A method for controlling liquid carbides in H13 hot working die steel
Through electric furnace + LF + VD + die casting smelting technology, combined with electroslag remelting, forging and annealing treatments, the problem of liquid carbide control in H13 steel has been solved, the material has been efficiently improved, and the impact absorption capacity and service life have been improved. Reduced production costs.
Patent Information
- Application Number
- CN202211686412.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-27
AI Technical Summary
Existing methods for controlling liquid carbides in H13 steel are expensive and not very operable, and cannot completely eliminate liquid carbides, resulting in low material toughness and premature failure.
The H13 steel is smelted using the electric furnace + LF + VD + die casting method. Through electroslag remelting, high temperature homogenization and forging, short-term high temperature homogenization and annealing treatment, liquid carbides are completely eliminated and the plasticity, toughness and use of the steel are improved. life.
It achieves the complete elimination of liquid carbide in H13 steel, improves the impact absorption capacity and material service life, reduces production costs, and improves product quality.
Smart Images

Figure CN116083779B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel smelting and hot processing, and in particular to a method for controlling liquid carbides in H13 hot working die steel. Background Art
[0002] H13 steel is one of the most commonly used hot working die steels at home and abroad. It is widely used in the production of aluminum alloy die-casting molds, extrusion molds and hot forging molds because of its excellent hardenability, hardenability, wear resistance, high temperature toughness, thermal fatigue resistance, as well as excellent machinability and polishing properties.
[0003] Due to the high content of strong carbide-forming elements Cr, Mo, and V in H13 steel, dendritic segregation is inevitably formed during the non-equilibrium solidification process of the molten steel. When the last solidified central area between the dendrite arms reaches the eutectic composition, liquid carbides will be generated. The coarse liquid carbides distributed in the crystal will increase the brittleness of the material due to self-cracking or separation from the matrix interface, resulting in reduced plasticity and toughness, and premature failure of the material.
[0004] According to incomplete statistics, the proportion of premature failure of H13 steel due to improper control of liquid carbides, which leads to low toughness of finished steel, accounts for about 20% of the total failure. NADCA#207 and SEP1614 standards provide corresponding banding and organization rating maps for evaluating banded segregation, liquid carbides and network carbides. In order to make the products meet the standard requirements and improve the product yield, researchers have sorted out the causes of liquid carbides and adopted various measures to control the generation of liquid carbides in steel.
[0005] Invention patent CN113649540B discloses "a method for refining liquid carbides in H13 hollow castings", which specifically includes vacuum induction melting of raw materials to obtain induction melting ingots; the induction melting ingots are used as parent materials after surface treatment and smelted in a medium frequency induction furnace, and a layer of smelting slag is covered on the upper part of the molten steel during the smelting process; after the smelting in the medium frequency induction furnace is completed, the molten steel and the slag are poured into a vertical centrifuge with a casting mold, and the vertical centrifuge rotates at different speeds at room temperature to generate a composite centrifugal field, reduce the degree of element segregation between dendrites of the ingot, and increase the solid phase rate of liquid carbides in the ingot, thereby achieving the effect of refining the size of liquid carbides in the H13 hollow castings.
[0006] Invention patent CN108015255B discloses a "method for preparing high-speed tool steel", which specifically includes the following process steps: 1) heating the ledeburite high-speed tool steel billet material to be processed to the liquidus T L 2) Cool the material to T L ~T SThe solid-liquid two-phase region between the two phases is kept warm to obtain a semi-solid structure with a solid phase ratio of more than 70%; 3) the material is deformed in the solid-liquid two-phase region with a forging ratio of more than 1.5; 4) the material is cooled to the solid phase line T S The invention can effectively break the dendrites generated during the solidification process of high-speed tool steel, reduce dendrite segregation, and inhibit the precipitation of liquid carbides by deforming in the solid-liquid two-phase region, thereby achieving the purpose of obtaining a homogenized structure, improving comprehensive mechanical properties, and extending service life.
[0007] At present, all methods for controlling liquid carbide in steel are mainly based on external equipment or high-precision control, which requires extremely high cost and poor operability. Moreover, most of them can only refine the size of liquid carbide but not completely eliminate it. Therefore, it is urgent to develop a method for controlling liquid carbide in steel, which can completely remove liquid carbide in steel, is easy to implement, has strong operability, and does not increase additional costs. Summary of the invention
[0008] The purpose of the present invention is to provide a control method for liquid carbides in H13 hot working die steel. The method is simple and easy to implement, has strong operability, can effectively eliminate liquid carbides in steel, improve the plasticity and toughness of steel, increase the service life of mold materials, improve product quality and reduce costs.
[0009] To achieve the above object, the present invention provides the following technical solutions:
[0010] According to one aspect of the present disclosure, a method for controlling liquid carbides in H13 hot working die steel is provided, the method comprising the following steps:
[0011] The H13 steel ring ingot is obtained by smelting using the method of electric furnace + LF + VD + mold casting;
[0012] The annular ingot is subjected to electroslag remelting treatment to obtain an electroslag ingot;
[0013] The electroslag ingot is subjected to high temperature homogenization and forging and blanking treatment to obtain a forged blank;
[0014] The forging billet is subjected to short-time high-temperature homogenization and thermal deformation to obtain a deformed billet;
[0015] The steel billet is annealed to obtain a finished steel product.
[0016] In a possible implementation manner, the chemical composition of the finished steel material includes, by mass percentage:
[0017] C: 0.35%~0.45%; Si: 0.80%~1.20%; Mn: 0.20%~0.50%; Cr: 4.80%~5.50%; V: 0.80%~1.20%; Mo: 1.10%~1.50%; the balance is Fe.
[0018] In a possible implementation manner, the molding process is:
[0019] The casting method is adopted. During casting, a cast iron core is placed in the center of the ingot mold to make it an annular solid ingot mold. The molten steel is injected from the ring of the annular mold and quickly solidifies and cools along the ingot mold wall and the cast iron core.
[0020] In a possible implementation manner, the slag system of the electroslag remelting is a ternary slag system of 65% CaF2-25% Al2O3-10% MgO.
[0021] In a possible implementation manner, the conditions for electroslag remelting include:
[0022] The voltage is 45V~60V, and the current is 7000A~13000A.
[0023] In a possible implementation, the high temperature homogenization conditions include:
[0024] The heating temperature is 1200-1300°C and the holding time is 5-10h.
[0025] In a possible implementation manner, the forging process is two-piercing and two-pulling.
[0026] In a possible implementation, the conditions for short-time high-temperature homogenization include:
[0027] The heating temperature is 1240-1300°C and the holding time is 1-2h.
[0028] In a possible implementation manner, the thermal deformation conditions include:
[0029] The method of thermal deformation is forging or rolling;
[0030] The final deformation temperature is ≥900℃.
[0031] In a possible implementation manner, the annealing conditions in step S5 include:
[0032] The heating temperature is 780-860°C and the insulation time is 10-25h.
[0033] Technical effects and advantages of the present invention:
[0034] First, the present invention can completely eliminate liquid carbides in H13 steel, so that the impact absorption energy of the finished steel is increased by more than 50%, the ratio of the transverse and longitudinal impact absorption energy is increased by more than 3%, and the impact absorption energy qualification rate reaches 100%.
[0035] Second, the method of the present invention is simple and easy to implement, has strong operability, can effectively eliminate liquid carbides in steel, improve the plasticity and toughness of steel, increase the service life of mold materials, improve product quality and reduce costs.
[0036] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 A flow chart of a method for controlling liquid carbides in H13 hot working die steel according to an exemplary embodiment of the present invention;
[0038] Figure 2 This is a diagram of the liquid separation carbide of the finished product of exemplary embodiment 1 of the present invention;
[0039] Figure 3 This is a liquid separation carbide diagram of the finished product of an exemplary comparative example of the present invention. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] In addition, the flowcharts shown in the accompanying drawings are only exemplary and do not necessarily include all the steps. For example, some steps can be decomposed, and some steps can be combined or partially combined, so the actual execution order may change according to the actual situation.
[0042] At the same time, the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example.
[0043] In addition, the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or apparatus comprising a series of steps or sub-modules is not necessarily limited to those steps or sub-modules explicitly listed, but may include other steps or sub-modules not explicitly listed or inherent to these processes, methods, products, or apparatuses.
[0044] Figure 1 FIG. 1 is a flow chart of a method for controlling liquid carbides in H13 hot working die steel according to an exemplary embodiment of the present invention. Figure 1 As shown, an exemplary embodiment of the present invention provides a method for controlling liquid carbides in H13 hot working die steel, the method comprising the following steps:
[0045] Step S1, adopting electric furnace + LF + VD + mold casting pouring method for casting, placing a cast iron core in the center of the ingot mold during casting to make it a ring-shaped solid ingot mold, and injecting molten steel from the ring of the ring mold, and rapidly solidifying and cooling along the ingot mold wall and the cast iron core to obtain an H13 steel ring-shaped ingot.
[0046] Step S2, the annular ingot obtained in step S1 is subjected to electroslag remelting treatment using a ternary slag system of 65% CaF2-25% Al2O3-10% MgO, with the voltage controlled between 45 and 60 V and the current controlled between 7000 and 13000 A, to obtain an electroslag ingot, whose chemical composition, in terms of mass percentage, includes:
[0047] C: 0.35%~0.45%; Si: 0.80%~1.20%; Mn: 0.20%~0.50%; Cr: 4.80%~5.50%; V: 0.80%~1.20%; Mo: 1.10%~1.50%; the balance is Fe.
[0048] Step S3, subjecting the electroslag ingot obtained in step S2 to a high temperature homogenization treatment at a heating temperature of 1200-1300° C. and a heat preservation time of 5-10 hours, and then subjecting the ingot to a two-pier and two-draw forging process to obtain a forging ingot;
[0049] Step S4, subjecting the forging billet obtained in step S3 to a short-time high-temperature homogenization treatment at a heating temperature of 1240-1300° C. and a holding time of 1-2 hours, and then subjecting the forging billet to forging or rolling treatment to ensure that the final forging or final rolling temperature is ≥900° C., thereby obtaining a deformed billet;
[0050] Step S5, subjecting the steel billet obtained in step S4 to annealing treatment at a heating temperature of 780-860° C. and a holding time of 10-25 hours to obtain a finished steel product.
[0051] Example 1
[0052] A method for controlling liquid carbides in H13 hot working die steel provided in exemplary embodiment 1 of the present invention specifically includes the following steps:
[0053] Step S1, adopting electric furnace + LF + VD + mold casting pouring method for casting, placing a cast iron core in the center of the ingot mold during casting to make it a ring-shaped solid ingot mold, and injecting molten steel from the ring of the ring mold, and rapidly solidifying and cooling along the ingot mold wall and the cast iron core to obtain an H13 steel ring-shaped ingot.
[0054] Step S2, the annular ingot obtained in step S1 is subjected to electroslag remelting treatment using a ternary slag system of 65% CaF2-25% Al2O3-10% MgO, with the voltage controlled to 55V and the current controlled to 8000A, to obtain an electroslag ingot, whose chemical composition, in terms of mass percentage, includes:
[0055] C: 0.42%; Si: 0.86%; Mn: 0.34%; Cr: 5.13%; V: 0.89%; Mo: 1.37%; the balance is Fe.
[0056] Step S3, heating the electroslag ingot obtained in step S2 to a high temperature of 1220° C. and a holding time of 8 hours for high temperature homogenization and performing two-pier and two-draw forging to obtain a forging blank;
[0057] Step S4, heating the forging billet obtained in step S3 to 1280° C. for a short-time high-temperature homogenization with a holding time of 1 hour, and performing forging treatment with a final forging temperature of 930° C. to obtain a deformed billet;
[0058] Step S5, subjecting the steel billet obtained in step S4 to an annealing treatment at a heating temperature of 790° C. and a holding time of 16 hours to obtain a finished steel product.
[0059] Figure 2 This is a liquid precipitation carbide diagram of the finished product of exemplary embodiment 1 of the present invention, as shown in Figure 2 As shown, no liquid carbide was found in the microstructure of the finished steel product. After being processed into 10*10*55mm, V-notch specimens, the longitudinal and transverse impact absorption energies were detected to be 86J and 74J, respectively, which were increased by 56.3% and 64.4% respectively compared with the products produced by the prior art. The longitudinal and transverse impact absorption energy ratio was 0.86, which was increased by 4.87% compared with the products produced by the prior art. The impact absorption energy qualification rate was 100%.
[0060] Example 2
[0061] A method for controlling liquid carbides in H13 hot working die steel provided in exemplary embodiment 2 of the present invention specifically includes the following steps:
[0062] Step S1, adopting electric furnace + LF + VD + mold casting pouring method for casting, placing a cast iron core in the center of the ingot mold during casting to make it a ring-shaped solid ingot mold, and injecting molten steel from the ring of the ring mold, and rapidly solidifying and cooling along the ingot mold wall and the cast iron core to obtain an H13 steel ring-shaped ingot.
[0063] Step S2: The annular ingot obtained in step S1 is subjected to electroslag remelting treatment using a ternary slag system of 65% CaF2-25% Al2O3-10% MgO, with the voltage controlled to 45V and the current controlled to 7500A, to obtain an electroslag ingot, whose chemical composition, in terms of mass percentage, includes:
[0064] C: 0.38%; Si: 0.84%; Mn: 0.41%; Cr: 4.87%; V: 1.18%; Mo: 1.12%; the balance is Fe.
[0065] Step S3, heating the electroslag ingot obtained in step S2 to a high temperature of 1290° C. and a holding time of 5 hours for high temperature homogenization and performing two-pier and two-draw forging to obtain a forging blank;
[0066] Step S4, heating the forging billet obtained in step S3 to 1240° C. for a short-time high-temperature homogenization with a holding time of 2 hours, and performing forging treatment with a final forging temperature of 920° C. to obtain a deformed billet;
[0067] Step S5, subjecting the steel billet obtained in step S4 to an annealing treatment at a heating temperature of 810° C. and a holding time of 10 h to obtain a finished steel product.
[0068] No liquid carbide was found in the microstructure of the finished steel product. After being processed into 10*10*55mm V-notch specimens, the longitudinal and transverse impact absorption energies were tested to be 90J and 81J respectively, which were 63.6% and 80.0% higher than those of products produced by the prior art. The ratio of longitudinal and transverse impact absorption energies was 0.90, which was 9.75% higher than those of products produced by the prior art. The qualified rate of impact absorption energy was 100%.
[0069] Example 3
[0070] A method for controlling liquid carbides in H13 hot working die steel provided in exemplary embodiment 3 of the present invention specifically includes the following steps:
[0071] Step S1, adopting electric furnace + LF + VD + mold casting pouring method for casting, placing a cast iron core in the center of the ingot mold during casting to make it a ring-shaped solid ingot mold, and injecting molten steel from the ring of the ring mold, and rapidly solidifying and cooling along the ingot mold wall and the cast iron core to obtain an H13 steel ring-shaped ingot.
[0072] Step S2: The annular ingot obtained in step S1 is subjected to electroslag remelting treatment using a ternary slag system of 65% CaF2-25% Al2O3-10% MgO, with the voltage controlled at 60V and the current controlled at 12500A to obtain an electroslag ingot, whose chemical composition, in terms of mass percentage, includes:
[0073] C: 0.36%; Si: 0.99%; Mn: 0.47%; Cr: 4.95%; V: 1.10%; Mo: 1.42%; the balance is Fe.
[0074] Step S3, heating the electroslag ingot obtained in step S2 to 1260° C., holding time for 5 hours, high temperature homogenization and two-pier and two-draw forging to obtain a forging blank;
[0075] Step S4, heating the forging billet obtained in step S3 to a temperature of 1260° C. and a holding time of 2 h for short-time high-temperature homogenization, and rolling the billet at a final rolling temperature of 950° C. to obtain a deformed billet;
[0076] Step S5, subjecting the steel billet obtained in step S4 to an annealing treatment at a heating temperature of 860° C. and a holding time of 10 hours to obtain a finished steel product.
[0077] No liquid carbide was found in the microstructure of the finished steel product. After being processed into 10*10*55mm V-notch specimens, the longitudinal and transverse impact absorption energies were tested to be 84J and 72J, respectively, which were 52.7% and 60.0% higher than those of products produced by the prior art. The ratio of longitudinal and transverse impact absorption energies was 0.86, which was 4.87% higher than those of products produced by the prior art. The qualified rate of impact absorption energy was 100%.
[0078] Example 4
[0079] A method for controlling liquid carbides in H13 hot working die steel provided in exemplary embodiment 4 of the present invention specifically includes the following steps:
[0080] Step S1, adopting electric furnace + LF + VD + mold casting pouring method for casting, placing a cast iron core in the center of the ingot mold during casting to make it a ring-shaped solid ingot mold, and injecting molten steel from the ring of the ring mold, and rapidly solidifying and cooling along the ingot mold wall and the cast iron core to obtain an H13 steel ring-shaped ingot.
[0081] Step S2: The annular ingot obtained in step S1 is subjected to electroslag remelting treatment using a ternary slag system of 65% CaF2-25% Al2O3-10% MgO, with the voltage controlled at 50V and the current controlled at 9000A, to obtain an electroslag ingot, the chemical composition of which, in terms of mass percentage, includes:
[0082] C: 0.39%; Si: 1.02%; Mn: 0.29%; Cr: 5.21%; V: 1.04%; Mo: 1.31%; the balance is Fe.
[0083] Step S3, subjecting the electroslag ingot obtained in step S2 to high temperature homogenization at a heating temperature of 1300° C. and a holding time of 5 hours, and to two-pier and two-draw forging to obtain a forging blank;
[0084] Step S4, heating the forging billet obtained in step S3 to a temperature of 1300° C. and a holding time of 1 h for short-time high-temperature homogenization, and performing rolling treatment with a final rolling temperature of 950° C. to obtain a deformed billet;
[0085] Step S5, subjecting the steel billet obtained in step S4 to an annealing treatment at a heating temperature of 840° C. and a holding time of 25 h to obtain a finished steel product.
[0086] No liquid carbide was found in the microstructure of the finished steel product. After being processed into 10*10*55mm V-notch specimens, the longitudinal and transverse impact absorption energies were tested to be 95J and 86J respectively, which were respectively increased by 72.7% and 91.1% compared with the products produced by the prior art. The ratio of longitudinal and transverse impact absorption energies was 0.90, which was increased by 9.75% compared with the products produced by the prior art. The qualified rate of impact absorption energy was 100%.
[0087] Example 5
[0088] Exemplary embodiment 5 of the present invention provides a method for controlling liquid carbides in H13 hot working die steel, which specifically includes the following steps:
[0089] Step S1, adopting electric furnace + LF + VD + mold casting pouring method for casting, placing a cast iron core in the center of the ingot mold during casting to make it a ring-shaped solid ingot mold, and injecting molten steel from the ring of the ring mold, and rapidly solidifying and cooling along the ingot mold wall and the cast iron core to obtain an H13 steel ring-shaped ingot.
[0090] Step S2: The annular ingot obtained in step S1 is subjected to electroslag remelting treatment using a ternary slag system of 65% CaF2-25% Al2O3-10% MgO, with the voltage controlled to 60V and the current controlled to 13000A, to obtain an electroslag ingot, whose chemical composition, in terms of mass percentage, includes:
[0091] C: 0.42%; Si: 1.10%; Mn: 0.48%; Cr: 5.04%; V: 1.17%; Mo: 1.14%; the balance is Fe.
[0092] Step S3, subjecting the electroslag ingot obtained in step S2 to high temperature homogenization at a heating temperature of 1200° C. and a heat preservation time of 10 hours and to two-pier and two-draw forging to obtain a forging blank;
[0093] Step S4, heating the forging billet obtained in step S3 to a temperature of 1260° C. and a holding time of 2 h for short-time high-temperature homogenization, and rolling the billet at a final rolling temperature of 930° C. to obtain a deformed billet;
[0094] Step S5, subjecting the steel billet obtained in step S4 to an annealing treatment at a heating temperature of 780° C. and a holding time of 20 h to obtain a finished steel product.
[0095] No liquid carbide was found in the microstructure of the finished steel product. After being processed into 10*10*55mm V-notch specimens, the longitudinal and transverse impact absorption energies were tested to be 89J and 76J, respectively, which were 61.8% and 68.9% higher than those of products produced by the prior art. The ratio of longitudinal and transverse impact absorption energies was 0.85, which was 3.65% higher than those of products produced by the prior art. The qualified rate of impact absorption energy was 100%.
[0096] Comparative Example
[0097] An exemplary comparative example of the present invention provides a method for controlling liquid carbide of H13 hot working die steel, which specifically includes the following steps:
[0098] Step S1, casting by electric furnace + LF + VD + mold casting pouring method, using a conventional ingot mold for casting, and casting to obtain a H13 steel solid ingot.
[0099] Step S2: The solid ingot obtained in step S1 is subjected to electroslag remelting treatment using a ternary slag system of 65% CaF2-25% Al2O3-10% MgO, with the voltage controlled to 50V and the current controlled to 10500A, to obtain an electroslag ingot, whose chemical composition, in terms of mass percentage, includes:
[0100] C: 0.39%; Si: 1.04%; Mn: 0.41%; Cr: 5.03%; V: 0.92%; Mo: 1.32%; the balance is Fe.
[0101] Step S3, subjecting the electroslag ingot obtained in step S2 to high temperature homogenization at a heating temperature of 1280° C. and a heat preservation time of 30 hours, and to two-pier and two-draw forging and blanking treatment to obtain a forging blank;
[0102] Step S4, the forging billet obtained in step S3 is reheated at a temperature of 1100° C. for a holding time of 5 h, and then subjected to subsequent fine forging treatment at a final forging temperature of 850° C. to obtain a deformed billet;
[0103] Step S5, subjecting the steel billet obtained in step S4 to an annealing treatment at a heating temperature of 790° C. and a holding time of 20 hours to obtain a finished steel product.
[0104] Figure 3 This is a liquid separation carbide diagram of the finished product of the exemplary comparative example of the present invention, such as Figure 3 As shown in the figure, the black chain-like structure is the liquid carbide in the microstructure at half the radius of the finished steel. Figure 3 Liquid carbides can be seen in the black chain-like distribution in the steel matrix. After being processed into 10*10*55mm, V-notch specimens, the longitudinal and transverse impact absorption energies were tested to be 55J and 45J respectively, the longitudinal and transverse impact absorption energy ratio was 0.82, and the impact absorption energy qualification rate was 81.1%.
[0105] Table 1 Performance test of finished steel products prepared in various embodiments and comparative examples
[0106]
[0107] Table 1 shows the performance test of finished steel prepared in each embodiment and comparative example. It can be seen from Table 1 that compared with the performance of steel produced by conventional process (as shown in comparative example), after the liquid carbide in H13 steel is eliminated by the method of the present invention, the longitudinal impact absorption energy of the steel is increased by 52.7% or more, the transverse impact absorption energy is increased by 60.0% or more, the longitudinal and transverse impact absorption energy ratio is increased by 3.65% or more, and the impact absorption energy qualification rate reaches 100%. The above data are sufficient to show that removing the liquid carbide in H13 steel can greatly improve the plastic toughness of the steel, increase the uniformity of performance, and reduce the anisotropy difference, so as to achieve the purpose of increasing the service life of the mold material, improving product quality, and reducing costs.
[0108] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for controlling liquid carbides in H13 hot working die steel. It is characterized in that The method comprises the following steps: The casting method of electric furnace + LF + VD + mold casting is adopted. During the casting, a cast iron core is placed in the center of the ingot mold to make it a ring-shaped solid ingot mold. The molten steel is injected from the ring of the ring mold, and it is rapidly solidified and cooled along the ingot mold wall and the cast iron core to obtain an H13 steel ring-shaped ingot. The annular ingot is made of 65% CaF 2 -25% Al 2 O 3 -10% MgO ternary slag system, the voltage is controlled between 45 and 60V, the current is controlled between 7000 and 13000A, and the electroslag remelting treatment is carried out to obtain electroslag ingots; The electroslag ingot is heated to a temperature of 1200-1300° C. and a heat preservation time of 5-10 hours for high temperature homogenization, and then subjected to a two-pier and two-draw forging process to obtain a forging blank; The forging billet is subjected to short-time high-temperature homogenization with a heating temperature of 1240-1300° C. and a holding time of 1-2 hours, and then subjected to forging or rolling treatment to ensure that the final forging or final rolling temperature is ≥900° C., thereby obtaining a deformed billet; The steel billet is subjected to annealing treatment at a heating temperature of 780 to 860° C. and a holding time of 10 to 25 hours to obtain a finished steel product; The chemical composition of the finished steel includes: C: 0.35%~0.45%; Si: 0.80%~1.20%; Mn: 0.20%~0.50%; Cr: 4.80%~5.50%; V: 0.80%~1.20%; Mo: 1.10%~1.50%; the balance is Fe.
Citation Information
Patent Citations
A method for preparing high-speed tool steel
CN108015255B
A method for refining liquid carbides in H13 hollow castings
CN113649540B
Method for manufacturing continuous pipe mill retained mandrel
CN102000954A
Production method of high-toughness high-isotropy large-section hot working die steel
CN105177258A
Preparation method of high-speed tool steel
CN108015255A