A device and method for alkali thermal debromination and blending regeneration of high-bromine PS plastic
Through the combined treatment of alkaline thermal debromination of high-brominated PS plastics and blended regeneration devices, efficient debromination and upgraded regeneration are achieved, solving the problems of lowering bromine concentration and physical properties in the prior art, improving the debromination efficiency and maintaining The physical properties of plastics.
Patent Information
- Application Number
- CN202310129752.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-17
AI Technical Summary
The prior art is difficult to effectively reduce the bromine element concentration in high bromine PS plastics in alkaline heat leaching methods, resulting in a decrease in the physical properties of the plastics, difficulty in reuse, and limited debromination efficiency.
The alkaline thermal debromination and blending regeneration device of high bromine PS plastic is adopted, and the alkaline thermal leaching pretreatment and modified granulation regeneration are carried out through the combined use of the debromination leaching mechanism, the modified granulation mechanism and the leaching liquid recovery mechanism. Achieve efficient debromination and upgraded regeneration.
Achieve 99.5% debromide efficiency of high bromine PS plastics, improve the debromide efficiency by 5 to 15%, maintain the physical properties of the plastics, solve the problem of reduced physical properties after alkaline thermal debromide, and realize high bromine PS waste High-efficiency debromination and upgrading of plastics.
Smart Images

Figure CN116140340B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste resource treatment, and relates to a device and method for alkali thermal debromination and co-blending regeneration of high-bromine PS plastic. Background Art
[0002] The recycling of waste plastics is an inevitable trend for achieving sustainable social development. With the reduction of fossil energy supply, waste plastics are gradually regarded as valuable resources. The function of waste plastic recycling enterprises has also changed from reducing pollution to future-oriented resource and energy export enterprises. However, waste plastics usually contain 5-20wt% of brominated flame retardants BFR, which seriously limits the recycling of bromine-containing waste plastics. For example, the high-bromine polystyrene (PS) waste plastics in the plastic back shell of discarded CRT TVs have a Br content of 5-20wt%. - Concentration> 150000ppm. Since BFR brominated flame retardants are difficult to degrade naturally in the environment and are bioaccumulative, causing endocrine disturbances, the EU restricted the use of polybrominated biphenyls (PBB) and polybrominated diphenyl ethers (PBDE) in electronic and electrical equipment in the RoHS 2.0 standard in 2011 (Br - In 2019, Canada also restricted the use and sale of decabromodiphenyl ethane (DBDPE), resulting in a large number of discarded high-bromine plastics that cannot be reused in high-value fields such as home appliances and IT communications, causing waste of resources and potential profit loss. Therefore, it is necessary to achieve efficient debromination and high-value recycling of high-bromine waste PS plastics through technological improvement and innovation.
[0003] The debromination methods of bromine-containing plastics mainly include mechanochemical method, pyrolysis liquefaction method and alkaline hot leaching method. In the mechanochemical method, mechanical stress drives the chemical reaction during the grinding process, and the C-Br bond is subjected to impact and shear force and then breaks. Chen Xi et al. (ACS Sustainable Chem. Eng. 2020, 8, 1, 172–178) accelerated electron transfer and bromide ion adsorption by adding nano zero-valent iron and metal oxides, but ball milling debromination can only remove bromine elements on the surface of particles, and it still needs to be practiced and applied in industrial production. The pyrolysis liquefaction method has a wide range of applicability. For example, patent ZL201610259354.7 uses fluidized bed cracking of bromine-containing plastics at 450°C to 550°C to obtain pyrolysis oil, but the integrity of the plastic matrix is lost. The alkali hot leaching method achieves selective debromination under high temperature and high pressure. For example, Patent ZL201510067170.6 uses ammonia water as a solution to carry out the debromination reaction of plastics at 300°C and 9.82MPa to obtain debrominated plastic solids. The alkali hot leaching method provides a good debromination effect while ensuring the integrity of the plastic matrix.
[0004] However, the debromination efficiency of the alkaline hot leaching method is limited, especially for high-bromine waste PS plastics (Br - The bromine concentration is greater than 150000ppm, and it is impossible to directly reduce the bromine concentration to less than 1000ppm through a one-step alkali hot leaching treatment. If the alkali hot leaching temperature and time are increased without limit, the integrity of the plastic matrix will be damaged, and the utilization value of the waste PS plastic will be reduced. Summary of the invention
[0005] In order to solve the deficiencies in the prior art, the purpose of the present invention is to propose a device and method for alkali thermal debromination and blending regeneration of high-bromine PS plastics, so as to solve the problem that the physical properties of plastics are reduced and difficult to reuse after alkali thermal debromination.
[0006] The present invention provides a debromination and regeneration method for high-bromine PS plastics, which performs two-stage debromination and bromine reduction treatment based on alkali hot leaching pretreatment combined with modified granulation regeneration, thereby achieving efficient debromination and upgraded reuse of high-bromine PS plastics.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] The present invention proposes an alkaline thermal debromination and blending regeneration device for high-bromine PS plastics, which comprises a debromination leaching mechanism, a modification granulation mechanism, and a leachate recovery mechanism;
[0009] Further,
[0010] The debromination leaching mechanism comprises a lower hopper and a debromination reactor, the lower hopper is connected to the debromination reactor through a pipeline, and the debromination reactor is also connected to the centrifugal dehydrator and the heat exchanger in the leachate recovery mechanism through pipelines; the lower hopper is used to add high-bromine PS plastic raw materials to the device, and the debromination reactor is used to provide high-temperature and high-pressure conditions required for the debromination leaching reaction, and perform alkaline heat enhanced leaching treatment on the bromine element in the high-bromine PS plastic flakes;
[0011] The modified granulation mechanism includes a cleaning dryer, a high-speed mixer, and a granulator. The cleaning dryer is connected to the centrifugal dehydrator and the high-speed mixer through pipelines, and the two ends of the high-speed mixer are connected to the cleaning dryer and the granulator through pipelines. The cleaning dryer is used to clean and dry the PS plastic matrix after debromination and centrifugal dehydration, and remove the alkali and moisture remaining on the surface of the PS plastic matrix due to the debromination reaction; the high-speed mixer is used to blend the bromine-free and / or low-bromine PS plastic and toughening agent added from the outside in different proportions to obtain a homogenized blended mixture; the granulator is used to granulate and regenerate the homogenized blended mixture to obtain regenerated PS particles;
[0012] The leachate recovery mechanism includes a centrifugal dehydrator, a heat exchanger, and a reverse osmosis concentration crystallizer. The debromination reactor discharge port is connected to the centrifugal dehydrator feed port, the centrifugal dehydrator water outlet is connected to the heat exchanger water inlet, the centrifugal dehydrator discharge port is connected to the cleaning dryer feed port, the heat exchanger water outlet is connected to the reverse osmosis concentration crystallizer water inlet, and the reverse osmosis concentration crystallizer water outlet is connected to the debromination reactor through the heat exchanger. The leachate recovery mechanism is used to recycle the heat and bromine element in the leaching reaction liquid generated in the debromination reactor.
[0013] Preferably, the debromination reactor is a pressure-resistant, closed, self-heating reactor, and the depressurized gas from the debromination reactor is discharged after being treated with activated carbon tail gas.
[0014] Preferably, the centrifugal dehydrator performs solid-liquid separation on the debrominated PS plastic matrix and the high-temperature bromine-containing leaching solution.
[0015] Preferably, the high-temperature bromine-containing leachate is cooled in a heat exchanger, and the heat energy is recovered for reheating the leachate.
[0016] Preferably, the reverse osmosis concentration crystallizer performs osmotic concentration and crystallization bromine extraction treatment on the bromine-containing leachate to obtain bromine-free leachate and crude bromine salt crystals, respectively.
[0017] Preferably, the bromine-free leachate can be reused, and the bromine-free leachate is heated in a heat exchanger and reused as the leachate for the debromination reaction.
[0018] Preferably, the number of the mechanisms is not limited to one, the debromination leaching mechanism, the modification granulation mechanism, and the leachate recovery mechanism are connected in series, the debromination leaching mechanism is connected to the debromination leaching mechanism in parallel, the modification granulation mechanism is connected to the modification granulation mechanism in parallel, and the leachate recovery mechanism is connected to the leachate recovery mechanism in parallel, so as to construct an intermittent continuous treatment system.
[0019] The present invention also proposes a method for alkali thermal debromination and co-blending regeneration of high-bromine PS plastic, which is applicable to the above-mentioned alkali thermal debromination and co-blending regeneration device of high-bromine PS plastic, and comprises the following steps:
[0020] S1: Add high-bromine PS plastic raw materials into the debromination leaching mechanism through the lower hopper, perform alkali heat enhanced leaching and primary debromination treatment in the debromination reactor, and obtain debrominated PS plastic matrix and high-temperature bromine-containing leaching liquid after centrifugal dehydration;
[0021] S2: The debrominated PS plastic matrix is blended with bromine-free and / or low-bromine PS plastic and toughening agent in a high-speed mixer in different proportions, and then extruded and granulated by a granulator to obtain secondary debrominated PS regenerated particles.
[0022] In step S1, the bromine content of the high-bromine PS plastic raw material is 150,000 to 500,000 ppm.
[0023] The debromination reaction conditions are: temperature 200-350°C, pH 9-14, pressure 0.4-1.2 MPa, and time 15-100 min; preferably, the temperature is 300°C, the pH is 12, the pressure is 0.8 MPa, and the time is 50 min.
[0024] Preferably, the addition ratio of the bromine-free and / or low-bromine PS plastic in step S2 is 30-98% (mass ratio), and the ratio is selected according to actual needs. The bromine concentration of the debrominated PS plastic matrix is further diluted and reduced during the blending and modified granulation process.
[0025] Preferably, the toughening agent in step S2 includes SBS, MBS, SEBS, POE, TPO, TPV, and one or more thereof can be selected according to actual use conditions; preferably, SBS and MBS, and only one or two can be used at the same time; the toughening agent is added in an amount of 1 to 15% (mass ratio), preferably 10%; by adding the toughening agent, the elongation at break and the impact resistance of the plastic can be improved, so that the PS plastic particles after granulation still have good physical properties.
[0026] The high-temperature bromine-containing leachate obtained after the centrifugal dehydrator is first cooled by a heat exchanger, and then enters a reverse osmosis concentration crystallizer for osmotic concentration and evaporation crystallization to obtain a bromine-free leachate and bromine salt crude crystals; the bromine-free leachate enters a heat exchanger to be heated and can be reused as a debromination reaction leachate.
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: the existing alkali hot leaching debromination method cannot well guarantee the original physical properties of the plastic while debrominating; while the present invention uses the two processes of alkali hot leaching pretreatment and modified granulation regeneration to carry out two-stage debromination and bromine reduction of high-bromine PS plastics, while reducing the concentration of bromine elements, the physical properties of PS plastics are kept stable, and the problem of reduced plastic properties and difficulty in reuse after alkali hot debromination is solved, and efficient debromination and upgrading of high-bromine PS waste plastics is achieved. The present invention can achieve a debromination efficiency of 99.5%, which is 5-15% higher than the existing alkali hot leaching debromination method, and can also achieve a good debromination effect of high-bromine waste PS plastics. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic structural diagram of the alkali thermal debromination and blending regeneration device for high-bromine PS plastics of the present invention.
[0029] Figure 2The present invention is a schematic flow chart of the alkali thermal debromination and blending regeneration method of high-bromine PS plastic.
[0030] Figure 1 Middle: 1- lower hopper, 2- debromination reactor, 3- centrifugal dehydrator, 4- cleaning dryer, 5- high-speed mixer, 6- granulator, 7- heat exchanger, 8- reverse osmosis concentration crystallizer. DETAILED DESCRIPTION
[0031] The invention is further described in detail with reference to the following specific embodiments and drawings. The process, conditions, experimental methods, etc. for implementing the present invention, except for the contents specifically mentioned below, are all common knowledge and common common sense in the art and are not particularly limited by the present invention.
[0032] The present invention discloses an alkali thermal debromination and co-blending regeneration device for high-bromine PS plastic, comprising a debromination leaching mechanism, a modified granulation mechanism, and a leachate recovery mechanism; the debromination leaching mechanism comprises a lower hopper and a debromination reactor; the modified granulation mechanism comprises a cleaning dryer, a high mixer, and a granulator; the leachate recovery mechanism comprises a centrifugal dehydrator, a heat exchanger, and a reverse osmosis concentration crystallizer. The present invention also discloses a method for alkali thermal debromination and co-blending regeneration of high-bromine PS plastic using the above device, wherein the high-bromine PS plastic is firstly subjected to primary alkali thermal debromination, and then co-blended and granulated with bromine-free and / or low-bromine PS and a toughening agent in different proportions to obtain secondary bromine-reduced PS recycled plastic. The present invention performs two-stage debromination and bromine reduction treatment on high-bromine PS plastic based on alkali thermal leaching pretreatment combined with modified granulation regeneration, solves the problem of reduced plastic properties and difficulty in reuse after alkali thermal debromination, and realizes the upgraded reuse of high-bromine PS waste plastic.
[0033] Example 1
[0034] After experimental verification, the following specific parameter conditions are all more suitable and can achieve the effects claimed in this technical solution. Those skilled in the art can choose from the following constraints as needed during specific implementation: The bromine content in high-bromine PS plastic is 150,000-500,000 ppm. The alkaline thermal debromination reaction conditions are: temperature 200-350°C, pH 9-14, pressure 0.4-1.2 MPa, time 15-100 min. The addition ratio of bromine-free or low-bromine PS plastic is 30-98%, and the addition ratio of toughening agent SBS and MBS is 1-15%.
[0035] High bromine-containing PS plastic with a bromine concentration of 169000ppm was selected as the research object. After crushing, it was sent to the debromination reactor 2 for alkaline heat enhanced leaching and primary debromination treatment. The reaction conditions of the debromination reactor 2 were set as temperature 300℃, time 1h, solid-liquid ratio 1:10, and pH value 13. After the reaction was completed, the solid-liquid mixture in the debromination reactor 2 was separated into solid and liquid by a centrifugal dehydrator 3 to obtain the debrominated PS plastic matrix and high-temperature bromine-containing leaching solution. According to ion chromatography analysis, the bromine concentration in the high bromine-containing PS plastic was reduced from 169000ppm to 9340ppm, and the bromine removal rate was 94.47%. After the reaction was completed, the depressurized gas of the debromination reactor 2 was discharged after activated carbon tail gas treatment.
[0036] After debromination, the PS plastic matrix is further hot-dried and dehydrated in a cleaning and drying machine 4, and then blended with 90% bromine-free PS plastic and 3% toughening agent in a high mixer 5. The bromine concentration is further diluted and reduced during the blending modification granulation process, and then extruded and granulated by a single screw granulator 6 to obtain PS regenerated particles after secondary bromine reduction. As shown in Table 1, the bromine concentration of the PS regenerated particles is further reduced to 863ppm, reaching the limit value (<1000ppm) in the RoHS 2.0 standard. At the same time, by comparing the physical properties of PS with 3% toughening agent added and without toughening agent added, the impact strength and elongation at break of the regenerated PS particles after adding 3% toughening agent are significantly improved. Compared with qualified ordinary PS, the physical properties of the recycled PS plastic are close to those of qualified PS, and have good application prospects. Based on this, debrominated regenerated PS particles with excellent physical properties and stability are finally obtained, realizing the upgrading and reuse of high-bromine PS plastics.
[0037] After the high-temperature bromine-containing leachate is cooled by the heat exchanger 7, it enters the reverse osmosis concentration crystallizer 8 for osmotic concentration and crystallization bromine extraction. After the bromine-containing leachate is osmotic concentrated, a bromine-free leachate and a bromine-containing concentrated solution are obtained. Furthermore, the bromine-free leachate can be reused, and after entering the heat exchanger 7 and being reheated, it is returned to the debromination reactor 2 to achieve the reuse of heat energy and water resources. At the same time, the bromine-containing concentrated solution is evaporated and crystallized to obtain crude bromine salt crystals, which can be used as chemical raw materials.
[0038] Table 1. Physical properties of different plastic particles (test methods are based on Chinese national standards)
[0039]
[0040] Example 2
[0041] This technical solution is also applicable to bromine-containing PS waste plastics with a bromine content of less than 150,000 ppm. Bromine-containing PS plastics with a bromine concentration of 49,300 ppm were selected as the research object, and after crushing, they were sent to the debromination reactor 2 for alkaline heat enhanced leaching and primary debromination treatment. The reaction conditions of the debromination reactor 2 were set to a temperature of 300°C, a time of 0.5h, a solid-liquid ratio of 1:10, and a pH value of 12.5. After the reaction was completed, the solid-liquid mixture in the debromination reactor 2 was separated into solid and liquid by a centrifugal dehydrator 3 to obtain a debrominated PS plastic matrix and a bromine-containing leachate. According to ion chromatograph analysis, the bromine concentration in the bromine-containing PS plastic was reduced from 49,300 ppm to 7,200 ppm, and the bromine removal rate was 85.40%. After the reaction was completed, the depressurized gas of the debromination reactor 2 was discharged after being treated with activated carbon tail gas.
[0042] After debromination, the PS plastic matrix is further hot-dried and dehydrated in a cleaning and drying machine 4, and then blended with 90% bromine-free PS plastic and 3% toughening agent in a high mixer 5. The bromine concentration is further diluted and reduced during the blending modification granulation process, and then extruded and granulated by a single screw granulator 6 to obtain PS regenerated particles after secondary bromine reduction. As shown in Table 2, the bromine concentration of the PS regenerated particles is further reduced to 613ppm, reaching the limit value (<1000ppm) in the RoHS 2.0 standard. At the same time, by comparing the physical properties of PS with 3% toughening agent added and without toughening agent added, the impact strength and elongation at break of the regenerated PS particles after adding 3% toughening agent are significantly improved. Compared with qualified ordinary PS, the physical properties of the recycled PS plastic are close to those of qualified PS, and have good application prospects. Based on this, debrominated regenerated PS particles with excellent physical properties and stability are finally obtained, realizing the upgrading and reuse of bromine-containing PS plastics.
[0043] After the high-temperature bromine-containing leachate is cooled by the heat exchanger 7, it enters the reverse osmosis concentration crystallizer 8 for osmotic concentration and crystallization bromine extraction. After the bromine-containing leachate is osmotic concentrated, a bromine-free leachate and a bromine-containing concentrated solution are obtained. Furthermore, the bromine-free leachate can be reused, and after entering the heat exchanger 7 and being reheated, it is returned to the debromination reactor 2 to achieve the reuse of heat energy and water resources. At the same time, the bromine-containing concentrated solution is evaporated and crystallized to obtain crude bromine salt crystals, which can be used as chemical raw materials.
[0044] Table 2. Physical properties of different plastic particles (test methods based on Chinese national standards)
[0045]
[0046] Example 3
[0047] Bromine-containing PS plastic with a bromine concentration of 251300ppm was selected as the research object. After crushing, it was sent to the debromination reactor 2 for alkaline heat enhanced leaching and primary debromination treatment. The reaction conditions of the debromination reactor 2 were set as temperature 300℃, time 1h, solid-liquid ratio 1:10, and pH value 12. After the reaction was completed, the solid-liquid mixture in the debromination reactor 2 was separated into solid and liquid by a centrifugal dehydrator 3 to obtain the debrominated PS plastic matrix and bromine-containing leaching solution. According to ion chromatography analysis, the bromine concentration in the bromine-containing PS plastic was reduced from 251300ppm to 16300ppm, and the bromine removal rate was 93.52%. After the reaction was completed, the depressurized gas of the debromination reactor 2 was discharged after activated carbon tail gas treatment.
[0048] After debromination, the PS plastic matrix is further hot-dried and dehydrated in a cleaning and drying machine 4, and then blended with 90% bromine-free PS plastic and 5% toughening agent in a high mixer 5. The bromine concentration is further diluted and reduced during the blending modification granulation process, and then extruded and granulated by a single screw granulator 6 to obtain PS regenerated particles after secondary bromine reduction. As shown in Table 2, the bromine concentration of the PS regenerated particles is further reduced to 945ppm, reaching the limit value (<1000ppm) in the RoHS 2.0 standard. At the same time, by comparing the physical properties of PS with 5% toughening agent added and without toughening agent added, the impact strength and elongation at break of the regenerated PS particles after adding 5% toughening agent are significantly improved. Compared with qualified ordinary PS, the physical properties of the recycled PS plastic are close to those of qualified PS, and have good application prospects. Based on this, debrominated regenerated PS particles with excellent physical properties and stability are finally obtained, realizing the upgrading and reuse of bromine-containing PS plastics.
[0049] After the high-temperature bromine-containing leachate is cooled by the heat exchanger 7, it enters the reverse osmosis concentration crystallizer 8 for osmotic concentration and crystallization bromine extraction. After the bromine-containing leachate is osmotic concentrated, a bromine-free leachate and a bromine-containing concentrated solution are obtained. Furthermore, the bromine-free leachate can be reused, and after entering the heat exchanger 7 and being reheated, it is returned to the debromination reactor 2 to achieve the reuse of heat energy and water resources. At the same time, the bromine-containing concentrated solution is evaporated and crystallized to obtain crude bromine salt crystals, which can be used as chemical raw materials.
[0050] Table 2. Physical properties of different plastic particles (test methods based on Chinese national standards)
[0051]
[0052]
[0053] The protection content of the present invention is not limited to the above embodiments. Without departing from the spirit and scope of the inventive concept, changes and advantages that can be thought of by those skilled in the art are included in the present invention and are protected by the attached claims.
Claims
1. A device for alkali thermal debromination and blending regeneration of high-bromine PS plastics, characterized in that: It includes debromination leaching mechanism, modification granulation mechanism and leachate recovery mechanism; The debromination leaching mechanism includes a lower hopper and a debromination reactor; the modified granulation mechanism includes a cleaning dryer, a high-speed mixer, and a granulator; the leachate recovery mechanism includes a centrifugal dehydrator, a heat exchanger, and a reverse osmosis concentration crystallizer; The debromination leaching mechanism, the modification granulation mechanism, and the leachate recovery mechanism are connected in parallel and / or in series through pipelines; the number of the debromination leaching mechanism, the modification granulation mechanism, and the leachate recovery mechanism is one or more; In the modified granulation mechanism, the cleaning and drying machine is connected to the centrifugal dehydrator and the high-speed mixer through pipelines, and the two ends of the high-speed mixer are connected to the cleaning and drying machine and the granulator through pipelines; the cleaning and drying machine is used to clean and dry the PS plastic matrix after debromination and centrifugal dehydration, and remove the alkali and moisture remaining on the surface of the PS plastic matrix due to the debromination reaction; the high-speed mixer is used to blend the bromine-free and / or low-bromine PS plastic and toughening agent added from the outside in different proportions to obtain a homogenized blended mixture; the granulator is used to granulate and regenerate the homogenized blended mixture to obtain regenerated PS particles.
2. The device according to claim 1, characterized in that In the debromination leaching mechanism, the lower hopper is connected to the debromination reactor through a pipeline, and the debromination reactor is also connected to the centrifugal dehydrator and the heat exchanger in the leachate recovery mechanism through pipelines; the lower hopper is used to add high-bromine PS plastic raw materials into the device, and the debromination reactor is used to provide high-temperature and high-pressure conditions required for the debromination leaching reaction, and perform alkaline heat enhanced leaching treatment on the bromine element in the high-bromine PS plastic raw materials.
3. The device according to claim 1, characterized in that In the leachate recovery mechanism, the feed port of the centrifugal dehydrator is connected to the discharge port of the debromination reactor, the water outlet of the centrifugal dehydrator is connected to the water inlet of the heat exchanger, the discharge port of the centrifugal dehydrator is connected to the feed port of the cleaning and drying machine, the water outlet of the heat exchanger is connected to the water inlet of the reverse osmosis concentration crystallizer, and the water outlet of the reverse osmosis concentration crystallizer is connected to the debromination reactor through the heat exchanger; the leachate recovery mechanism is used to recycle the heat and bromine element in the leachate.
4. The device according to claim 1, characterized in that The debromination reactor is a pressure-resistant, closed, self-heating reactor, and the depressurized gas from the debromination reactor is discharged after being treated with activated carbon tail gas; The centrifugal dehydrator performs solid-liquid separation on the debrominated PS plastic matrix and the high-temperature bromine-containing leaching solution; The heat exchanger is used to perform heat exchange with the bromine-containing leaching solution, so as to cool the high-temperature bromine-containing leaching solution and use the recovered heat to reheat the bromine-free leaching solution that can be reused; The reverse osmosis concentration crystallizer performs osmotic concentration and crystallization bromine extraction treatment on the bromine-containing leachate to obtain bromine-free leachate and bromine salt crude crystals respectively.
5. A method for alkali thermal debromination and co-regeneration of high-bromine PS plastic, applicable to the alkali thermal debromination and co-regeneration device for high-bromine PS plastic as described in any one of claims 1 to 4, characterized in that: The steps include: S1: Add high-bromine PS plastic raw materials into the debromination leaching mechanism through the lower hopper, perform alkali heat enhanced leaching and primary debromination treatment in the debromination reactor, and obtain debrominated PS plastic matrix and high-temperature bromine-containing leaching liquid after centrifugal dehydration; S2: The debrominated PS plastic matrix is blended with bromine-free and / or low-bromine PS plastic and toughening agent in a high-speed mixer in different proportions, and then extruded and granulated by a granulator to obtain secondary debrominated PS regenerated particles.
6. The method according to claim 5, characterized in that In step S1, the content of bromine element in the high-bromine PS plastic raw material is 150,000-500,000 ppm; the debromination reactor is a pressure-resistant, closed, self-heating reactor, and the debromination reaction conditions are: temperature 200-350° C., pH 9-14, pressure 0.4-1.2 MPa, and time 15-100 min.
7. The method according to claim 5, characterized in that In step S2, the mass ratio of the bromine-free and / or low-bromine PS plastic added is 30-98%.
8. The method according to claim 5, characterized in that In step S2, the toughening agent is selected from one or more of SBS, MBS, SEBS, POE, TPO, and TPV, and is added in a mass ratio of 1 to 15% to maintain the physical properties of the recycled PS plastic.
9. The method according to claim 5, characterized in that The high-temperature bromine-containing leachate obtained after the centrifugal dehydrator is first cooled by a heat exchanger, and then enters a reverse osmosis concentration crystallizer for osmotic concentration and evaporation crystallization to obtain a bromine-free leachate and bromine salt crude crystals; the bromine-free leachate enters a heat exchanger to be heated and can be reused as a debromination reaction leachate.
Citation Information
Patent Citations
Method for harmlessly debrominating bromine-containing plastic waste
CN104722555A
Device and method for preparing pyrolytic oil by pyrolyzing and catalytically debrominating brominated flame-retarded waste plastics
CN105713641A
Waste circuit board smelting soot reinforced alkaline leaching debromination recovery method
CN110724823A
Method for synchronously removing antimony and bromine from electronic waste flame-retardant plastic and recovering plastic matrix
CN113321848A
Full-automatic static rotary closed pyrolysis waste circuit board treatment system and process