Heterojunction nanoparticles, preparation method and application thereof
By constructing heterojunction nanoparticles composed of CuSe and CoSe2, the problem of insufficient absorption capacity of existing semiconductor photocatalysts under visible light and near-infrared light is solved, and efficient photothermal conversion and redox reaction are achieved, and applied to air purification. Water purification and other fields.
Patent Information
- Application Number
- CN202310133252.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-17
AI Technical Summary
Existing semiconductor photocatalysts show strong photogenerating carrier generation under ultraviolet light, but have poor absorption capacity under visible and near-infrared light, and electron-hole pairs are easy to recombinate, limiting the photocatalytic performance.
By constructing heterojunction nanoparticles composed of CuSe and CoSe2, a hollow nanosphere structure is formed, which increases the specific surface area and active sites, and uses its unique flower-like structure to show good light absorption capacity in the visible and near-infrared regions. And reduce the recombination of electron-hole pairs by appropriate band arrangement.
The photothermal conversion efficiency and redox reaction efficiency were significantly improved, especially under 808nm near-infrared light, which showed a photothermal conversion efficiency of 64.7%, and the efficiency of generating reactive oxygen species under light activation was significantly improved.
Smart Images

Figure CN116099556B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of nano materials, and in particular relates to heterojunction nano particles, a preparation method and application thereof. Background Art
[0002] Nanomaterials have been widely used in many fields such as biomedicine, environmental protection and aerospace technology due to their unique size effect, physical and chemical properties, and high efficiency and tunability that are difficult to achieve with macroscopic materials. Among them, inorganic semiconductor nanomaterials can absorb light energy well and convert it into heat and chemical energy due to their specific band structure, so they are widely used in the field of photocatalysis. The preparation of highly active photocatalysts is of great significance for the practical application of efficient light energy conversion systems. They should have strong absorption capacity for light in a wide wavelength range, and at the same time be able to generate abundant electron-hole pairs under light excitation for effective charge separation. In addition, photocatalytic reactions also require sufficient surface area and active sites. Traditional semiconductors, such as titanium dioxide, can generate a large number of photogenerated carriers under ultraviolet light, but their visible light absorption capacity is poor, and electron-hole pairs are easy to recombine quickly, which greatly limits the photocatalytic performance. Therefore, it is necessary to develop semiconductor photocatalysts with a band gap suitable for wavelength light absorption, high charge mobility and fast surface reaction kinetics.
[0003] Up to now, it is impossible to find a semiconductor material that satisfies all of the above characteristics at the same time, and heterojunctions have become an effective strategy to improve the performance of semiconductor materials because they can combine the advantages of different materials. When different photoresponsive materials are combined, the constructed heterojunction can broaden the absorption of the spectrum and establish an internal electric field through appropriate energy band arrangement, thereby reducing the recombination of electron-hole pairs and improving the efficiency of redox reactions. In addition, the large specific surface area of the hollow structure can provide abundant active centers for redox reactions, and the resulting light scattering and reflection effects can enhance the absorption and utilization of light. Therefore, the method of synthesizing hollow heterostructured photocatalysts to improve light conversion efficiency is of great research significance.
[0004] Copper selenide (CuSe) nanomaterials, as narrow bandgap inorganic semiconductors, have been studied in the fields of information sensing, electrocatalysis and photocatalysis, but it is difficult to maintain uniformity and monodispersity in their nanostructures. Therefore, it is possible to further study CuSe-based heterostructured photocatalysts and explore their photocatalytic properties. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a heterojunction nanoparticle, a preparation method and application thereof. The heterojunction nanoparticle is prepared by compounding CuSe and CoSe 2, which can achieve higher photothermal conversion efficiency, photocatalytic efficiency of producing active oxygen and electron-hole pair separation efficiency, and has good application prospects.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In the first aspect, the present invention provides a heterojunction nanoparticle, comprising CuSe and CoSe 2 The heterojunction nanoparticles are hollow nanospheres, and the surface of the hollow nanospheres has nanorods and nanosheets.
[0008] Preferably, the average particle size of the heterojunction nanoparticles is 70 to 90 nm.
[0009] In a second aspect, the present invention provides a method for preparing heterojunction nanoparticles, comprising the following steps:
[0010] Cu 2 O, a cobalt source, a first solvent, a first reducing agent and a selenium source are mixed and reacted to obtain heterojunction nanoparticles.
[0011] Preferably, the Cu 2 O was prepared by the following method:
[0012] The copper source, the alkaline substance, the second solvent, the dispersant and the second reducing agent are mixed and reacted to obtain Cu 2 O.
[0013] Preferably, the second reducing agent is a hydrazine hydrate solution.
[0014] Preferably, the copper source is selected from Cu(NO 3 ) 2 ·3H 2 O and / or CuCl 2 ·2H 2 O.
[0015] Preferably, the alkaline substance is selected from sodium hydroxide and / or potassium hydroxide.
[0016] Preferably, the second solvent is selected from isopropanol.
[0017] Preferably, the dispersant is selected from polyvinyl pyrrolidone.
[0018] Preferably, the ratio of the copper source, the alkaline substance, the second solvent, the dispersant and the hydrazine hydrate solution is 0.1 mmol: (0.08-0.15) mmol: (25-40) mL: (0.0015-0.0025) mmol: (250-300) μL.
[0019] Preferably, the copper source and the alkaline substance are first mixed with the second solvent to obtain a copper source solution and an alkaline substance solution, and then the copper source solution, the alkaline substance solution, the dispersant and the second reducing agent are mixed and reacted to obtain Cu 2 O.
[0020] Preferably, the cobalt source is selected from Co(NO 3 ) 2 ·3H 2 O and / or CoCl 2 6H 2 O.
[0021] Preferably, the first solvent is selected from water.
[0022] Preferably, the first reducing agent is selected from sodium borohydride and / or potassium borohydride.
[0023] Preferably, the selenium source is selected from selenium powder.
[0024] Preferably, the Cu 2 The ratio of O, cobalt source, first solvent, first reducing agent and selenium source is 0.05mmol:(0.08~0.15)mmol:(1.5~4)mL:(0.08~0.15)mmol:(0.08~0.15)mmol.
[0025] In a third aspect, the present invention provides a photocatalyst comprising the heterojunction nanoparticles involved in the above technical solution.
[0026] In a fourth aspect, the present invention also provides the use of the above-mentioned photocatalyst in air purification, water purification or photocatalytic treatment.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The heterojunction nanoparticles provided by the present invention are composed of CuSe and CoSe 2 The composition is a hollow nanoflower-like structure with good monodispersity. The heterojunction nanoparticles have a large specific surface area and active sites due to their unique flower-like structure, so they can show good absorption in both the visible and near-infrared regions, and thus have obvious photothermal effects under 808nm near-infrared light, and show a high photothermal conversion efficiency (64.7%). At the same time, CuSe and CoSe 2 The heterojunction formed by the nanostructured carbon nanotubes significantly improves the separation efficiency of electron-hole pairs, and more electrons and holes are transferred to the surface of the material. Compared with CuSe with a narrower band gap, it has a strong improvement effect in the redox reaction of generating active oxygen activated by light. The heterojunction nanoparticles can be used to prepare photocatalysts and applied in the fields of air purification, water purification or photocatalytic therapy. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The Cu prepared in Example 1 2 SEM image of O;
[0030] Figure 2 TEM image of CS prepared in Comparative Example 1;
[0031] Figure 3 is a SEM image of the CSC prepared in Example 2;
[0032] Figure 4 TEM image of CSC prepared in Example 2;
[0033] Figure 5 Cu obtained in Example 3 2 SEM image of O;
[0034] Figure 6 Cu obtained in Example 4 2 SEM image of O;
[0035] Figure 7 is the SEM image of the CSC obtained in Example 5;
[0036] Figure 8 is a SEM image of the CSC obtained in Example 6;
[0037] Fig. 9 is the N of CSC obtained in Example 1 2 Adsorption-desorption isotherm curves;
[0038] Fig.10 is a comparison diagram of the UV-visible absorption spectra of the CS obtained in Comparative Example 1 and the CSC obtained in Example 2;
[0039] Fig.11 The heating and cooling curves of the CSC obtained in Example 2 under 808 nm laser irradiation;
[0040] Fig.12 The electron spin spectra of hydroxyl radicals generated by CS obtained in Comparative Example 1 and CSC obtained in Example 2 under different conditions;
[0041] Fig.13 The electron spin spectra of singlet oxygen generated by CS obtained in Comparative Example 1 and CSC obtained in Example 2 under different conditions;
[0042] Fig.14 The electron spin spectra of superoxide anions produced by CS obtained in Comparative Example 1 and CSC obtained in Example 2 under different conditions;
[0043] Fig.15Electrochemical impedance spectra of CS obtained in Comparative Example 1 and CSC obtained in Example 2;
[0044] Fig.16 It is a comparison diagram of the photothermal temperature rise curves of the CSC obtained in Examples 2, 5, and 6 under 808 nm laser irradiation. DETAILED DESCRIPTION
[0045] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] In view of the fact that the semiconductor photocatalysts in the prior art cannot simultaneously meet the characteristics of having a band gap suitable for wavelength light absorption, high charge mobility and fast surface reaction kinetics, the present invention provides a CSC heterojunction nanoparticle composed of CuSe and CoSe 2 The heterojunction nanoparticles are characterized by SEM and found to be hollow nanospheres with nanorods and nanosheets on the surface of the hollow nanospheres, and their macroscopic morphology is similar to that of hollow nanoflowers. 2 Adsorption-desorption isotherm test further proves that it is a hollow structure. The heterojunction nanoparticles provided by the present invention have good monodispersity and an average particle size of 70-90 nm.
[0047] The heterojunction nanoparticles provided by the present invention are composed of CuSe and CoSe 2 Composition, good monodispersity and unique flower-like structure, which gives it a large specific surface area and active sites. According to research, it has obvious photothermal effect under 808nm near-infrared light and shows a high photothermal conversion efficiency (64.7%). 2 The heterojunction formed by the nanostructured carbon nanotubes significantly improves the separation efficiency of electron-hole pairs, and more electrons and holes are transferred to the surface of the material. Compared with the single CuSe (referred to as "CS") with a narrower band gap, it has a strong improvement effect in the redox reaction of generating active oxygen activated by light. The heterojunction nanoparticles can be used to prepare photocatalysts and applied in the fields of air purification, water purification or photocatalytic therapy.
[0048] In some embodiments of the present invention, the heterojunction nanoparticles are prepared by the following preparation method:
[0049] Cu 2 O, a cobalt source, a first solvent, a first reducing agent and a selenium source are mixed and reacted to obtain heterojunction nanoparticles.
[0050] In some embodiments of the present invention, the Cu 2 O is obtained by mixing a copper source, an alkaline substance, a second solvent, a dispersant, and a second reducing agent, and reacting for 15 to 30 minutes. The copper source is selected from Cu(NO 3 ) 2 ·3H 2 O and / or CuCl 2 ·2H 2 O, the alkaline substance is selected from sodium hydroxide and / or potassium hydroxide, the second solvent is selected from isopropanol, the dispersant is selected from polyvinyl pyrrolidone (PVP), such as any one or more of PVP-40000, PVP-K30 or PVP-58000, preferably PVP-K30 (Mw=44000), the second reducing agent is selected from hydrazine hydrate solution, and the mass fraction of hydrazine hydrate solution is 35-50%. According to research, if the amount of hydrazine hydrate is too high, it will lead to the synthesis of Cu 2 O is small in size and easy to agglomerate or even collapse. If the amount of hydrazine hydrate is too low, Cu 2 O is large in size but not solid, which is not conducive to the subsequent experimental process. Therefore, in some embodiments of the present invention, according to the ratio of 0.1mmol: (0.08-0.15)mmol: (25-40)mL: (0.0015-0.0025)mmol: (250-300)μL, preferably 0.1mmol: (0.08-0.15)mmol: (25-40)mL: (0.0015-0.0025)mmol: (270-280)μL, the copper source, the alkaline substance, the second solvent, the dispersant and the hydrazine hydrate solution are mixed and reacted for 15-30min to obtain Cu 2 In some embodiments of the present invention, the copper source and the alkaline substance are first mixed with the second solvent to obtain a copper source solution and an alkaline substance solution, and then the copper source solution, the alkaline substance solution, the dispersant and the second reducing agent are mixed and reacted to obtain Cu 2 In some embodiments of the present invention, the copper source and the alkaline substance are preferably dispersed in the second solvent in the above proportions, and then a dispersant is added in proportion and stirred for 5 to 10 minutes, and then a hydrazine hydrate solution is added in proportion to carry out a reduction reaction for 5 to 10 minutes, and centrifuged to obtain the target product Cu 2 In some embodiments of the present invention, it is preferred to obtain Cu 2 O were washed with deionized water and / or ethanol to partially oxidize Cu 2 Cu in O + Partially oxidized to Cu in water 2+, thereby forming a CuO intermediate, which facilitates the subsequent replacement of CuO oxygen anions with selenium anions to synthesize CuSe, and the number of washings is not less than 3 times. In a specific embodiment of the present invention, 0.1 mmol of Cu(NO 3 ) 2 ·3H 2 O and NaOH were dissolved in 30 mL of isopropanol, and then the two were mixed and added to PVP-K30 (Mw = 44000), stirred for 10 min, and then 280 μL of hydrazine hydrate (50 wt%) was added. After the reaction continued for 10 min, the product was centrifuged (11000 rpm min -1 , 8min), washed with deionized water and ethanol three times respectively to obtain Cu 2 O.
[0051] In the preparation of Cu 2 O, according to the present invention, Cu 2 O, a cobalt source, a first solvent, a first reducing agent and a selenium source are mixed and reacted for 25 to 45 minutes to obtain heterojunction nanoparticles. In the present invention, it is preferred to react for 30 minutes, otherwise if the reaction time is too short, there will be few heterojunctions of the nanoflower-like structure, and if the reaction time is too long, the heterojunction nanoparticles will agglomerate. The cobalt source is selected from Co(NO 3 ) 2 ·3H 2 O and / or CoCl 2 6H 2 O, the first solvent is selected from water, the first reducing agent is selected from sodium borohydride and / or potassium borohydride, and the selenium source is selected from selenium powder. In some embodiments of the present invention, Cu is preferably added in a ratio of 00.05 mmol: (0.08-0.15) mmol: (1.5-4) mL: (0.08-0.15) mmol: (0.08-0.15) mmol. 2 O, a cobalt source, a first solvent, a first reducing agent and a selenium source are mixed and reacted to obtain heterojunction nanoparticles. In some embodiments of the present invention, it is preferred to 2 O is dispersed in a first solvent, and then mixed and reacted with a solution of a first reducing agent and a selenium source, and the mixing is preferably carried out under stirring conditions to obtain CuSe nanoparticles. Then, the CuSe nanoparticles are mixed and reacted with a cobalt source, a first solvent, a first reducing agent and a selenium source, and the mixing is preferably carried out under stirring conditions to obtain the heterojunction nanoparticles. In some embodiments of the present invention, the obtained heterojunction nanoparticles are preferably washed with deionized water, and the number of washings is not less than 3 times. In a specific embodiment of the present invention, the obtained Cu 2 O was dissolved in 10 mL of water and 0.0291 g of Co(NO 3) 2 ·3H 2 O was stirred for 20 min, then the precipitate was centrifuged and redispersed in 10 mL of water for later use. 0.0079 g of selenium powder and 0.0038 g of sodium borohydride were ultrasonically reacted in 2 mL of water for 5 min to form Se 2- solution, and then Se 2- The solution was quickly added to the above 10 mL reserve solution and reacted for 30 min. Finally, the product was centrifuged (11000 rpm min -1 , 8min), and washed with deionized water three times to obtain heterojunction nanoparticles.
[0052] The preparation method provided by the present invention uses cuprous oxide as a template and mixes it with Se 2- Solution mixing, through the Kirkendall effect, Se 2- The copper ions are adsorbed on the surface of cuprous oxide, and the copper ions inside are diffused into the solution to form a hollow structure. Then, by introducing a cobalt source, the cobalt ions and cuprous oxide are ion exchanged to obtain heterojunction nanoparticles. The preparation method provided by the invention is simple, convenient, easy to implement, and is conducive to industrialization or industrial production.
[0053] The heterojunction nanoparticles provided by the present invention can be used to prepare photocatalysts. According to research, they have obvious photothermal effects under 808nm near-infrared light and show a high photothermal conversion efficiency (64.7%). 2 The heterojunction formed by the material significantly improves the separation efficiency of electron-hole pairs, and more electrons and holes are transferred to the surface of the material. Compared with the single CuSe with a narrower band gap, it has a strong improvement effect in the redox reaction of photoactivated generation of active oxygen. It has broad application prospects in the fields of air purification, water purification or photocatalytic therapy.
[0054] In order to further illustrate the present invention, the following examples are provided for detailed description. The experimental raw materials used in the following examples of the present invention can be purchased from the market or prepared according to conventional preparation methods well known to those skilled in the art.
[0055] Example 1
[0056] This example is used to prepare Cu 2 O precursor, the specific method is as follows:
[0057] 0.0242 g Cu(NO 3 ) 2 ·3H 2O and 0.04g sodium hydroxide were dispersed in 30mL isopropanol respectively. The two 30mL solutions obtained above were quickly mixed and 0.2g polyvinyl pyrrolidone was quickly added, stirred at room temperature for 10min, and then 280μL hydrazine hydrate (50%) was added dropwise thereto. After the reaction was continued for 10min, the product was centrifuged (11000rpm min -1 , 8 min), washed with deionized water and ethanol three times respectively and then used for later use.
[0058] Example 2
[0059] This embodiment is used to prepare a hollow CSC heterojunction, and the specific method is as follows:
[0060] The Cu obtained in Example 1 above 2 O precursor was dissolved in 10 mL of water and 0.0291 g of Co(NO 3 ) 2 ·3H 2 O was stirred for 20 min, then the precipitate was centrifuged and redispersed in 10 mL of water for later use. 0.0079 g of selenium powder and 0.0038 g of sodium borohydride were ultrasonically reacted in 2 mL of water for 5 min to form Se 2- solution, and then Se 2- The solution was quickly added to the above 10 mL reserve solution and reacted for 30 min. Finally, the product was centrifuged (11000 rpm min -1 , 8 min), and washed with deionized water three times to obtain a hollow CSC heterojunction.
[0061] Embodiment 3-4
[0062] In this example, Cu 2 The O precursor is different from Example 1 only in that the added amounts of hydrazine hydrate are 260 μL and 300 μL respectively, and the other parameters and steps are consistent with Example 1.
[0063] Embodiment 5-6
[0064] This embodiment prepares a hollow CSC heterojunction, which is different from the embodiment 2 only in that the Cu obtained in the embodiment is 2 O precursors were replaced by the Cu obtained in Examples 3 to 4 2 O precursor, and the other parameters and steps are consistent with Example 1.
[0065] Comparative Example 1
[0066] This comparative example provides a hollow CuSe, and the specific method is as follows:
[0067] The Cu obtained in Example 1 above 2The O precursor was dissolved in 10 mL of water and set aside. 0.0079 g of selenium powder and 0.0038 g of sodium borohydride were ultrasonically reacted in 2 mL of water for 5 min to form Se 2- solution, and then Se 2- The solution was quickly added to the above 10 mL reserve solution and reacted for 30 minutes. Finally, the product was centrifuged (11000 rpm min -1 , 8 min), and washed three times with deionized water to obtain CuSe.
[0068] The surface morphology of the products obtained in Example 1, Example 2 and Comparative Example 1 was characterized by scanning electron microscopy and transmission electron microscopy. Figures 1 to 4 As shown. Among them, Figure 1 Cu 2 SEM images of O, Figure 2 TEM image of CS, Figure 3 is the SEM image of CSC. Figure 4 TEM image of CSC. Figure 1 It can be seen that Cu 2 O is a nanosphere structure, Figure 2 It can be seen that CS is a mesoporous hollow sphere structure. Figure 3 and Figure 4 It can be seen that CSC is a hollow nanoflower structure.
[0069] The surface morphology of the products obtained in Examples 3 to 6 was characterized by scanning electron microscopy and transmission electron microscopy. Figures 5 to 8 As shown. Among them, Figure 5 Cu obtained in Example 3 2 SEM images of O, Figure 6 Cu obtained in Example 4 2 SEM images of O, Figure 7 is the SEM image of CSC obtained in Example 5, Figure 8 is a SEM image of CSC obtained in Example 6. Figure 5 and Figure 7 It can be seen that when the amount of hydrazine hydrate added is low, the Cu 2 O also has a nanosphere structure, but it will affect the subsequent 2 O as the template affects the structure of the CSC, and the nanoflower structure is not obvious. Figure 6 and Figure 8 It can be seen that when the amount of hydrazine hydrate added is high, the Cu 2 O also has a nanosphere structure, but its size is slightly smaller. 2 The CSCs obtained with O as template are prone to agglomeration and even collapse. The results show that the amount of hydrazine hydrate used will affect the morphology of the final heterojunction nanoparticles.
[0070] The hollow CSC heterojunction obtained in Example 2 was subjected to N 2 Adsorption-desorption test, the results are as follows Fig. 9 As shown, from the shape of the curve, it can be seen that CSC has a porous structure.
[0071] The hollow CSC heterojunction obtained in Example 2 and the CuSe obtained in Comparative Example 1 were tested for UV-visible absorption spectra. The results are as follows: Fig.10 As shown, it can be seen that the CSC heterojunction shows good absorption in both the visible and near-infrared regions, and it can be seen that the CSC absorption is stronger than that of single CuSe. This is due to its unique flower-like structure, which gives it a larger specific surface area and active sites.
[0072] The hollow CSC heterojunction obtained in Example 2 was irradiated with 808 nm laser, and its heating and cooling curve is as follows: Fig.11 As shown, after calculation, it was found that the CSC heterojunction has a high light-to-heat conversion efficiency, which can reach 64.7%.
[0073] The hollow CSC heterojunction obtained in Example 2 and the CuSe obtained in Comparative Example 1 were tested under different conditions using an electron spin resonance spectrometer. The results are as follows: Figures 12-14 As shown, Fig.12 The electron spin spectra of hydroxyl radicals produced under different conditions are shown in Figure 2. Fig.13 The electron spin spectra produced by singlet oxygen under different conditions are shown in Figure 2. Fig.14 The electron spin spectra of superoxide anions produced under different conditions are shown in Figure 2. Figures 12-14 It can be seen that CSC has a stronger efficiency in photocatalytically generating reactive oxygen species than CS.
[0074] Electrochemical tests were performed on the hollow CSC heterojunction obtained in Example 2 and the CuSe obtained in Comparative Example 1. The test method is as follows:
[0075] 10 mg of powdered hollow CSC heterojunction and CuSe were weighed as samples and dispersed in 1 mL of ultrapure water, and then 50 μL of Nafion solution was added. After ultrasonic treatment for 30 min, a uniform suspension was formed. Then 150 μL of the suspension was dropped on the ITO glass and dried at room temperature for photoelectric testing.
[0076] Test results such as Fig.15 As shown, Fig.15 Figure 2 is the electrochemical impedance spectra of CS and CSC. It can be seen that the radius of the curve of CSC is significantly smaller than that of CS, indicating that the separation efficiency of electron-hole pairs is significantly improved after the heterojunction is formed.
[0077] The hollow CSC heterojunctions obtained in Examples 2, 5, and 6 were irradiated with 808 nm laser, and the photothermal heating curves were as follows: Fig.16 As shown, it can be seen that the hollow CSC heterojunctions obtained in Examples 2, 5, and 6 have higher heating rates and better photothermal effects. Among them, the heating rate of the hollow CSC heterojunction obtained in Example 2 is slightly higher than that of the CSC in Examples 5 and 6, indicating that its photothermal effect is better.
[0078] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A heterojunction nanoparticle, It is characterized in that CuSe and CoSe 2 composition; The heterojunction nanoparticles are hollow nanospheres, and the surface of the hollow nanospheres has nanorods and nanosheets; The method for preparing heterojunction nanoparticles comprises the following steps: 2 O, a cobalt source, a first solvent, a first reducing agent and a selenium source are mixed and reacted to obtain heterojunction nanoparticles; The Cu 2 O was prepared by the following method: First, a copper source and an alkaline substance are mixed with a second solvent respectively to obtain a copper source solution and an alkaline substance solution, and then the copper source solution, the alkaline substance solution, a dispersant and a second reducing agent are mixed and reacted to obtain Cu 2 O; The second reducing agent is a hydrazine hydrate solution; The copper source is selected from Cu(NO 3 ) 2 ·3H 2 O and / or CuCl 2 ·2H 2 O; The second solvent is selected from isopropanol; The ratio of the copper source, the alkaline substance, the second solvent, the dispersant and the hydrazine hydrate solution is 0.1 mmol:(0.08-0.15) mmol:(25-40) mL:(0.0015-0.0025) mmol:(250-300) μL.
2. A heterojunction nanoparticle as claimed in claim 1, It is characterized in that The average particle size is 70~90 nm.
3. A method for preparing heterojunction nanoparticles according to claim 1 or 2, It is characterized in that The following steps are involved: Cu 2 O, a cobalt source, a first solvent, a first reducing agent and a selenium source are mixed and reacted to obtain heterojunction nanoparticles; The Cu 2 O was prepared by the following method: First, a copper source and an alkaline substance are mixed with a second solvent respectively to obtain a copper source solution and an alkaline substance solution, and then the copper source solution, the alkaline substance solution, a dispersant and a second reducing agent are mixed and reacted to obtain Cu 2 O; The second reducing agent is a hydrazine hydrate solution; The copper source is selected from Cu(NO 3 ) 2 ·3H 2 O and / or CuCl 2 ·2H 2 O; The second solvent is selected from isopropanol; The ratio of the copper source, the alkaline substance, the second solvent, the dispersant and the hydrazine hydrate solution is 0.1 mmol:(0.08-0.15) mmol:(25-40) mL:(0.0015-0.0025) mmol:(250-300) μL.
4. The preparation method according to claim 3, It is characterized in that The alkaline substance is selected from sodium hydroxide and / or potassium hydroxide; The dispersant is selected from polyvinyl pyrrolidone.
5. The preparation method according to claim 3 or 4, It is characterized in that The cobalt source is selected from Co(NO 3 ) 2 ·3H 2 O and / or CoCl 2 6H 2 O; The first solvent is selected from water; The first reducing agent is selected from sodium borohydride and / or potassium borohydride; The selenium source is selected from selenium powder; The Cu 2 The ratio of O, cobalt source, first solvent, first reducing agent and selenium source is 0.05 mmol:(0.08~0.15) mmol:(1.5~4) mL: (0.08~0.15) mmol:(0.08~0.15) mmol.
6. A photocatalyst, It is characterized in that The invention comprises the heterojunction nanoparticles according to claim 1 or 2 or the heterojunction nanoparticles prepared by the preparation method according to any one of claims 3 to 5.
7. Use of the photocatalyst according to claim 6 in air purification or water purification.