A preparation method of a new type of cementitious material produced by using solid waste from granite mines

By calcining and grinding the solid waste of granite mine soil covering layer, weathered layer and filter cake, a new efficient and environmentally friendly cementitious material was prepared, which solved the problems of mine solid waste treatment and cement carbon emissions, and achieved the production of high-quality concrete and comprehensive utilization of resources.

CN116102270BActive Publication Date: 2024-11-01RICHANGSHENG BUILDING NEW MATERIAL DESIGN & RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211465389.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-11-01
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

The existing technology has waste of land resources and ecological environment for the treatment of solid waste in granite mines. The cement-based cementitious material is sensitive to particles with particle size less than 0.075mm, and cannot be used in large quantities, so it cannot effectively utilize the soil covering and weathering layers of granite mines. and the tailings produced by aggregate production.

Method used

By forcibly stirring the sand-washed solid waste and machined sand filter cakes of the granite mine soil cladding layer and weathered layer according to a specific weight ratio, calcining it in a baking furnace, annealing and cooling it and grinding it, a high specific surface area and suitable particle diameter are prepared. New gelling materials distributed.

Benefits of technology

The comprehensive and coordinated utilization of solid waste in granite aggregate mines has been realized, the problems of high treatment costs and technical difficulties have been solved, high-quality concrete has a fast gelling rate and no CO2 release, and is a green and low-carbon material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116102270B_ABST
    Figure CN116102270B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of comprehensive resource utilization and building materials, and specifically provides a method for preparing a new type of cementitious material produced by using solid waste from granite mines. The specific preparation steps are as follows: the remaining part after extracting mountain sand from the overburden layer and weathering layer of the granite mine is used as the matrix, mainly including the sand washing mud screened out before extraction and the weak substances removed during the ball milling process, and the machine-made sand filter cake is evenly mixed according to the weight ratio, sand washing mud: weak substances: filter cake = 40% to 70%: 15% to 45%: 7% to 30%, calcined at 800 to 900°C, annealed, cooled and ground, and the cementitious properties can be generated under the action of water glass and sodium hydroxide. The preparation of the above-mentioned new type of cementitious material has a simple process, realizes the resource utilization of mine solid waste, and is a new type of green and low-carbon cementitious material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of comprehensive utilization of resources and building materials, and mainly relates to a method for preparing a new type of cementitious material produced by utilizing solid waste from granite mines. Background Art

[0002] During the mining and production process of aggregate sand and gravel mines, a large amount of solid waste such as overburden, stone powder and filter cake will be generated. The existing technology for treating solid waste from aggregate mines is still mainly stacking, which causes waste of land resources and seriously damages the ecological environment. Except for a small amount of overburden used for mine reclamation, the rest is still stacked and taken up space; some stone powder is also used as filler in concrete, but cement-based cementitious materials are sensitive to particles with a particle size of less than 0.075mm, resulting in limited stone powder dosage and inability to use it in large quantities; the flocculant contained in the filter cake is easy to absorb admixtures such as water reducer, making the admixture ineffective.

[0003] Carbon neutrality is a hot topic of concern around the world. Existing buildings are still dominated by cement-based cementitious materials, but the cement production process releases a large amount of CO2. To promote the realization of the carbon neutrality goal, it is necessary to reduce the carbon emissions of cement or adopt new cementitious materials to replace cement. For example, the master's thesis of Inner Mongolia University of Science and Technology, "Experimental Research on the Development of New Cementitious Materials Based on Phosphogypsum and Slag from Jinchuan No. 2 Mine", uses industrial solid waste phosphogypsum and Tangshan Iron and Steel slag powder as the main raw materials, and combines quicklime, sodium hydroxide, mirabilite and other substances to prepare a new type of cementitious material with strength properties that meet the requirements of layered filling and good economy. In terms of patents, the invention patents disclosed include "Method for producing new cementitious materials using industrial waste slag and slag" with announcement number CN201811200282.4, "A new cementitious material with clinker-free tailings filling" CN201910634842.5, and "A process for preparing new calcium-magnesium cementitious materials by decolorizing halogen-containing gypsum", etc. These studies and patents show that the use of various solid wastes to prepare new cementitious materials is an important way to dispose of solid waste and recycle resources. However, research on the preparation of new cementitious materials using tailings produced by granite mine overburden, weathering layer, and aggregate production as the main raw materials is relatively rare, and there is no specific utilization plan. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a new type of cementitious material produced by using solid waste from granite mines.

[0005] The object of the present invention is achieved through the following technical scheme: A method for preparing a new type of cementitious material produced by using solid waste from granite mines, which is made from a granite mine overburden layer, weathered layer sand washing solid waste, and machine-made sand filter cake, and comprises the following specific steps:

[0006] (1) Take the washed sand and weak materials for filter pressing, and control the moisture content at 20%;

[0007] (2) Weighing each raw material according to the weight ratio, forcibly stirring and uniformly obtaining a mixture a; the weight ratio of each raw material component is: sand washing mud 40% to 70%, weak material 15% to 45%, filter cake 7% to 30%;

[0008] (3) calcining the mixture a in a calcining furnace for 2 to 4 hours, with the combustion chamber temperature controlled at 800 to 900° C.;

[0009] (4) annealing and cooling to obtain a mixture b;

[0010] (5) Grind the mixture b to a specific surface area of ​​300 m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0011] Furthermore, the sand washing solid waste is the sand washing mud and weak substances remaining after extracting mountain sand from the overburden layer and weathering layer of the granite mine.

[0012] Furthermore, the sand washing mud is all the substances except hard materials removed from the overburden layer and weathering layer of the granite mine before extracting the mountain sand, mainly becoming kaolin phase, weathered quartz, weathered feldspar, mica, organic matter, etc. The kaolin phase in the sand washing mud forms amorphous metakaolin after calcination, providing gelling properties. The organic matter in the sand washing mud decomposes and volatilizes after calcination, without adverse effects.

[0013] Furthermore, the weak material is the soft material removed from the overburden layer and weathered layer of the granite mine during the ball milling process of extracting mountain sand. The main components are weathered feldspar, weathered quartz, mica, etc. The weathered feldspar in the weak material forms active feldspar after calcination, which has certain gelling activity.

[0014] Furthermore, the machine-made sand filter cake is tailings generated during the production of sand and gravel aggregates in a granite mine.

[0015] Furthermore, the tailings are stone powder produced by dry-process aggregate production in granite mines and filter cake produced by wet-process aggregate production. The filter cake contains flocculants, and organic flocculants decompose and volatilize after calcination without adverse effects; inorganic flocculants contain aluminum elements, which can provide the elements required for the polymerization of aluminum oxide tetrahedrons for metakaolin after calcination.

[0016] Furthermore, other substances in the raw materials are mainly used as fillers to adjust gel strength, provide water retention and improve fluidity.

[0017] Furthermore, the use method of the novel gelling material requires that the novel gelling material has gelling activity only when it is stimulated by water glass and sodium hydroxide.

[0018] The novel cementitious material prepared by utilizing solid waste from granite mines of the present invention has the following beneficial effects:

[0019] (1) The main raw materials used in the present invention are all solid waste, which is beneficial to protecting the ecological environment;

[0020] (2) The present invention realizes the comprehensive and coordinated utilization of solid wastes such as overburden, filter cake, and stone powder in granite aggregate mines, solving the problems of high cost and technical difficulty in separate disposal;

[0021] (3) The novel cementitious material described in the present invention is not sensitive to small particles of mud and powder, and can be used to prepare high-quality concrete using aggregates with a high powder content.

[0022] (4) The new type of cementitious material described in the present invention has a fast gelling rate and can reach final setting within a few hours after molding, which can greatly improve the production efficiency of the product. If steam curing is used, the setting time can be shortened and the final strength can be improved.

[0023] (5) The new type of cementitious material described in the present invention does not release CO2 during the production process and is a new type of green and low-carbon inorganic cementitious material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0025] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail in combination with the embodiments below. The following content is only an example and explanation of the concept of the present invention. The technicians in the technical field make various modifications or supplements to the specific implementation cases described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined in the claims, they should all fall within the protection scope of the present invention.

[0026] Example 1: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0027] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0028] Step 2: Weigh the raw materials according to the weight ratio: 40% of washed sand mud, 36% of weak matter, and 24% of filter cake.

[0029] Force stirring to obtain a mixture a;

[0030] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0031] Step 4: annealing and cooling to obtain a mixture b;

[0032] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0033] Example 2: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0034] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0035] Step 2: Weigh the raw materials according to the weight ratio: 55% of washed sand mud, 28% of weak material, and 17% of filter cake.

[0036] Force stirring to obtain a mixture a;

[0037] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0038] Step 4: annealing and cooling to obtain a mixture b;

[0039] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0040] Example 3: The method for preparing a new type of cementitious material using granite mine solid waste in this example is implemented by the following steps:

[0041] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0042] Step 2: Weigh the raw materials according to the weight ratio: 70% of washed sand mud, 17% of weak matter, and 13% of filter cake.

[0043] Force stirring to obtain a mixture a;

[0044] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0045] Step 4: annealing and cooling to obtain a mixture b;

[0046] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0047] Example 4: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0048] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0049] Step 2: Weigh the raw materials according to the weight ratio: 52% of washed sand mud, 15% of weak material, and 33% of filter cake.

[0050] Force stirring to obtain a mixture a;

[0051] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0052] Step 4: annealing and cooling to obtain a mixture b;

[0053] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0054] Example 5: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0055] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0056] Step 2: Weigh the raw materials according to the weight ratio: 59% of washed sand mud, 30% of weak material, and 11% of filter cake.

[0057] Force stirring to obtain a mixture a;

[0058] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0059] Step 4: annealing and cooling to obtain a mixture b;

[0060] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0061] Example 6: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0062] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0063] Step 2: Weigh each raw material according to the weight ratio: 48% of washed sand mud, 45% of weak material, and 7% of filter cake.

[0064] Force stirring to obtain a mixture a;

[0065] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0066] Step 4: annealing and cooling to obtain a mixture b;

[0067] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0068] Example 7: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0069] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0070] Step 2: Weigh each raw material according to the weight ratio: 67% of washed sand mud, 23% of weak matter, and 0% of filter cake.

[0071] Force stirring to obtain a mixture a;

[0072] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0073] Step 4: annealing and cooling to obtain a mixture b;

[0074] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0075] Example 8: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0076] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0077] Step 2: Weigh the raw materials according to the weight ratio: 45% of washed sand mud, 40% of weak material, and 15% of filter cake.

[0078] Force stirring to obtain a mixture a;

[0079] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0080] Step 4: annealing and cooling to obtain a mixture b;

[0081] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0082] Example 9: The method for preparing a new type of cementitious material using solid waste from granite mines in this example is implemented by the following steps:

[0083] Step 1: Take the washed sand and mud and weak substances for filter pressing, and control the moisture content at about 20%;

[0084] Step 2: Weigh the raw materials according to the weight ratio: 51% of washed sand mud, 19% of weak material, and 30% of filter cake.

[0085] Force stirring to obtain a mixture a;

[0086] Step 3, calcining the mixture a in a calcining furnace for 2 to 4 hours, and controlling the combustion chamber temperature at 800 to 900° C.;

[0087] Step 4: annealing and cooling to obtain a mixture b;

[0088] Step 5: Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or the 45 micron sieve residue is less than 30%, and a new type of cementitious material of granite mine solid waste is obtained.

[0089] The raw material ratios of Examples 1 to 9 are shown in Table 1:

[0090] Table 1 Ratio of raw materials in Examples 1 to 9

[0091] Sand washing mud (%) Weak substances (%) Filter cake (%) Example 1 40 36 24 Example 2 55 28 17 Example 3 70 17 13 Example 4 52 15 33 Example 5 59 30 11 Example 6 48 45 7 Example 7 67 23 0 Example 8 45 40 15 Example 9 51 19 30

[0092] The new gelling materials obtained in the above examples 1 to 9 were tested for performance. Strength test conditions: water glass and sodium hydroxide were used as the activator, the alkali equivalent was fixed at 30%, the modulus of the activator was 1.8, and the water-solid ratio was 0.6. The test results are shown in Table 2:

[0093] Table 2 Test results of Examples 1 to 9

[0094]

[0095]

[0096] It is understandable that, for those skilled in the art, any equivalent replacement or change to the technical solution and inventive concept of the present invention should fall within the protection scope of the claims attached to the present invention.

Claims

1. A method for preparing a new type of cementitious material produced by using solid waste from granite mines, characterized in that: It is made of sand washing solid waste and machine-made sand filter cake. The sand washing solid waste is the sand washing mud and weak substances left after extracting mountain sand from the overburden layer and weathering layer of the granite mine, and includes the following specific steps: (1) Take the washed sand and weak materials for filter pressing, and control the moisture content at 20%; (2) Weigh each raw material according to the weight ratio, forcefully stir evenly, and obtain a mixture a; the weight ratio of each raw material component is: sand washing mud 40%~70%, weak material 15%~45%, machine-made sand filter cake 7%~30%; (3) calcining the mixture a in a calcining furnace for 2 to 4 hours, with the combustion chamber temperature controlled at 800 to 900°C; (4) After annealing and cooling, a mixture b is obtained; (5) Grind the mixture b to a specific surface area of ​​300m 2 / kg or more or less than 30% of the 45 micron sieve residue, to obtain a new type of cementitious material from granite mine solid waste; The sand washing mud comprises kaolin phase, weathered quartz, weathered feldspar, mica, and organic matter. The kaolin phase in the sand washing mud forms amorphous metakaolin after calcination, providing gelling properties; The weak material is the soft material removed from the overburden layer and weathered layer of the granite mine during the ball milling process of extracting mountain sand. The weathered feldspar in the weak material forms active feldspar after calcination and has certain gelling activity. The machine-made sand filter cake is tailings produced in the process of producing sand and gravel aggregates in granite mines. The tailings are stone powder produced by dry-process aggregate production in granite mines and filter cakes produced by wet-process aggregate production. The filter cake contains flocculants, and the organic flocculants are decomposed and volatilized after calcination. The inorganic flocculant contains aluminum element, which provides the elements required for the polymerization of aluminum oxide tetrahedron to the kaolin after calcination.