Method and system for producing nickel matte from nickel-containing solid waste

By combining an oxygen-rich side-blown bath melting furnace with an electric-heated settling furnace, the problem of small scale, complexity, and environmental pollution of blast furnaces in processing nickel-containing solid waste has been solved, and efficient and continuous nickel matte production has been achieved, reducing costs and environmental pollution. .

CN116083737BActive Publication Date: 2024-10-22CHINA ENFI ENG CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310040284.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-13
Publication Date
2024-10-22
Estimated Expiration
2043-01-13

AI Technical Summary

Technical Problem

Existing blast furnaces for treating nickel-containing solid waste have problems such as small processing scale, complex material preparation, low fuel thermal efficiency and large environmental pollution. In particular, the large amount of carbon monoxide contained in the flue gas has a great impact on the environment.

Method used

Using a method that combines an oxygen-rich side-blown molten pool smelting furnace with an electric-heated settling furnace, the nickel-containing solid waste is vulcanized with a vulcanizing agent and a reducing agent, and energy and oxygen-rich air are blown into the melt through a lance to stir it to generate a mixed melt. After solidification, it directly flows into the electric settling furnace for settling and separation of nickel matte and slag. The electric settling furnace is used to achieve efficient, continuous and stable process operation.

Benefits of technology

It improves the recovery efficiency of nickel matte and the continuity of the process, reduces environmental pollution, reduces the low thermal efficiency of fuel and the formation of frozen layer of alloy on the furnace bottom, and reduces investment and operating costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116083737B_ABST
    Figure CN116083737B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of nickel-containing solid waste treatment, and discloses a method and system for producing nickel matte from nickel-containing solid waste. The method comprises: mixing and drying nickel-containing solid waste and a vulcanizing agent; mixing the dried material with a reducing agent and a flux and sending the dried material into an oxygen-enriched side-blown molten pool smelting furnace for vulcanization reaction to obtain a mixed melt; a spray gun is provided on the side of the oxygen-enriched side-blown molten pool smelting furnace, and energy and oxygen-enriched air / pure oxygen are blown into the furnace through the spray gun to stir the mixed melt; the mixed melt flows directly from the discharge port of the oxygen-enriched side-blown molten pool smelting furnace through a chute into an electric thermal settling furnace for settling and separation of nickel matte and slag, and discharges nickel matte and slag. The present invention combines an oxygen-enriched side-blown molten pool smelting furnace with an electric thermal settling furnace, wherein the oxygen-enriched side-blown molten pool smelting furnace only performs smelting without separation, and the spray gun stirs violently to fully carry out the reaction, and the produced mixed melt flows directly into the electric thermal settling furnace to calmly separate nickel matte and slag, thereby ensuring efficient, continuous and stable operation of the process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nickel-containing solid waste treatment, and in particular to a method and system for producing nickel matte from nickel-containing solid waste. Background Art

[0002] HW46 Nickel-containing wastes mainly come from the basic chemical raw material manufacturing and battery manufacturing industries, including reaction residues, unqualified, obsolete and discarded products generated in the production process of nickel compounds; waste slag and wastewater treatment sludge generated in the production process of nickel-hydrogen batteries, and discarded nickel catalysts.

[0003] The recycling and treatment of nickel-containing solid waste is mainly based on the wet method. With the rapid development of new energy vehicles, the recycling and reuse technology of nickel-containing solid waste has gradually gained attention. The pyrometallurgical smelting of nickel-containing solid waste produces low-nickel matte, which is then blown into high-nickel matte. The slag produced by smelting is general solid waste, which has been recognized by the industry. Therefore, it is of great significance to develop a simple, efficient and stable new pyrometallurgical smelting technology for nickel-containing solid waste.

[0004] At present, some documents use blast furnace smelting technology, after calcium sulfate, nickel-containing solid waste and other materials are mixed to make bricks, low-nickel matte with high iron content and low sulfur content is obtained by blast furnace smelting, and then high-nickel matte is smelted to produce nickel sulfate. For example, Chinese application publication number CN108950215A discloses a method for treating low-grade nickel-containing waste, which dehydrates and dries the nickel-containing waste, presses the dried nickel-containing waste into bricks, and smelts the obtained nickel-containing waste bricks in an oxygen-enriched blast furnace to obtain nickel matte and slag, and casts the matte into anode plates, and electrolyzes the anode plates by diaphragm electrolysis to obtain metallic nickel and nickel electrolysis waste liquid, which can treat low-grade nickel-containing waste, and the nickel recovery rate can reach more than 95%.

[0005] In summary, the existing blast furnace for treating nickel-containing solid waste has the following disadvantages: (1) The treatment scale is small; (2) The material preparation is complicated and needs to be dried after brick making; (3) The oxygen enrichment concentration is about 32%, and the fuel is coke, and the fuel thermal efficiency is not high; (4) The flue gas contains a large amount of carbon monoxide, which has a great impact on the environment and has become the most fatal factor in the existence of this process. Summary of the invention

[0006] According to one embodiment of the present invention, the object is to provide a method and system for producing nickel matte from nickel-containing solid waste. The above object can be achieved by the following technical solution:

[0007] According to one aspect of the present invention, the present invention provides a method for producing nickel matte from nickel-containing solid waste, comprising:

[0008] Mixing nickel-containing solid waste and sulfiding agent and drying;

[0009] The dried material, reducing agent and flux ingredients are sent to an oxygen-enriched side-blown molten pool smelting furnace for sulfidation reaction to obtain a mixed melt; wherein a spray gun is provided on the side of the oxygen-enriched side-blown molten pool smelting furnace, and the spray gun is 300mm to 400mm away from the furnace bottom, and energy and oxygen-enriched air / pure oxygen are blown into the furnace through the spray gun, and the mixed melt is stirred;

[0010] The mixed melt flows directly from the discharge port of the oxygen-enriched side-blown molten pool smelting furnace through the chute into the electric thermal settling furnace for sedimentation and separation of nickel matte and slag. The nickel matte is discharged from the nickel matte discharge port, and the slag is discharged from the slag discharge port.

[0011] Optionally, the oxygen-enriched side-blown molten pool smelting furnace adopts a "hearthless" form.

[0012] Optionally, the oxygen concentration of the oxygen-enriched air is ≥60%, and the pressure of the blown gas is 0.1 MPa to 0.35 MPa.

[0013] Optionally, during the vulcanization reaction, the furnace temperature is 1300°C to 1450°C.

[0014] Optionally, the discharge port of the oxygen-enriched side-blown molten pool smelting furnace is siphon discharge or burn-eye discharge, wherein, when it is burn-eye discharge, the slag surface exceeds the slag port by more than 100 mm.

[0015] Optionally, drying is performed to a moisture content of no more than 10%.

[0016] Optionally, the electric heat settling furnace has a settling separation time of 2 to 6 hours and a furnace operating temperature of 1300°C to 1500°C.

[0017] Optionally, the nickel matte discharge port of the electrothermal settling furnace is arranged at a position 100 mm away from the furnace bottom, and the slag discharge port is arranged at a position 500 to 600 mm high from the furnace bottom.

[0018] Optionally, the nickel matte is granulated by water and sold, and the slag is crushed by wind or water and sold as general solid waste. If the nickel matte product contains more than 10% iron, the nickel matte is sent to an oxidation insulation furnace for blowing to remove the iron, and high-nickel matte with qualified iron content and blowing slag are produced. The high-nickel matte is granulated by water, and the blowing slag is returned to the electric thermal settling furnace.

[0019] Optionally, the oxygen-enriched side-blown molten pool smelting furnace is also provided with a group of electrodes for heat preservation of the melt in an emergency state.

[0020] Optionally, the furnace top of the oxygen-enriched side-blowing molten pool smelting furnace is higher than that of the electric thermal settling furnace, or is arranged at the same height as the electric thermal settling furnace.

[0021] Optionally, the vulcanizing agent is gypsum slag or sulfur-containing waste.

[0022] Optionally, the reducing agent is one or more of coke, graphite powder and carbon essence.

[0023] Optionally, the energy injected by the spray gun is one or more of natural gas, coal powder, and organic solvent.

[0024] According to another aspect of the present invention, a system for producing nickel matte from nickel-containing solid waste provided by the present invention comprises a drying furnace, an oxygen-enriched side-blown molten pool smelting furnace and an electric thermal settling furnace, wherein the drying furnace is used to dry the nickel-containing solid waste and the sulfiding agent batch after batching; the oxygen-enriched side-blown molten pool smelting furnace is used to receive the dried material after batching and the reducing agent and the flux and carry out a sulfidation reaction to obtain a mixed melt; a spray gun is provided on the side of the oxygen-enriched side-blown molten pool smelting furnace, the spray gun is 300mm to 400mm away from the furnace bottom, the spray gun is used to blow energy and oxygen-enriched air / pure oxygen into the furnace to stir the mixed melt; the inlet of the electric thermal settling furnace is connected to the discharge port of the oxygen-enriched side-blown molten pool smelting furnace through a chute, which is used to receive the mixed melt discharged from the discharge port, and to carry out sedimentation separation of nickel matte and slag, and discharge the nickel matte from the nickel matte discharge port and the slag from the slag discharge port.

[0025] Beneficial effect: According to the above-mentioned embodiment of the present invention, the oxygen-enriched side-blown molten pool smelting furnace and the electric thermal settling furnace are combined. The oxygen-enriched side-blown molten pool smelting furnace only performs smelting without separation, and the output mixed melt directly flows into the electric thermal settling furnace for calm separation of nickel matte and slag, thereby ensuring efficient, continuous and stable operation of the process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic flow chart of a method for producing nickel matte from nickel-containing solid waste in one embodiment of the present invention.

[0027] Figure 2 It is a schematic structural diagram of a side-blowing depletion furnace in one embodiment of the present invention. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Figure 1 The process of producing nickel matte from nickel-containing solid waste in one embodiment of the present invention is schematically shown. The method of producing nickel matte from nickel-containing solid waste in this embodiment comprises the following steps:

[0030] (1) After the nickel-containing solid waste and gypsum slag are mixed, they are added into a dryer and dried until the moisture content is no more than 10%. The gypsum slag used as the vulcanizing agent in this embodiment is certainly not limited thereto, and other sulfur-containing waste materials may also be used.

[0031] (2) The dried material is mixed with coke, quartz and limestone and then fed into an oxygen-enriched side-blown molten pool smelting furnace, i.e., a side-blown depletion furnace, for sulfidation reaction. In this embodiment, the reducing agent is coke, but it is certainly not limited thereto. The reducing agent may also be other C-containing materials such as graphite powder and carbon concentrate.

[0032] The main reaction equation of the sulfidation reaction process in the side-blowing depletion furnace is:

[0033] NiO+CaSO4+C→Ni3S2+CaO+CO(g)

[0034] Fe3O4+CaSO4+C→FeS+CaO+CO(g)

[0035] In addition to the sulfidation reaction, the following reduction reaction also occurs to produce Ni-Fe alloy:

[0036] NiO+C→Ni+CO(g)

[0037] Fe3O4+C→Fe+CO(g)

[0038] The oxygen-enriched side-blown molten pool smelting furnace adopts a "hearthless" form. A spray gun is arranged on the side of the oxygen-enriched side-blown molten pool smelting furnace. The spray gun is only about 300mm to 400mm away from the furnace bottom, for example, 400mm, which is relatively close to the furnace bottom. The spray gun is arranged at the above position. While providing heat to the furnace body, it can effectively improve the stirring effect and prevent the formation of an alloy freezing layer at the furnace bottom to cause a dead furnace. Natural gas and oxygen-enriched air (or 99.6% pure oxygen) are blown in, and the oxygen concentration of the oxygen-enriched air is ≥60%, specifically 60 to 99.6%, and the gas pressure is 0.1MPa to 0.35MPa.

[0039] The energy source blown into the spray gun is natural gas, which provides heat for the reaction. In addition to natural gas, it can also be other energy sources such as coal powder, organic flux, etc.; oxygen-enriched air is used as fuel to act as a combustion-supporting gas. In addition to oxygen-enriched air, it can also be pure oxygen. Natural gas and oxygen-enriched air (or pure oxygen) are blown into the side-blowing spray gun, but the amount of oxygen is insufficient for natural gas to prevent excess oxygen from oxidizing nickel matte.

[0040] The gas blown into the furnace body by the spray gun not only provides heat for the furnace body, but also strengthens the reaction kinetics through the blown natural gas and oxygen-enriched air or pure oxygen, so that the nickel-iron alloy that may be deposited can be stirred and lifted up for a second time to be fully mixed with the slag and undergo a sulfidation reaction, preventing the Ni-Fe alloy in the high-iron and low-sulfur nickel matte from being deposited at the bottom of the furnace, and preventing the "dead furnace" caused by the formation of an alloy freezing layer at the bottom of the furnace. The nickel matte and slag produced by the side-blowing depletion furnace are not separated, only the smelting process is completed, and they flow directly into the sedimentation furnace through the flow channel. The sedimentation separation is undertaken by the electric furnace, ensuring the high efficiency, continuity and stability of the smelting process.

[0041] The discharge port of the side-blowing depletion furnace is set as siphon discharge or burn-eye discharge, for example, set to two or more, wherein siphon discharge can prevent unreacted materials from being discharged from the slag mouth; when burning eye discharge, the slag surface exceeds the slag mouth by more than 100mm, which can prevent unreacted materials from being discharged.

[0042] In addition, when the sulfidation reaction is carried out in the side-blowing depletion furnace, the furnace temperature is controlled to be 1300° C. to 1450° C. The oxygen-enriched side-blowing molten pool smelting furnace is also provided with a group of electrodes for heat preservation of the melt in an emergency state.

[0043] (3) The mixed melt, i.e., the melt-slag mixture, produced by the side-blowing depletion furnace flows directly from the discharge port through the chute into the electric heat settling furnace, i.e., the settling electric furnace. The nickel matte and slag are separated by the electric heat settling furnace, and the separated nickel matte and slag are discharged through their respective discharge ports. The nickel matte discharge port is set at a position 100 mm from the furnace bottom, and the slag discharge port is set at a position 500-600 mm high from the furnace bottom.

[0044] After 2-6 hours of sedimentation, the high-nickel matte and slag in the electric heat sedimentation furnace are clarified and separated, the high-nickel matte is granulated by water and sold, and the slag is sold as general solid waste after being crushed by wind or water. Qualified high-nickel matte products contain 65%-73% nickel, 4-10% iron, and 18-23% sulfur. The nickel content of slag is less than 0.3%.

[0045] In addition, the top of the oxygen-enriched side-blowing molten pool smelting furnace is higher than that of the electric heating settling furnace, or is arranged at the same height as the electric heating settling furnace, which can further improve the efficient, continuous and stable operation of the production process. The electric heating settling furnace has an operating temperature of 1300°C to 1500°C.

[0046] In addition, if the raw material contains high iron, resulting in the iron content in the high-nickel matte product being higher than 10%, an oxidation insulation furnace is required to be equipped. The high-nickel matte with excessive iron content is sent to the oxidation insulation furnace for blowing and iron removal, and the high-nickel matte with qualified iron and blowing slag are produced. The high-nickel matte is sent to water for granulation, and the blowing slag is returned to the sedimentation furnace. The flue gas produced by the side-blowing depletion furnace and the sedimentation furnace or the oxidation insulation furnace is sent to the desulfurization treatment, and the tail gas meets the emission standards.

[0047] The above-mentioned embodiment utilizes the high efficiency and continuity of the oxygen-enriched / pure oxygen side-blowing molten pool smelting technology, carries out reduction and sulfidation in the oxygen-enriched side-blowing molten pool smelting furnace, and vigorously stirs the nickel matte and slag through a spray gun to allow the reaction to proceed fully; and the output mixed melt is quietly settled and separated into nickel matte and slag in an electric thermal settling furnace, fully considering the problems arising in the production process of treating copper-containing solid waste, zinc leaching slag, etc. using the oxygen-enriched side-blowing molten pool smelting technology, and the oxygen-enriched side-blowing molten pool smelting furnace is designed to be without a furnace, and the nickel matte and slag output by smelting are not separated, and the nickel-iron alloy that may be deposited can be stirred and lifted for a second time to be fully mixed with the slag to prevent a "dead furnace" caused by the formation of an alloy frozen layer at the bottom of the furnace.

[0048] The present application creatively combines the side-blowing combustion depletion technology with the electric heating temperature raising and settling technology. When the "molten slag side-blowing depletion furnace and electric heating settling furnace" are used to deplete and settle the molten slag, there are also the following advantages: First, the improvement of chemical kinetic conditions makes the furnace bed energy efficiency higher, does not require too large a furnace bed area and too high an electrode power, the investment cost is low, and the furnace body heats less and the operating cost is low. Secondly, the excellent chemical kinetic conditions of the side-blowing depletion furnace combined with the relatively calm and weakly stirred molten pool of the electric heating settling furnace not only efficiently depletes the valuable metals lost chemically in the molten slag, but also makes the valuable metals lost physically therein well settled, and finally ensures that the valuable metals contained in the tailings are controlled within an acceptable range. Then, the improvement of chemical kinetic conditions makes the Fe3O4 in the slag also well reduced and suppressed, and the reduction of furnace slag ensures the molten pool volume, which is also conducive to the depletion and sedimentation of valuable metals. Thirdly, the molten pool volume is guaranteed, and after the valuable metals contained in the tailings are controlled, the safety of the water quenching system is guaranteed. Finally, there is no longer the problem of reducing agent floating on the surface of the molten pool and burning over a large area, and the life of the upper furnace body is also guaranteed.

[0049] The present application is further described below in conjunction with specific embodiments:

[0050] Embodiment 1:

[0051] Nickel-containing solid waste (low Fe) and gypsum slag are added to the dryer and dehydrated to 10% water content; the flux is quartz and limestone, and the silicon-calcium ratio in the raw materials is SiO2 / CaO=1.5; the reducing agent is coke, and the amount of coke added accounts for 5% of the total weight of the raw materials. The furnace temperature is 1300℃~1450℃, and the thickness of the melt mixed with nickel matte and slag is 800mm. Natural gas and oxygen-enriched air containing 70% O2 are sprayed into the furnace through a side-blowing spray gun. The ratio of oxygen in the oxygen-enriched air to natural gas is 1.98:1, oxygen is insufficient, and the melt pressure is 0.3MPa.

[0052] The side-blowing depletion furnace is equipped with two melt burn-eye discharge ports. The mixed melt of fully reacted nickel matte and slag flows into the electric thermal settling furnace through the flow channel and is discharged every 6 hours. When the burn-eye is discharged, the slag surface exceeds the slag mouth by more than 100mm to prevent the discharge of unreacted materials. The power of the electric thermal settling furnace is about 100kVA / t melt, and the furnace operating temperature is 1300℃~1500℃. After 5h of sedimentation period for clarification and separation, the nickel matte is discharged from the nickel matte mouth and sent to water for granulation; the slag is discharged from the slag discharge port and granulated by wind.

[0053] The nickel matte produced by the settling furnace contains 65% Ni, 7% Fe, and 20% S. The slag contains 0.15% Ni.

[0054] Embodiment 2:

[0055] Nickel-containing solid waste (high Fe) and nickel sulfide waste are added to the dryer and dehydrated to 8% water content; the flux is quartz and limestone, and the silicon-calcium ratio in the raw materials is SiO2 / CaO=1.5; the reducing agent is carbon, and the amount of carbon added accounts for 5.5% of the total weight of the raw materials. The furnace temperature is 1300℃~1400℃, and the thickness of the melt mixed with nickel matte and slag is 800~1200mm. Natural gas and oxygen-enriched air containing 80% O2 are sprayed into the furnace through a side-blowing spray gun. The ratio of oxygen in the oxygen-enriched air to natural gas is 1.95:1, oxygen is insufficient, and the melt pressure is 0.35MPa.

[0056] The side-blowing depletion furnace is equipped with two siphon discharge ports. The mixed melt of fully reacted nickel matte and slag flows into the electric heat settling furnace through the flow channel and is discharged every 8 hours. The power of the electric heat settling furnace is about 100kVA / t melt, and the furnace operating temperature is 1450℃. After clarification and separation during the 6h settling period, high-Fe nickel matte is discharged from the nickel matte port and flows into the oxidation insulation furnace for blowing and iron removal. The slag is discharged from the slag discharge port and granulated by water.

[0057] High-Fe nickel matte is blown in an oxidation holding furnace to remove iron, the qualified high-nickel matte produced is sent to water for granulation, and the blowing slag is returned to the settling electric furnace.

[0058] The high nickel matte in the oxidation holding furnace contains 60% Ni, 9% Fe, and 21% S. The slag contains 0.2% Ni.

[0059] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.

Claims

1. A method for producing nickel matte from nickel-containing solid waste, It is characterized in that include: Dry the nickel-containing solid waste and the sulfiding agent ingredients until the moisture content is no more than 10%; The dried material is mixed with the reducing agent and flux ingredients and sent to an oxygen-enriched side-blown molten pool smelting furnace for sulfidation reaction. The furnace temperature is 1300°C to 1450°C to obtain a mixed melt. A spray gun is provided on the side of the oxygen-enriched side-blown molten pool smelting furnace. The spray gun is 300mm to 400mm away from the furnace bottom. Energy and oxygen-enriched air / pure oxygen are blown into the furnace through the spray gun. The blown gas pressure is 0.1MPa to 0.35MPa, and the oxygen concentration is ≥60%. The ratio of oxygen to energy is controlled. Forming oxygen deficiency and stirring the mixed melt; wherein the oxygen-enriched side-blown molten pool smelting furnace adopts a "hearthless" form, the discharge port of the oxygen-enriched side-blown molten pool smelting furnace is a siphon discharge port or a burn eye discharge port, and when it is a burn eye discharge port, the slag surface exceeds the slag port by more than 100mm, and the discharge port is directly connected to the entrance of the electric thermal settling furnace through a chute, and the oxygen-enriched side-blown molten pool smelting furnace only performs smelting, and the produced mixed melt is not separated from nickel matte and slag in the oxygen-enriched side-blown molten pool smelting furnace; The mixed melt flows directly from the discharge port of the oxygen-enriched side-blown molten pool smelting furnace through the chute into the electric thermal settling furnace for sedimentation separation of nickel matte and slag. The furnace operating temperature is 1300℃~1500℃, the sedimentation separation time is 2~6h, and the nickel matte is discharged from the nickel matte discharge port and the slag is discharged from the slag discharge port.

2. The method for producing nickel matte from nickel-containing solid waste according to claim 1, It is characterized in that The nickel matte discharge port of the electrothermal settling furnace is arranged at a position 100 mm away from the furnace bottom, and the slag discharge port is arranged at a position 500-600 mm high from the furnace bottom.

3. The method for producing nickel matte from nickel-containing solid waste according to claim 1, It is characterized in that The nickel matte is crushed by water and granulated for sale, and the slag is crushed by wind or water and sold as general solid waste. If the iron content in the nickel matte product is higher than 10%, the nickel matte will be sent to an oxidation insulation furnace for blowing to remove the iron, and high-nickel matte with qualified iron and blowing slag will be produced. The high-nickel matte will be crushed by water and the blowing slag will be returned to the electric thermal settling furnace.

4. The method for producing nickel matte from nickel-containing solid waste according to claim 1, It is characterized in that The oxygen-enriched side-blowing molten pool smelting furnace is also provided with a group of electrodes for heat preservation of the melt in an emergency state.

5. The method for producing nickel matte from nickel-containing solid waste according to claim 1, It is characterized in that The furnace top of the oxygen-enriched side-blowing molten pool smelting furnace is higher than that of the electric thermal settling furnace, or is arranged at the same height as the electric thermal settling furnace.

6. The method for producing nickel matte from nickel-containing solid waste according to claim 1, It is characterized in that The vulcanizing agent is gypsum slag or sulfur-containing waste; The reducing agent is one or more of coke, graphite powder and carbon essence; The energy injected by the spray gun is one or more of natural gas, coal powder and organic solvent.

7. A system used in the method for producing nickel matte from nickel-containing solid waste according to any one of claims 1 to 6, It is characterized in that include: A drying furnace, used to dry the nickel-containing solid waste and the sulfiding agent ingredients after batching; The oxygen-enriched side-blown molten pool smelting furnace is used to receive the dried material after batching, the reducing agent and the flux and carry out a sulfidation reaction to obtain a mixed melt, and the oxygen-enriched side-blown molten pool smelting furnace only carries out smelting, and the nickel matte and slag in the produced mixed melt are not separated in the oxygen-enriched side-blown molten pool smelting furnace; a spray gun is arranged on the side of the oxygen-enriched side-blown molten pool smelting furnace, and the spray gun is 300mm to 400mm away from the furnace bottom, and the spray gun is used to blow energy and oxygen-enriched air / pure oxygen into the furnace to stir the mixed melt; the oxygen-enriched side-blown molten pool smelting furnace adopts a "hearth-free" form, and the discharge port of the oxygen-enriched side-blown molten pool smelting furnace is a siphon discharge port or a burn eye discharge port, and when it is a burn eye discharge port, the slag surface exceeds the slag port by more than 100mm; The electric thermal settling furnace has an inlet directly connected to the discharge port of the oxygen-enriched side-blown molten pool smelting furnace through a chute, and is used to receive the mixed melt discharged from the discharge port, and to separate the nickel matte and slag by settling, and to discharge the nickel matte from the nickel matte discharge port and the slag from the slag discharge port.