packaged to obtain the silicon wafer retaining ring grinding liquid.

[0029] The present invention pre-disperses abrasive aluminum oxide in deionized water to improve the dispersion effect of the abrasive in the solution and reduce the caking phenomenon, then adds abrasive silica sol and a bactericide in steps to ensure the dispersibility of the solution, and then uses a pH regulator to adjust the pH value of the solution. The obtained silicon wafer retaining ring grinding liquid has good suspension properties; at the same time, no oxidant is added during the preparation, and the grinding liquid is green and environmentally friendly.

[0030] Preferably, the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-grade cleanroom.

[0031] The preparation of the silicon wafer retaining ring grinding liquid needs to be carried out in a high cleanliness environment to avoid the introduction of impurities to contaminate the grinding liquid and cause significant damage to the silicon wafer surface.

[0032] Preferably, the uniform mixing, the first mixing, the second mixing and the third mixing are all carried out in a 1T reactor.

[0033] Preferably, the rotation speed of the uniform mixing is 38-42 r / min, for example, it can be 38 r / min, 39 r / min, 40 r / min, 41 r / min or 42 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the rotation speed of the first mixing is 38-42 r / min, for example, it can be 38 r / min, 39 r / min, 40 r / min, 41 r / min or 42 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the first mixing time is 15-20 min, for example, 15 min, 16 min, 18 min, 19 min or 20 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the rotation speed of the second mixing is 38-42 r / min, for example, it can be 38 r / min, 39 r / min, 40 r / min, 41 r / min or 42 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the second mixing time is 15-20 min, for example, 15 min, 16 min, 18 min, 19 min or 20 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the rotation speed of the third mixing is 38-42 r / min, for example, it can be 38 r / min, 39 r / min, 40 r / min, 41 r / min or 42 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the third mixing time is 15-20 min, for example, 15 min, 16 min, 18 min, 19 min or 20 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the filtration uses a double-stage filter element.

[0041] As a preferred technical solution of the preparation method described in the second aspect of the present invention, the preparation method comprises the following steps:

[0042] Alumina and deionized water are uniformly mixed in a 1T reactor at a rotation speed of 38-42r / min to obtain an alumina solution; a dispersant is added to the obtained alumina solution and mixed for a first time at a rotation speed of 38-42r / min for 15-20min, and then silica sol is added and mixed for a second time at a rotation speed of 38-42r / min for 15-20min, and then a bactericide is added and mixed for a third time at a rotation speed of 38-42r / min for 15-20min, and a pH adjuster is used to adjust the pH value of the solution to 3.9-4.1, and the obtained mixed solution is filtered and packaged through a double-stage filter element to obtain the silicon wafer retaining ring grinding liquid; the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-class purification workshop.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] The silicon wafer retaining ring grinding liquid provided by the present invention can effectively eliminate scratches on the silicon wafer retaining ring, improve its flatness and surface gloss, and achieve a roughness of less than 100nm by controlling the ratio and particle size of abrasive aluminum oxide and silica sol. At the same time, the settling speed of the abrasive is reduced, thereby avoiding the caking of the silicon wafer retaining ring grinding liquid when it is placed for a long time, reducing the step of pure water rinsing, and having good dispersibility of the grinding liquid, thereby improving production efficiency and saving water resources. In addition, no additives such as oxidants are added, and the grinding liquid has the characteristics of being green, environmentally friendly, and having low raw material costs. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0046] Example 1

[0047] The present embodiment provides a silicon wafer retaining ring grinding liquid, which is composed of the following raw materials in terms of mass percentage: 60wt% deionized water, 5wt% aluminum oxide, 2.5wt% sodium polyacrylate, 32wt% silica sol, 0.5wt% 1,2-phenylisothiazoline-3-one, and nitric acid; the total mass percentage of the aluminum oxide and the silica sol is 37wt%; the particle size of the silica sol is 100-120nm; the particle size of the aluminum oxide is 0.99-1.02μm;

[0048] The method for preparing the silicon wafer retaining ring grinding liquid comprises the following steps:

[0049] Alumina and deionized water are uniformly mixed in a 1T reactor at a speed of 40 r / min to obtain an alumina solution; sodium polyacrylate is added to the obtained alumina solution and mixed for a first time at a speed of 40 r / min for 18 minutes, and then silica sol is added and mixed for a second time at a speed of 40 r / min for 18 minutes, and then 1,2-phenylisothiazoline-3-one is added and mixed for a third time at a speed of 40 r / min for 18 minutes, and nitric acid with a concentration of 1.5 mol / L is used to adjust the pH value of the solution to 4, and the obtained mixed solution is filtered and packaged through a double-stage filter element to obtain the silicon wafer retaining ring grinding liquid; the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-class purification workshop.

[0050] Example 2

[0051] The present embodiment provides a silicon wafer retaining ring grinding liquid, which is composed of the following raw materials in terms of mass percentage: 47wt% deionized water, 8wt% aluminum oxide, 4.2wt% sodium polyacrylate, 40wt% silica sol, 0.8wt% 1,2-phenylisothiazoline-3-one, and nitric acid; the total mass percentage of the aluminum oxide and the silica sol is 48wt%; the particle size of the silica sol is 90-110nm; the particle size of the aluminum oxide is 0.97-1μm;

[0052] The method for preparing the silicon wafer retaining ring grinding liquid comprises the following steps:

[0053] Alumina and deionized water are uniformly mixed in a 1T reactor at a speed of 39 r / min to obtain an alumina solution; sodium polyacrylate is added to the obtained alumina solution and mixed for a first time at a speed of 39 r / min for 19 minutes, and then silica sol is added and mixed for a second time at a speed of 39 r / min for 19 minutes, and then 1,2-phenylisothiazoline-3-one is added and mixed for a third time at a speed of 39 r / min for 19 minutes, and the pH value of the solution is adjusted to 4.05 with nitric acid with a concentration of 1.2 mol / L. The obtained mixed solution is filtered and packaged through a double-stage filter element to obtain the silicon wafer retaining ring grinding liquid; the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-class purification workshop.

[0054] Example 3

[0055] The present embodiment provides a silicon wafer retaining ring grinding liquid, which is composed of the following raw materials in terms of mass percentage: 70wt% deionized water, 3wt% aluminum oxide, 1.7wt% sodium polyacrylate, 25wt% silica sol, 0.3wt% 1,2-phenylisothiazoline-3-one, and nitric acid; the total mass percentage of the aluminum oxide and the silica sol is 28wt%; the particle size of the silica sol is 110-130nm; the particle size of the aluminum oxide is 1.01-1.03μm;

[0056] The method for preparing the silicon wafer retaining ring grinding liquid comprises the following steps:

[0057] Alumina and deionized water are uniformly mixed in a 1T reactor at a speed of 41r / min to obtain an alumina solution; sodium polyacrylate is added to the obtained alumina solution and mixed for a first time at a speed of 41r / min for 16min, and then silica sol is added and mixed for a second time at a speed of 41r / min for 16min, and then 1,2-phenylisothiazoline-3-one is added and mixed for a third time at a speed of 41r / min for 16min, and nitric acid with a concentration of 1.8mol / L is used to adjust the pH value of the solution to 3.95, and the obtained mixed solution is filtered and packaged through a double-stage filter element to obtain the silicon wafer retaining ring grinding liquid; the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-class purification workshop.

[0058] Example 4

[0059] The present embodiment provides a silicon wafer retaining ring grinding liquid, which is composed of the following raw materials in terms of mass percentage: 34wt% deionized water, 10wt% alumina, 5wt% sodium polyacrylate, 50wt% silica sol, 1wt% 1,2-phenylisothiazoline-3-one, and nitric acid; the total mass percentage of the alumina and the silica sol is 60wt%; the particle size of the silica sol is 80-100nm; the particle size of the alumina is 0.95-0.98μm;

[0060] The method for preparing the silicon wafer retaining ring grinding liquid comprises the following steps:

[0061] Alumina and deionized water are uniformly mixed in a 1T reactor at a speed of 38 r / min to obtain an alumina solution; sodium polyacrylate is added to the obtained alumina solution and mixed for a first time at a speed of 38 r / min for 20 minutes, and then silica sol is added and mixed for a second time at a speed of 38 r / min for 20 minutes, and then 1,2-phenylisothiazoline-3-one is added and mixed for a third time at a speed of 38 r / min for 20 minutes, and nitric acid with a concentration of 1 mol / L is used to adjust the pH value of the solution to 4.1, and the obtained mixed solution is filtered and packaged through a double-stage filter element to obtain the silicon wafer retaining ring grinding liquid; the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-class purification workshop.

[0062] Example 5

[0063] The present embodiment provides a silicon wafer retaining ring grinding liquid, which is composed of the following raw materials in terms of mass percentage: 80wt% deionized water, 2.3wt% alumina, 1.5wt% sodium polyacrylate, 16wt% silica sol, 0.2wt% 1,2-phenylisothiazoline-3-one, and nitric acid; the total mass percentage of the alumina and the silica sol is 18.3wt%; the particle size of the silica sol is 120-140nm; the particle size of the alumina is 1.03-1.05μm;

[0064] The method for preparing the silicon wafer retaining ring grinding liquid comprises the following steps:

[0065] Alumina and deionized water are uniformly mixed in a 1T reactor at a speed of 42 r / min to obtain an alumina solution; sodium polyacrylate is added to the obtained alumina solution and mixed for a first time at a speed of 42 r / min for 15 minutes, and then silica sol is added and mixed for a second time at a speed of 42 r / min for 15 minutes, and then 1,2-phenylisothiazoline-3-one is added and mixed for a third time at a speed of 42 r / min for 15 minutes, and nitric acid with a concentration of 2 mol / L is used to adjust the pH value of the solution to 3.9, and the obtained mixed solution is filtered and packaged through a double-stage filter element to obtain the silicon wafer retaining ring grinding liquid; the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-class purification workshop.

[0066] Example 6

[0067] This embodiment provides a silicon wafer retaining ring grinding liquid, which is different from Embodiment 1 in that, except for adjusting the particle size of the silica sol to 150-170 nm, the rest is the same as Embodiment 1.

[0068] Example 7

[0069] This embodiment provides a silicon wafer retaining ring grinding liquid, which is different from Embodiment 1 in that, except that the particle size of the aluminum oxide is adjusted to 1.5-1.6 μm, the rest is the same as Embodiment 1.

[0070] Example 8

[0071] This embodiment provides a silicon wafer retaining ring grinding liquid. The preparation method of the silicon wafer retaining ring grinding liquid is different from that of Example 1 in that aluminum oxide, deionized water, sodium polyacrylate, silica sol and 1,2-phenylisothiazoline-3-one are uniformly mixed at a speed of 40 r / min without step-by-step mixing. The rest is the same as Example 1.

[0072] Example 9

[0073] This embodiment provides a silicon wafer retaining ring grinding liquid. The difference between the preparation method of the silicon wafer retaining ring grinding liquid and that of Example 1 is that the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 10,000-level cleanroom, and the rest is the same as Example 1.

[0074] Example 10

[0075] This embodiment provides a silicon wafer retaining ring grinding liquid, which is different from Example 1 in that the sodium polyacrylate is replaced with sodium dodecylbenzene sulfonate, and the rest is the same as Example 1.

[0076] Comparative Example 1

[0077] This comparative example provides a silicon wafer retaining ring grinding liquid, which differs from Example 1 in that nitric acid is replaced by sodium hydroxide solution, and the amount of sodium hydroxide solution added is adaptively adjusted so that the pH value of the silicon wafer retaining ring grinding liquid is 10, and the rest is the same as Example 1.

[0078] Comparative Example 2

[0079] This comparative example provides a silicon wafer retaining ring grinding liquid, which is different from Example 1 in that the silicon wafer retaining ring grinding liquid contains: 90wt% deionized water, 1wt% aluminum oxide, 1wt% sodium polyacrylate, 7.9wt% silica sol, and 0.1wt% 1,2-phenylisothiazoline-3-one. The total mass percentage of the aluminum oxide and the silica sol is 8.9wt%, and the rest is the same as Example 1.

[0080] Comparative Example 3

[0081] This comparative example provides a silicon wafer retaining ring grinding liquid, which is different from Example 1 in that the silicon wafer retaining ring grinding liquid contains: 18wt% deionized water, 12wt% aluminum oxide, 8wt% sodium polyacrylate, 60wt% silica sol, and 2wt% 1,2-phenylisothiazoline-3-one. The total mass percentage of the aluminum oxide and the silica sol is 72wt%, and the rest is the same as Example 1.

[0082] The silicon wafer retaining ring grinding liquids provided in Examples 1-10 and Comparative Examples 1-3 were subjected to grinding tests, and the obtained glossiness, flatness and roughness are shown in Table 1, wherein the glossiness results are divided into "bright", "relatively bright" and "dark";

[0083] The silicon wafer retaining ring grinding liquid provided in Examples 1-10 and Comparative Examples 1-3 was placed in a container. The dispersion was judged by observing the adsorption of powder at the bottom of the container while pouring the liquid. The dispersion results were divided into "good", "relatively good" and "poor". The results are shown in Table 1.

[0084] Table 1

[0085] Glossiness Flatness(wire) Roughness(nm) Dispersibility Example 1 Bright 0.07 <100 good Example 2 Bright 0.08 <100 good Example 3 Bright 0.09 <100 good Example 4 Bright 0.10 <100 good Example 5 Bright 0.11 <100 good Example 6 Brighter 0.08 <100 better Example 7 Bright 0.15 <100 better Example 8 Bright 0.12 <100 better Example 9 Bright 0.08 <100 good Example 10 Bright 0.18 <100 Difference Comparative Example 1 Brighter 1.5 <100 good Comparative Example 2 dark 0.17 <100 good Comparative Example 3 dark 0.07 120 good

[0086] It can be seen from Table 1 that the silicon wafer retaining ring grinding liquid provided by the present invention is green and environmentally friendly and has good dispersibility. The surface of the silicon wafer retaining ring is ground to have good glossiness and flatness;

[0087] By comparing Example 1 with Examples 6 and 7, it can be seen that the particle size of silica sol or alumina is too large, the powder settles quickly, and will be adsorbed on the bottom of the container in large quantities, and the dispersibility of the grinding liquid is reduced; by comparing Example 1 with Example 8, it can be seen that when no step-by-step mixing is performed, the raw materials agglomerate together, and the effect of dispersion in deionized water is significantly reduced; by comparing Example 1 with Example 9, it can be seen that when preparing the silicon wafer retaining ring grinding liquid in a 10,000-level cleanroom, impurities are easily introduced into the grinding liquid to cause pollution, thereby reducing the grinding effect; by comparing Example 1 with Example 10, it can be seen that compared with the sodium polyacrylate of the present application, the dispersion effect is significantly reduced;

[0088] By comparing Example 1 with Comparative Example 1, it can be seen that by using an alkaline pH regulator to adjust the pH of the silicon wafer retaining ring grinding liquid, the flatness of the silicon wafer retaining ring is significantly reduced after grinding; by comparing Example 1 with Comparative Examples 2 and 3, it can be seen that the ratio of powder to solvent in the raw material needs to be controlled within a reasonable range in order to obtain a grinding liquid with good dispersibility and grinding effect. Too high a powder content or too high a solvent content will bring adverse effects.

[0089] To summarize, the silicon wafer retaining ring grinding liquid provided by the present invention can effectively eliminate scratches on the silicon wafer retaining ring, improve its flatness and surface gloss, and achieve a roughness of <100nm by controlling the ratio and particle size of abrasive aluminum oxide and silica sol. It also reduces the settling rate of the abrasive, thereby avoiding the hardening of the silicon wafer retaining ring grinding liquid when it is placed for a long time, reduces the step of pure water rinsing, has good dispersibility, improves production efficiency and saves water resources. In addition, no additives such as oxidants are added, and the system has the characteristics of being green, environmentally friendly and having low raw material costs.

[0090] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A silicon wafer retaining ring grinding liquid, characterized in that: The silicon wafer retaining ring grinding liquid is composed of the following raw materials in terms of mass percentage: 34-80wt% of deionized water, 2.3-10wt% of aluminum oxide, 1.5-5wt% of a dispersant, 16-50wt% of silica sol, and 0.2-1wt% of a bactericide; the total mass percentage of the raw materials is 100%; the pH value of the silicon wafer retaining ring grinding liquid is adjusted to 3.9-4.1 by using a pH adjuster; The total mass percentage of the alumina and the silica sol is 37-60wt%; The particle size of the aluminum oxide is 0.95-1.05 μm; The dispersant includes alkyl aryl phosphate and / or sodium polyacrylate; The particle size of the silica sol is 80-140nm; The silicon wafer retaining ring grinding liquid is prepared by the following method, which comprises the following steps: Alumina and deionized water are uniformly mixed to obtain an alumina solution; a dispersant is added to the obtained alumina solution for a first mixing, and then silica sol is added for a second mixing, and then a bactericide is added for a third mixing, and a pH adjuster is used to adjust the pH value of the solution to 3.9-4.

1. The obtained mixed solution is filtered and packaged to obtain the silicon wafer retaining ring grinding liquid.

2. The silicon wafer retaining ring grinding liquid according to claim 1, characterized in that: The fungicide comprises 2-methyl-4-isothiazoline-3-one and / or 1,2-phenylisothiazoline-3-one.

3. The silicon wafer retaining ring grinding liquid according to claim 1, characterized in that: The concentration of the pH regulator is 1-2 mol / L.

4. The silicon wafer retaining ring grinding liquid according to claim 1, characterized in that: The pH adjuster includes any one of nitric acid, hydrochloric acid or oxalic acid, or a combination of at least two of them.

5. A method for preparing a silicon wafer retaining ring grinding liquid as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Alumina and deionized water are uniformly mixed to obtain an alumina solution; a dispersant is added to the obtained alumina solution for a first mixing, and then silica sol is added for a second mixing, and then a bactericide is added for a third mixing, and a pH adjuster is used to adjust the pH value of the solution to 3.9-4.

1. The obtained mixed solution is filtered and packaged to obtain the silicon wafer retaining ring grinding liquid.

6. The preparation method according to claim 5, characterized in that: The preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-level purification workshop.

7. The preparation method according to claim 5, characterized in that: The uniform mixing, the first mixing, the second mixing and the third mixing are all carried out in a 1T reactor.

8. The preparation method according to claim 5, characterized in that: The rotation speed of the uniform mixing is 38-42 r / min.

9. The preparation method according to claim 5, characterized in that: The rotation speed of the first mixing is 38-42 r / min.

10. The preparation method according to claim 5, characterized in that: The first mixing time is 15-20 minutes.

11. The preparation method according to claim 5, characterized in that: The rotation speed of the second mixing is 38-42 r / min.

12. The preparation method according to claim 5, characterized in that: The second mixing time is 15-20 minutes.

13. The preparation method according to claim 5, characterized in that: The rotation speed of the third mixing is 38-42 r / min.

14. The preparation method according to claim 5, characterized in that: The third mixing time is 15-20 minutes.

15. The preparation method according to claim 5, characterized in that: The filtration adopts a double-stage filter element.

16. The preparation method according to claim 5, characterized in that: The preparation method comprises the following steps: Alumina and deionized water are uniformly mixed in a 1T reactor at a rotation speed of 38-42r / min to obtain an alumina solution; a dispersant is added to the obtained alumina solution and mixed for a first time at a rotation speed of 38-42r / min for 15-20min, and then silica sol is added and mixed for a second time at a rotation speed of 38-42r / min for 15-20min, and then a bactericide is added and mixed for a third time at a rotation speed of 38-42r / min for 15-20min, and a pH adjuster is used to adjust the pH value of the solution to 3.9-4.1, and the obtained mixed solution is filtered and packaged through a double-stage filter element to obtain the silicon wafer retaining ring grinding liquid; the preparation of the silicon wafer retaining ring grinding liquid is carried out in a 100,000-class purification workshop.

Citation Information

Patent Citations

  • Method for controlling retaining ring planeness and produced retaining ring and semiconductor manufacturing system

    CN107717639A

  • Chemical mechanical polishing ring

    CN211103391U

  • Silicon slice grinding rate control method

    CN101367194A

  • Sapphire wafer polishing solution

    CN104356950A

  • Grinding method for wafer locating ring, wafer locating ring and application thereof and chemical-mechanical polishing device of wafer locating ring

    CN108857860A