Catalyst and its preparation method and application

By using a catalyst with MOF skeleton derived structural support and Fe active ingredients, the low performance problem caused by the complexity of the construction of Fe-based catalyst activity center is solved, and the efficient catalysis of CO2 hydrogenation is achieved, which is suitable for industrial applications.

CN116139896BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111376025.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-19
Publication Date
2024-12-06
Estimated Expiration
2041-11-19

AI Technical Summary

Technical Problem

The complexity of the construction of active centers in existing Fe-based catalysts leads to low catalytic performance, making it difficult to effectively improve the efficiency of CO2 hydrogenation to prepare low-carbon olefins.

Method used

The catalyst with a support with a MOF skeleton derived structure and a Fe active ingredient are prepared by mixing and calcining the imidazole and a metal source to form active centers such as Fe3O4 and Fe5C2, thereby improving the dispersion and reaction activity of the catalyst.

Benefits of technology

It significantly improves the catalytic activity and selectivity of CO2 hydrogenation to prepare low-carbon olefins, and only requires a low Fe content to achieve excellent catalytic effect, which is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116139896B_ABST
    Figure CN116139896B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of catalysts, and discloses a catalyst and a preparation method and application thereof. A catalyst comprises a carrier having a MOF skeleton-derived structure and an active component Fe, wherein the content of the active component is 1-40% based on the total mass of the catalyst and the Fe element. The catalyst provided by the present invention contains a carrier having a specific MOF skeleton-derived structure, so that the catalyst has excellent catalytic reaction efficiency and can effectively improve the efficiency of CO2 hydrogenation to produce light olefins. The method of the present invention is simple to operate, easy to implement, and can be suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a catalyst and a preparation method and application thereof. Background Art

[0002] The large-scale use of fossil fuels such as coal, oil, and natural gas, along with changes in land use, has led to an increasing amount of carbon dioxide emissions in the atmosphere. While the economy is booming, it has also brought a great burden to our living environment, making global warming and ocean acidification more serious. In order to achieve the dual carbon emission goals, in addition to deploying renewable energy and improving the efficiency of existing energy, strategies such as CO2 capture, storage, and secondary utilization can be used to reduce CO2 emissions.

[0003] CO2 is a linear triatomic molecule with a symmetrical structure, with carbon and oxygen atoms connected by covalent bonds. Since the bond length of its C=O bond is shorter than that of ketone, more energy is required for bond breaking, which is reflected in better thermodynamic stability. In order to overcome the barrier of high energy barrier and obtain the required energy in activation and conversion, another substance with relatively high Gibbs energy can be added, so the use of high-energy and renewable H2 to catalyze CO2 hydrogenation reaction is considered to be a promising direction. Low-carbon olefins are essential chemical raw materials. For example, ethylene and propylene, which are the top two petrochemical products in the world. In 2017, the annual consumption of ethylene and propylene in the world was about 150 million tons and 100 million tons, respectively. The high demand for low-carbon olefins is due to their use as basic materials for the production of plastics, polymers, solvents and cosmetics in the chemical industry. At the same time, olefin oligomerization into long-chain hydrocarbons for fuel has high potential as an ideal low-molecular-weight target product.

[0004] Many catalysts used for CO2 hydrogenation to produce light olefins are based on Fischer-Tropsch synthesis catalysts because they have similar reaction principles and active components. In terms of converting CO2 into hydrocarbons, Fe, Co, Ru and Ni catalysts supported on SiO2, γ-Al2O3, TiO2 and carbon nanomaterials have been comprehensively studied. Among them, iron-based catalysts are widely used in Fischer-Tropsch-like CO2 reactions. On the one hand, they are highly active in both reverse water gas shift (RWGS) and Fischer-Tropsch reactions. On the other hand, Fe catalysts can inhibit CO2 methanation and secondary hydrogenation of olefins, thereby improving the selectivity of light olefins in the product. However, at this stage, limited by the complexity of the construction of active centers in Fe-based catalysts, how to further improve the performance of catalytic centers has become a key scientific issue restricting the hydrogenation of CO2 to produce light olefins. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem of low catalytic center performance caused by the complexity of the construction of active centers in catalysts in the prior art, and to provide a catalyst and a preparation method and application thereof. The catalyst contains a carrier with a specific MOF skeleton-derived structure, so that the catalyst has good catalytic reaction efficiency and effectively improves the efficiency of CO2 hydrogenation to produce light olefins.

[0006] In order to achieve the above object, the first aspect of the present invention provides a catalyst, which includes a carrier having a MOF framework-derived structure and an active ingredient Fe, wherein the content of the active ingredient is 1-40% based on the total mass of the catalyst and calculated as Fe element.

[0007] Preferably, in the catalyst, Fe exists in the form of Fe3O4 and Fe5C2.

[0008] A second aspect of the present invention provides a method for preparing a catalyst, the method comprising the following steps:

[0009] (1) mixing imidazole and / or an imidazole derivative, an M metal source, an Fe source, and an organic solvent to obtain a precursor precipitate;

[0010] (2) In an inert atmosphere or a reducing atmosphere, the precursor is precipitated and calcined.

[0011] The third aspect of the present invention provides the use of the catalyst described in the first aspect or the catalyst prepared by the preparation method described in the second aspect in the preparation of olefins by CO2 hydrogenation.

[0012] In the present invention, a catalyst containing a specific MOF skeleton-derived structure carrier is provided. The MOF skeleton-derived structure can promote the dispersion of Fe active centers in the catalyst and increase the contact area between metal and reactants in the catalytic reaction. The active centers constructed by Fe in the catalyst and metal heteroatoms in the MOF skeleton-derived structure can further utilize the electron donation effect of heteroatoms to promote the co-adsorption effect of CO2 molecules and H2 molecules on the surface of the active centers, greatly improving the catalytic activity and selectivity in the CO2 hydrogenation reaction to prepare light olefins. During the reaction, only a lower Fe content is required to achieve an excellent catalytic effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 is a SEM image of the catalyst prepared in Example 1 of the present invention;

[0014] Figure 2 is a TEM image of the catalyst prepared in Example 1 of the present invention;

[0015] Figure 3 is the Mössbauer plot of the catalyst prepared in Example 1 of the present invention;

[0016] Figure 4 is a SEM image of the catalyst prepared in Example 8 of the present invention;

[0017] Figure 5 is a TEM image of the catalyst prepared in Example 8 of the present invention;

[0018] Figure 6 is a SEM image of the catalyst prepared in Example 13 of the present invention;

[0019] Figure 7 is a TEM image of the catalyst prepared in Example 16 of the present invention;

[0020] Figure 8 This is a comparison chart of the catalytic CO2 hydrogenation activities of the catalysts prepared in Example 1 of the present invention and Comparative Example 1;

[0021] Fig. 9 1 is a comparison chart of the catalytic CO2 hydrogenation activities of the catalysts prepared in Example 16 of the present invention and in Comparative Example 1;

[0022] Fig.10 is a comparison chart of the catalytic CO2 hydrogenation activities of the catalysts prepared in Examples 2, 3, 4 and 5 of the present invention;

[0023] Fig.11 This is a comparison chart of the catalytic CO2 hydrogenation activities of the catalysts prepared in Examples 17, 18 and 19 of the present invention. DETAILED DESCRIPTION

[0024] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0025] In this specification, the numerical range expressed using "numerical value A - numerical value B" means a range including the endpoint numerical values ​​A and B.

[0026] In this specification, unless otherwise stated, "multiple" in "multiple", "multiple", "plurality", etc. means a numerical value of 2 or more.

[0027] In this specification, unless otherwise specified, "%" means mass percentage.

[0028] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0029] In the present specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes cases where the event occurs and cases where it does not occur.

[0030] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0031] The first aspect of the present invention provides a catalyst, which includes a carrier having a MOF framework-derived structure and an active component Fe, wherein the content of the active component is 1-40% based on the total mass of the catalyst and calculated as Fe element.

[0032] In the present invention, the MOF skeleton derivative structure refers to a CN derivative having a MOF skeleton, and the carrier derivative means using MOFs as characteristic precursors to achieve in-situ decomposition under an inert atmosphere (for example, N2) or a reducing atmosphere (for example, a mixed atmosphere of N2 and H2), while maintaining the porous characteristics of the MOF structure to obtain a carrier.

[0033] The MOF skeleton-derived structure of the present invention can be characterized and measured by SEM, TEM, and N2 adsorption and desorption. Specifically, the average particle size of the carrier and the catalyst is measured by SEM and TEM, and the specific surface area and pore volume of the catalyst are measured by N2 adsorption and desorption to characterize the MOF skeleton-derived structure.

[0034] In a preferred embodiment, the content of the active ingredient is 2-30%. The advantage of adopting this preferred embodiment is that the content of highly dispersed Fe active centers can be controlled.

[0035] In a preferred embodiment, in the catalyst, Fe exists in the form of Fe3O4 and Fe5C2. The advantage of adopting this preferred embodiment is to utilize the rich pore structure of the CN carrier of the MOF-derived carrier to construct abundant and accessible Fe active centers.

[0036] In the present invention, the presence of Fe3O4 and Fe5C2 in the catalyst can be measured by Mossbauer spectroscopy.

[0037] In the present invention, the carrier having a MOF framework-derived structure contains a metal framework component, and the type of the metal framework component can be selected from a wide range. Preferably, the metal framework component in the carrier having a MOF framework-derived structure is at least one of Co, Zn, Cu and Mn.

[0038] In the present invention, the content of the metal skeleton component can be selected in a wide range. Preferably, based on the weight of the catalyst, the content of the metal skeleton component is 10-40%, preferably 15-35%. The advantage of adopting this preferred embodiment is that the heteroatom metal skeleton is more evenly distributed.

[0039] In a preferred embodiment, based on the total mass of the catalyst, the nitrogen content in the carrier is 0.5-10%, and the carbon content is 0.5-10%.

[0040] In a preferred embodiment, the catalyst further comprises an alkali metal, and the purpose of adopting this preferred embodiment is to further control and optimize the product distribution and maximize the olefin production. There is no specific limitation on the content of the alkali metal in the present invention. Preferably, the alkali metal content is 1-20%, preferably 2-10%, based on the total mass of the catalyst.

[0041] In the present invention, there is no specific limitation on the type of alkali metal, and conventional alkali metals in the art are suitable for the present invention. Preferably, the alkali metal is selected from at least one of Li, Na, K and Rb, and more preferably Na and / or K.

[0042] In a preferred embodiment, the average particle size of the carrier having a MOF framework-derived structure is 0.3-2 μm. The advantage of adopting this preferred embodiment is that the carrier having a MOF framework-derived structure can confine the active components to a certain extent, thereby controlling the particle size within a certain range, so that the structure-sensitive reaction can be controlled and the active sites can be utilized to the maximum extent.

[0043] In a preferred embodiment, the average particle size of the active ingredient is 5-100 nm.

[0044] In the present invention, the average particle sizes of the carrier and active ingredients of the MOF framework-derived structure are measured by SEM and TEM.

[0045] In a preferred embodiment, the specific surface area of ​​the catalyst is 20-300 m 2 / g.

[0046] In a preferred embodiment, the pore volume of the catalyst is 0.1-0.6 cm 3 / g.

[0047] In the present invention, the specific surface area and pore volume of the catalyst are measured by N2 physical adsorption and desorption test.

[0048] In the present invention, the provided catalyst has a large specific surface area and pore volume, and the catalyst has excellent activity and selectivity, and can further improve the reaction efficiency of the catalyst in the CO2 hydrogenation reaction to prepare light olefins.

[0049] A second aspect of the present invention provides a method for preparing a catalyst, the method comprising the following steps:

[0050] (1) mixing imidazole and / or an imidazole derivative, an M metal source, an Fe source, and an organic solvent to obtain a precursor precipitate;

[0051] (2) In an inert atmosphere or a reducing atmosphere, the precursor is precipitated and calcined.

[0052] The preparation method provided by the invention is simple and easy to implement, the raw materials are easy to obtain, and it is suitable for industrial mass production.

[0053] In the present invention, the type of imidazole and / or imidazole derivative in step (1) can be selected from a wide range, as long as it can meet the preparation requirements of the catalyst. Preferably, the imidazole and / or imidazole derivative is selected from at least one of 2-methylimidazole, 1-methylimidazole, 4-methylimidazole, 5-methylimidazole, 1-ethylimidazole and 2-ethylimidazole, more preferably 2-methylimidazole.

[0054] In the present invention, there is no specific restriction on the type of the M metal source in step (1), and those skilled in the art can make a conventional selection according to specific needs. Preferably, the M metal in the M metal source is selected from at least one of Co, Zn, Cu and Mn. In a preferred embodiment, the M metal source is selected from at least one of Co(NO3)2, CoCl3, Zn(NO3)2, ZnCl2, KMnO4, Na3MnO4, CuCl2 and Cu(NO3)2. The M metal source can be selected from the above substances, and can also be selected from the above substances with crystallization water. For example, the M metal source with crystallization water can be Co(NO3)2·6H2O and / or Zn(NO3)2·6H2O.

[0055] In the present invention, there is no specific limitation on the type of organic solvent in step (1), as long as it can provide a reaction environment. Preferably, the organic solvent is selected from methanol and / or ethanol. The organic solvent can be selected from the above substances, and can also be selected from anhydrous methanol and / or anhydrous ethanol.

[0056] According to the present invention, preferably, the Fe source is an Fe complex prepared by complexing an Fe salt with an organic amine. This preferred embodiment is more conducive to improving the stability of the Fe metal in the mixture, thereby improving the dispersion of the metal in the catalyst.

[0057] In a preferred embodiment, the Fe salt is selected from at least one of FeCl2, FeCl3, FeSO4, Fe2(SO4)3, Fe(NO3)3 and Fe(C5H7O2)3, and is further preferably selected from at least one of FeCl2, FeCl3 and Fe(C5H7O2)3.

[0058] In a preferred embodiment, the organic amine is ethylenediamine and / or N-[3-(trimethoxysilyl)propyl]ethylenediamine.

[0059] In the present invention, there is no specific limitation on the amount of Fe salt and organic amine used. Preferably, the molar ratio of Fe salt to organic amine calculated as Fe element is 1:1-6.

[0060] In the present invention, there is no specific limitation on the preparation method of the Fe complex, and conventional preparation methods in the art are applicable to the present invention. For example, it can be prepared by the following method: in the presence of a solvent (preferably methanol), an Fe salt and an organic amine are mixed. There is no particular limitation on the temperature of the mixing, and it can be carried out at room temperature (e.g., 20-30° C.). Preferably, the mixing is carried out under stirring conditions. In the present invention, there is no specific limitation on the stirring conditions. Preferably, the stirring time is 1-10 hours.

[0061] In the present invention, there is no specific restriction on the amount of each substance used in step (1), as long as it can meet the preparation requirements of the catalyst. Preferably, the molar ratio of imidazole and / or imidazole derivative, M metal source, Fe source and organic solvent is (2-50):1:(0.01-4):(30-500), preferably (5-40):1:(0.02-2):(50-300).

[0062] In the present invention, the mixing conditions of the substances in step (1) are not specifically limited. Preferably, in the presence of an organic solvent, imidazole and / or an imidazole derivative and the M metal source are dissolved separately to obtain a mixture. Preferably, the dissolution is carried out under stirring conditions. In the present invention, the stirring conditions in step (1) can be selected in a wide range. Preferably, the stirring temperature is 20-30° C. and the time is 2-24 h.

[0063] According to the present invention, the method further comprises: centrifuging and filtering the mixture to obtain a precursor precipitate.

[0064] In a preferred embodiment, the method further comprises impregnating the precursor precipitate with an alkali metal salt impregnation solution, and then performing the step (2). The purpose of adopting this preferred embodiment is to adjust the surface electronic properties and acidity and alkalinity of the carrier in the precursor precipitate to improve the surface adsorption capacity and activation capacity of the carrier.

[0065] In the present invention, the types of alkali metals have been described in the first aspect of the present invention and will not be described in detail here.

[0066] In the present invention, the alkali metal is provided by a metal salt containing an alkali metal. Preferably, the alkali metal salt is selected from at least one of NaCl, NaNO3, KCl and KNO3.

[0067] According to the present invention, preferably, the alkali metal salt is used in an amount such that the alkali metal content in the prepared catalyst is 1-20%, preferably 2-10%, based on the total mass of the catalyst.

[0068] In the present invention, there is no specific limitation on the impregnation method, and all conventionally defined impregnation methods in the art are applicable to the present invention. For example, excess impregnation method, equal volume impregnation method, multiple impregnation method, impregnation precipitation method, etc. Preferably, the precursor precipitate is impregnated by equal volume impregnation method. Specifically, the following method can be used: dissolve the alkali metal salt in a solvent (preferably water) to obtain an alkali metal-containing impregnation solution, stir the impregnation solution evenly and add it dropwise to the precursor precipitate, then dry it, and finally dry it overnight. In the present invention, the specific conditions for drying have a wide range of selection. Preferably, the drying temperature is 20-60°C, and the time is 6-12h. In the present invention, the specific conditions for drying overnight have a wide range of selection. Preferably, the temperature for drying overnight is 80-140°C, and the time is 6-24h.

[0069] In order to obtain an appropriate amount of alkali metal loading, a small amount of multiple impregnations may be used. The present invention has no specific restrictions on the number of impregnations and specific operations, and those skilled in the art may perform the operations according to conventional procedures.

[0070] In the present invention, preferably, the method further comprises washing and / or drying the precursor precipitate, and then performing the step (2); washing and drying are further preferred. In the present invention, there is no specific restriction on the type of detergent used for washing, and those skilled in the art can select it according to actual needs. Preferably, the detergent is methanol and water. In the present invention, there is no specific restriction on the washing conditions. Preferably, the washing method is alternating washing, and the number of washings is 1-5 times. In the present invention, the range of drying conditions is relatively wide. Preferably, the drying temperature is 20-60°C, and the time is 6-24h. In the present invention, the precipitated precursor is washed and / or dried to obtain a dried product, and then the dried product is dried overnight. Preferably, the temperature of the overnight drying is 80-140°C, and the time is 6-24h.

[0071] In the present invention, the type of the inert atmosphere or reducing atmosphere in step (2) is not specifically limited, and the inert atmosphere or reducing atmosphere conventionally defined in the art is applicable to the present invention. Preferably, in step (2), the inert atmosphere is provided by an inert gas, and the reducing atmosphere is provided by H2 and optionally an inert gas.

[0072] In a preferred embodiment, the inert gas is selected from at least one of N2, helium, neon and argon.

[0073] In a particularly preferred embodiment, the reducing atmosphere is a mixed atmosphere of H2 and N2. The advantage of adopting this preferred embodiment is that the high temperature atmosphere after N2 mixed with H2 has a milder decomposition effect on the MOF precursor skeleton, which can keep the morphology of the MOF skeleton-derived structure more stable.

[0074] In a preferred embodiment, in step (2), calcination is carried out in a mixed atmosphere of N2 and H2, and more preferably, the volume ratio of N2 to H2 is 1:(0.1-1).

[0075] According to the present invention, the calcination process is carried out in a reducing atmosphere. Preferably, the calcination conditions include: a flow rate of 40-200 mL min -1 , heating rate is 0.5-3℃min -1 .

[0076] In a preferred embodiment, the calcination conditions include: a calcination temperature of 300-750° C. and a calcination time of 2-48 hours; more preferably, the calcination temperature is 450-600° C. and the calcination time is 2-4 hours.

[0077] The third aspect of the present invention provides the use of the catalyst described in the first aspect or the catalyst prepared by the preparation method described in the second aspect in the preparation of olefins by CO2 hydrogenation.

[0078] Preferably, the conditions for the CO2 hydrogenation reaction to produce olefins include: a reaction pressure of 1-4 MPa, a reaction temperature of 300-600°C, a volume space velocity of 2-12 L g -1 h -1 , the volume ratio of H2 / CO2 / N2 is 69 / 23 / 8.

[0079] In the present invention, before the CO2 hydrogenation reaction to prepare olefins, the reaction device needs to be checked for air tightness. Preferably, nitrogen is first introduced to adjust the pressure of the device to be higher than the required pressure to check the air tightness of the device, and more preferably, the device pressure is 3-5MPa higher than the required pressure.

[0080] In the present invention, the catalyst needs to be subjected to reduction treatment before use. Preferably, the reduction treatment comprises: conducting the reduction treatment in a reducing atmosphere, preferably hydrogen, at a reduction temperature of 300-600° C. for 1-5 hours.

[0081] The present invention will be described in detail by way of examples below. In the following examples, all raw materials used are commercially available unless otherwise specified. The water used in the present invention is deionized water, and the reagents used are analytically pure reagents; the high-power transmission microscope test of the obtained catalyst is carried out using JEM-2100, with an accelerating voltage of 200KV; the field emission scanning electron microscope image of the obtained catalyst is carried out using Hitachi S4800; the pore volume and specific surface area are obtained by testing on a Micomeritics ASAP 2420 instrument; the composition of the catalyst is measured by ICP-OES test.

[0082] Example 1

[0083] 2g of ferric acetylacetonate (Fe(C5H7O2)3) and 1.235g of ethylenediamine were added to 10mL of methanol and stirred at room temperature for 1 hour to prepare Fe-complexed ethylenediamine solution. 1.127g of Fe-complexed ethylenediamine solution, 3.28g of 2-methylimidazole and 1.425g of Co(NO3)2·6H2O were dissolved in 30mL of anhydrous methanol respectively. The two solutions were then mixed and stirred at room temperature for 24h. A purple precipitate was obtained after centrifugal filtration, and was washed alternately with water and methanol for 3 times and then dried. Finally, the MOF material containing Fe-Co metal was obtained after drying in an oven at 100°C overnight.

[0084] Furthermore, the conventional equal volume impregnation method was used to make an aqueous NaNO3 solution (0.133 g of NaNO3 dissolved in 1.5 g of water), which was then evenly stirred in a beaker with a built-in magnet and then added dropwise to 1 g of MOF material containing Fe-Co metal. The obtained product was dried at 25 °C for 8 h and dried in an oven at 110 °C overnight. This impregnation behavior was repeated five times in total. The obtained sample was named Fe / Co-MOF. Fe / Co-MOF was placed in a N2-H2 atmosphere (N2 / H2 volume ratio = 1:0.2, 40 mL min -1 ) at 3℃min -1 The temperature was raised to 500°C and calcined for 2 hours, then cooled to 25°C. The obtained product was named Fe-Co / NC, and the composition of the product was obtained by ICP-OES test as shown in Table 1. The SEM image of the catalyst obtained in Example 1 is shown in Figure 1 As shown, the macroscopic size of the catalyst carrier is 1 μm. Figure 2 As shown in Figure 2, the average particle size of the metal active center is 15.82nm. The specific surface area of ​​the catalyst is 110m 2 / g, pore volume 0.35cm 3 / g, the Mössbauer spectrum of the catalyst is as follows Figure 3 As shown, the relevant parameters are shown in Table 2. It can be seen that the active components Fe in the catalyst are Fe3O4 and Fe5C2.

[0085] Example 2

[0086] Example 2 The method of Example 1 was followed, except that the mass of Co(NO3)2·6H2O used was 1.062 g, the mass of NaNO3 was 0.106 g, and the composition of the product was shown in Table 1. The average particle size of the metal active center was 12.11 nm, and the specific surface area of ​​the catalyst was 121 m 2 / g, pore volume 0.33cm 3 / g.

[0087] Example 3

[0088] Example 3 The method of Example 1 was followed, except that the mass of Co(NO3)2·6H2O used was 1.247 g, the mass of NaNO3 was 0.115 g, and the composition of the product was shown in Table 1. The average particle size of the metal active center was 11.86 nm, and the specific surface area of ​​the catalyst was 126 m 2 / g, pore volume 0.37cm 3 / g.

[0089] Example 4

[0090] Example 4 The method of Example 1 was followed, except that the mass of Co(NO3)2·6H2O used was 1.679 g, the mass of NaNO3 was 0.148 g, and the composition of the product was shown in Table 1. The average particle size of the metal active center was 15.51 nm, and the specific surface area of ​​the catalyst was 134 m 2 / g, pore volume 0.39cm 3 / g.

[0091] Example 5

[0092] Example 5 The method of Example 1 was followed, except that the mass of Co(NO3)2·6H2O used was 1.824 g, the mass of NaNO3 was 0.151 g, and the composition of the product was shown in Table 1. The average particle size of the metal active center was 13.63 nm, and the specific surface area of ​​the catalyst was 140 m 2 / g, pore volume 0.32cm 3 / g.

[0093] Example 6

[0094] 3.861g of FeCl3 and 1.961g of ethylenediamine were added to 10mL of methanol and stirred at room temperature for 1 hour to prepare Fe-complexed ethylenediamine solution. 1.312g of Fe-complexed ethylenediamine solution, 3.28g of 2-methylimidazole and 1.425g of Co(NO3)2·6H2O were dissolved in 30mL of anhydrous methanol respectively. The two solutions were then mixed and stirred at room temperature for 24h. After centrifugal filtration, the MOF material containing Fe-Co metal was obtained after drying overnight. A purple precipitate was obtained, and it was washed alternately with water and methanol 3 times and then dried. Finally, the MOF material containing Fe-Co metal was obtained after drying in an oven at 100°C overnight.

[0095] Furthermore, the conventional equal volume impregnation method was used to prepare an aqueous NaNO3 solution (0.133 g NaNO3 dissolved in 1.5 g water), which was then uniformly stirred in a beaker with a built-in magnetic device and then added dropwise to 1 g of the MOF material containing Fe-Co metal. The obtained product was dried at 25 °C for 8 h and dried in an oven at 110 °C overnight, and the impregnation was repeated five times. The obtained sample was named Fe / Co-MOF. Fe / Co-MOF was placed in a N2-H2 atmosphere (N2 / H2 volume ratio = 1:0.4, atmosphere (40 mL min -1 ) at 3℃min -1 The temperature was raised to 500°C at a rate and maintained for 2 h, and then cooled to 25°C. The obtained product was named Fe-Co / NC, and the composition of the product is shown in Table 1.

[0096] Example 7

[0097] Example 7 The method of Example 6 was followed, except that the mass of FeCl2 used was 4.125 g, and the composition of the product was shown in Table 1. The average particle size of the metal active center was 20.02 nm, and the specific surface area of ​​the catalyst was 121 m 2 / g, pore volume 0.357cm 3 / g.

[0098] Example 8

[0099] Example 8 The method of Example 6 was followed, except that the mass of FeCl3 used was 3.622 g, and the composition of the product was shown in Table 1. The SEM image of the catalyst obtained in Example 8 is shown in Figure 4 As shown, the macroscopic size of the catalyst carrier is 700nm. The TEM image is shown in Figure 5 The average particle size of the metal active center is 22.15 nm, and the specific surface area of ​​the catalyst is 124 m 2 / g, pore volume 0.384cm 3 / g.

[0100] Example 9

[0101] Example 9 The method of Example 6 was followed, except that the mass of FeCl3 used was 3.276 g, and the composition of the product was shown in Table 1. The average particle size of the metal active center was 19.63 nm, and the specific surface area of ​​the catalyst was 132 m 2 / g, pore volume 0.362cm 3 / g.

[0102] Example 10

[0103] Example 10 The method of Example 6 was followed, except that the mass of Fe(C5H7O2)3 used was 2.012 g, and the composition of the product was shown in Table 1. The average particle size of the metal active center was 19.77 nm, and the specific surface area of ​​the catalyst was 135 m 2 / g, pore volume 0.341cm 3 / g.

[0104] Embodiment 11

[0105] 2g of ferric acetylacetonate (Fe(C5H7O2)3) and 1.235g of ethylenediamine were added to 10mL of methanol and stirred at room temperature for 1 hour to prepare Fe-complexed ethylenediamine solution. 1.127g of Fe-complexed ethylenediamine solution, 3.28g of 2-methylimidazole and 1.425g of Co(NO3)2·6H2O were dissolved in 30mL of anhydrous methanol respectively. The two solutions were then mixed and stirred at room temperature for 24h. A purple precipitate was obtained after centrifugal filtration, and was washed alternately with water and methanol for 3 times and then dried. Finally, the MOF material containing Fe-Co metal was obtained after drying in an oven at 100°C overnight.

[0106] Furthermore, the conventional equal volume impregnation method was used to make an aqueous NaNO3 solution (0.133 g NaNO3 dissolved in 1.5 g water), which was then evenly stirred in a beaker with a built-in magnet and then added dropwise to 1 g of MOF material containing Fe-Co metal. The obtained product was dried at 25 °C for 8 h and dried in an oven at 110 °C overnight. This impregnation behavior was repeated five times in total. The obtained sample was named Fe / Co-MOF. Fe / Co-MOF was placed in a N2-H2 atmosphere (N2 / H2 volume ratio = 1:0.2, 40 ml min -1 ) at 3℃min -1 The temperature was raised to 400°C at a rate and maintained for 2 h, and then cooled to 25°C. The obtained product was named Fe-Co / NC, and the composition of the product is shown in Table 1.

[0107] Example 12

[0108] Example 12 is carried out according to the method of Example 11, except that the calcination temperature is 450°C and the calcination time is 3 hours.

[0109] Embodiment 13

[0110] Example 13 The method of Example 11 was followed, except that the calcination temperature was 500°C and the calcination time was 3 h. The SEM image of the catalyst prepared in Example 13 is shown in FIG. Figure 6 As shown, the size of the catalyst macrocarrier is 600 nm and the specific surface area of ​​the catalyst is 103 m 2 / g, pore volume 0.354cm 3 / g.

[0111] Embodiment 14

[0112] Example 14 is carried out according to the method of Example 11, except that the calcination temperature is 550°C and the calcination time is 3 hours.

[0113] Embodiment 15

[0114] Example 15 follows the method of Example 11, except that the calcination temperature is 600°C and the time is 3 hours.

[0115] Example 16

[0116] 2g of ferric acetylacetonate (Fe(C5H7O2)3) and 1.235g of ethylenediamine were added to 10mL of methanol and stirred at room temperature for 1 hour to prepare Fe-complexed ethylenediamine solution. 1.127g of Fe-complexed ethylenediamine solution, 3.28g of 2-methylimidazole and 1.47g of Zn(NO3)2·6H2O were dissolved in 30mL of anhydrous methanol respectively. The two solutions were then mixed and stirred at room temperature for 24h. A purple precipitate was obtained after centrifugal filtration, and was washed alternately with water and methanol 3 times and then dried. Finally, the MOF material containing Fe-Zn metal was obtained after drying in an oven at 100°C overnight.

[0117] Furthermore, the conventional equal volume impregnation method was used to dissolve an aqueous NaNO3 solution (0.133 g NaNO3 in 1.5 g water), which was then evenly stirred in a beaker with a built-in magnet and then added dropwise to 1 g of the MOF material containing Fe-Co metal. The obtained product was dried at 25 °C for 8 h and dried in an oven at 110 °C overnight. This impregnation behavior was repeated five times in total. The obtained sample was named Fe / Zn-MOF. Fe-Zn / MOF was placed in a N2-H2 atmosphere (N2 / H2 volume ratio = 1:0.2, 40 mL min -1 ) at 3℃min -1 The temperature was raised to 500°C at a rate of 100 °C and maintained for 2 h, and then cooled to 25°C. The obtained product was named Fe-Zn / NC, and the composition of the product is shown in Table 1. The TEM image of the catalyst prepared in Example 16 is shown in Figure 7 As shown in the figure, it can be seen that the metal Fe is highly dispersed inside the MOF-derived carbon-nitrogen carrier, the average particle size of the metal active component is about 6 nm, and the specific surface area of ​​the catalyst is 111 m 2 / g, pore volume 0.323cm 3 / g.

[0118] Embodiment 17

[0119] The method of Example 16 was followed, except that the mass of Zn(NO3)2·6H2O used was 1.06 g. The composition of the product is shown in Table 1.

[0120] Embodiment 18

[0121] The method of Example 18 was followed, except that the mass of Zn(NO3)2·6H2O used was 0.98 g. The composition of the product is shown in Table 1.

[0122] Embodiment 19

[0123] The method of Example 19 was followed, except that the mass of Zn(NO3)2·6H2O used was 1.22 g. The composition of the product is shown in Table 1.

[0124] Comparative Example 1

[0125] Preparation method of directly supported metal Fe catalyst: Fe / γ-Al2O3 catalyst is synthesized by traditional equal volume impregnation method. Usually, 0.145g FeCl3 is dissolved in 1.8mL methanol. Then, it is evenly stirred in a beaker with a built-in magnet and added dropwise to the surface of 1g γ-Al2O3 sample. The obtained product is dried at 25°C for 8h and dried in an oven at 110°C overnight. This impregnation behavior is repeated five times in total. Then, NaNO3 aqueous solution (0.133g NaNO3 dissolved in 1.5g water) is impregnated into the obtained product in the same way. The final product is dried at 25°C for 8h and at 110°C overnight. The sample is refrigerated in a muffle furnace in an air atmosphere at 3°C ​​min -1 The temperature was raised to 550°C at a rate of 100°C, maintained for 3 hours, and then cooled to 25°C. The obtained product was named Fe / γ-Al2O3.

[0126] Table 1 Catalyst composition (mass percentage)

[0127] Catalyst composition Catalyst composition Example 1 Fe: 16.2, Co: 26.3, Na: 4.2 Example 9 Fe: 12.5, Co: 32.8, Na: 5.0 Example 2 Fe: 17.2, Co: 23.2, Na: 3.2 Example 10 Fe: 16.5, Co: 26.7, Na: 4.2 Example 3 Fe: 16.4, Co: 24.7, Na: 3.6 Embodiment 11 Fe: 15.9, Co: 25.4, Na: 4.5 Example 4 Fe: 14.8, Co: 27.8, Na: 4.7 Example 12 Fe: 16.1, Co: 26, Na: 4.3 Example 5 Fe: 14, Co: 30.5, Na: 4.9 Example 16 Fe: 20.1, Zn: 22.5, Na: 3.7 Example 6 Fe: 13.4, Co: 28.9, Na: 4.5 Embodiment 17 Fe: 19.6, Zn: 21.3, Na: 3.9 Example 7 Fe: 14.1, Co: 28.6, Na: 4.4 Embodiment 18 Fe: 19.7, Zn: 20.2, Na: 3.8 Example 8 Fe: 13.1, Co: 30.1, Na: 4.7 Embodiment 19 Fe: 21.4, Zn: 20, Na: 4.1

[0128] Note: Calculated by element, the proportion of each component in the catalyst

[0129] Table 2

[0130]

[0131]

[0132] Test Example 1

[0133] The catalyst (Fe-Co / NC) obtained in Example 1 is used in the reaction of CO2 hydrogenation to prepare light olefins, which specifically includes the following steps: an appropriate amount of catalyst (0.5g, 20-30 mesh) is mixed with 3.5g quartz sand (20-30 mesh) and loaded in the middle of the reaction tube, 20-mesh quartz sand is loaded at both ends of the catalyst bed, and a small amount of quartz wool is laid between different interfaces. Before the reaction, nitrogen is introduced first, and the pressure is adjusted to slightly higher than the required pressure through the back pressure valve to check the air tightness of the device. Then the pressure is relieved to normal pressure and purged with nitrogen for 30 minutes to remove the residual air in the tube. The gas is switched to high-purity hydrogen, and the catalyst is placed in pure hydrogen (40mLmin -1) was reduced at 400°C for 2h. Subsequently, the reactor was cooled to room temperature, and a reaction gas mixture with a volume ratio of H2 / CO2 / N2 of 69 / 23 / 8 (N2 was used as an internal standard gas) was fed into the reactor and the pressure was gradually increased to 2MPa, the temperature was raised to 350°C, and the volume space velocity was 6.24L g -1 h -1 After stabilization for about 20 hours, the samples were collected and analyzed every 4 hours. Usually, the data when the reaction time was 24 hours was taken. The reaction products were analyzed by gas chromatography. CO2, CO, N2 and CH4 were analyzed using GCMicro 490 equipped with TCD (alumina column, PPU column and MS5A column). Organic compounds including hydrocarbons and oxygen-containing compounds were analyzed using GC 2010 equipped with FID (PONA capillary column).

[0134] The testing conditions of Fe / γ-Al2O3 and catalyst (Fe-Co / NC) were the same.

[0135] The catalytic activities of the catalysts in Example 1 and Comparative Example 1 are as follows: Figure 8 As shown, it can be found that compared with the Fe / γ-Al2O3 catalyst, the Fe-Co / NC catalyst provided by the present invention has higher reaction activity and low-carbon olefin yield, which is related to the introduction of cobalt. In addition, the carbon-nitrogen layer formed by high-temperature pyrolysis of the carrier can effectively anchor and disperse metal nanoparticles, promote the reduction and carburization of the metal during the reaction, and thus facilitate higher olefin selectivity.

[0136] Test Example 2

[0137] The catalyst obtained in Example 16 was used in the reaction of preparing light olefins by hydrogenation of CO2, and the test conditions were the same as those in Test Example 1. The catalytic activities of the catalysts in Example 16 and Comparative Example 1 are shown in FIG. Fig. 9 As shown, it can be found that compared with the Fe / γ-Al2O3 catalyst, the cobalt-iron bimetallic Fe-Zn / NC catalyst provided by the present invention has higher reaction activity and low-carbon olefin yield.

[0138] Test Example 3

[0139] The catalysts prepared in Examples 2, 3, 4 and 5 were used in the CO2 hydrogenation reaction, and the test conditions were the same as those in Test Example 1. The catalytic activity results are shown in FIG. Fig.10 As shown, it can be found that with the increase of Co content and Na content in the catalyst, the catalytic activity for CO2 conversion rate shows a gradually increasing trend, but the selectivity of light olefins first increases and then decreases.

[0140] Test Example 4

[0141] The catalysts prepared in Examples 17, 18, and 19 were used in the CO2 hydrogenation reaction, and the test conditions were the same as those in Test Example 1. The catalytic activity results are shown in FIG. Fig.11 As shown, it can be found that with the increase of Zn content in the catalyst, the catalyst prepared in Example 18 has the highest CO2 conversion rate, and the yield of light olefins gradually increases.

[0142] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A catalyst comprising a carrier having a MOF framework-derived structure and an active ingredient Fe, wherein the content of the active ingredient is 1-40% by weight of the total mass of the catalyst and is calculated as Fe element; in the catalyst, Fe exists in the form of Fe3O4 and Fe5C2; The preparation method of the catalyst comprises the following steps: (1) mixing imidazole and / or an imidazole derivative, an M metal source, an Fe source, and an organic solvent to obtain a precursor precipitate; (2) calcining the precursor precipitation under an inert atmosphere or a reducing atmosphere; The M metal in the M metal source is selected from at least one of Co, Zn, Cu and Mn; The Fe source is an Fe complex prepared by complexing an Fe salt with an organic amine.

2. The catalyst according to claim 1, wherein The content of the active ingredient is 2-30%.

3. The catalyst according to claim 1 or 2, wherein The metal skeleton component in the carrier having the MOF skeleton-derived structure is at least one of Co, Zn, Cu and Mn.

4. The catalyst according to claim 1 or 2, wherein Based on the total mass of the catalyst, the content of the metal skeleton component is 10-40%.

5. The catalyst according to claim 4, wherein Based on the total mass of the catalyst, the content of the metal skeleton component is 15-35%.

6. The catalyst according to claim 1 or 2, wherein The catalyst further contains alkali metal, and the alkali metal content is 1-20% based on the total mass of the catalyst.

7. The catalyst according to claim 6, wherein The catalyst further contains alkali metal, and the alkali metal content is 2-10% based on the total mass of the catalyst.

8. The catalyst according to claim 6, wherein The alkali metal is selected from at least one of Li, Na, K and Rb.

9. The catalyst according to claim 8, wherein The alkali metal is Na and / or K.

10. The catalyst according to claim 1 or 2, wherein The average particle size of the carrier having a MOF framework-derived structure is 0.3-2 μm; and / or, the average particle size of the active ingredient is 5-100 nm; And / or, the specific surface area of ​​the catalyst is 20-300m 2 / g; And / or, the pore volume of the catalyst is 0.1-0.6 cm 3 / g.

11. A method for preparing a catalyst according to any one of claims 1 to 10, comprising the following steps: (1) mixing imidazole and / or an imidazole derivative, an M metal source, an Fe source, and an organic solvent to obtain a precursor precipitate; (2) calcining the precursor precipitation under an inert atmosphere or a reducing atmosphere; The M metal in the M metal source is selected from at least one of Co, Zn, Cu and Mn; The Fe source is an Fe complex prepared by complexing an Fe salt with an organic amine.

12. The method according to claim 11, wherein: The imidazole and / or imidazole derivative is at least one selected from 2-methylimidazole, 1-methylimidazole, 4-methylimidazole, 5-methylimidazole, 1-ethylimidazole and 2-ethylimidazole.

13. The method according to claim 11, wherein: The M metal source is selected from at least one of Co(NO3)2, CoCl3, Zn(NO3)2, ZnCl2, KMnO4, Na3MnO4, CuCl2 and Cu(NO3)2.

14. The method according to claim 11, wherein: The organic solvent is selected from methanol and / or ethanol.

15. The method according to claim 11, wherein: The Fe salt is selected from at least one of FeCl2, FeCl3, FeSO4, Fe2(SO4)3, Fe(NO3)3 and Fe(C5H7O2)3.

16. The method according to claim 11, wherein: The organic amine is ethylenediamine and / or N-[3-(trimethoxysilyl)propyl]ethylenediamine.

17. The method according to claim 11, wherein: The molar ratio of the Fe salt to the organic amine is 1:1-6.

18. The method according to any one of claims 11 to 17, wherein: The molar ratio of imidazole and / or imidazole derivative, M metal source, Fe source and organic solvent is (2-50):1:(0.01-4):(30-500).

19. The method according to claim 18, wherein: The molar ratio of imidazole and / or imidazole derivative, M metal source, Fe source and organic solvent is (5-40):1:(0.02-2):(50-300).

20. The method according to any one of claims 11 to 17, wherein: The method further comprises impregnating the precursor precipitate with an impregnation solution containing an alkali metal salt, and then performing the step (2).

21. The method according to claim 20, wherein: The alkali metal is selected from at least one of Li, Na, K and Rb.

22. The method according to claim 21, wherein: The alkali metal is Na and / or K.

23. The method according to claim 20, wherein: The alkali metal salt is used in an amount such that the alkali metal content in the prepared catalyst is 1-20% based on the total mass of the catalyst.

24. The method according to claim 23, wherein: The alkali metal salt is used in an amount such that the alkali metal content in the prepared catalyst is 2-10% based on the total mass of the catalyst.

25. The method according to any one of claims 11 to 17, wherein: The method further comprises washing and / or drying the precursor precipitate and then performing step (2).

26. The method according to any one of claims 11 to 17, wherein: In step (2), the inert atmosphere is provided by an inert gas, and the reducing atmosphere is provided by H2 and optionally an inert gas.

27. The method according to claim 26, wherein: In step (2), calcination is carried out in a mixed atmosphere of N2 and H2.

28. The method according to claim 27, wherein: The volume ratio of N2 to H2 is 1:(0.1-1).

29. The method according to claim 27, wherein: The calcination conditions include: a calcination temperature of 300-750° C. and a calcination time of 2-48 hours.

30. Use of the catalyst according to any one of claims 1 to 10 in the preparation of olefins by hydrogenation of CO2.