A method and application of preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon
The CoO/Co loaded lotus biomass carbon material is prepared by jointly reducing Co3O4 with hydrogen and carbon, which solves the problems of high weight characteristics and high preparation cost of absorbing materials, and achieves simple and low-cost preparation of absorbing materials and improvement of dielectric properties.
Patent Information
- Application Number
- CN202310163774.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-24
AI Technical Summary
Existing absorbing materials have problems with insufficient weight characteristics and high preparation costs in improving reflection loss and dielectric properties, especially the weight characteristics of pure CoO materials and the high preparation costs of graphene composite materials.
The CoO/Co-loaded lotus pod biomass carbon material is prepared by jointly reducing Co3O4 with hydrogen and carbon. A simple liquid-phase chemistry method is used to prepare porous materials in an eco-friendly biomass pyrolysis. Co3O4 particles are evenly attached to the lotus pod biomass carbon, and The wave absorption effect is enhanced by adjusting the dielectric properties of ferromagnetic materials.
The preparation of easy-to-operate and low-cost cobalt oxide-loaded lotus biomass carbon materials has been achieved, which enhances the wave absorption effect, adjusts the dielectric properties, and reduces production costs.
Smart Images

Figure CN116143183B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of wave absorbing materials, and in particular relates to a method for preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon and its application. Background Art
[0002] With the development of communication technology and modern science and technology, constructing absorbing materials with light weight, strong absorption, thin thickness and wide frequency characteristics is of great significance to weaken the impact of electromagnetic radiation.
[0003] In the past few years, transition metals and their compounds have been widely studied for use in absorbing materials, especially CoO containing metal Co, which can effectively improve reflection loss by increasing interface polarization. However, due to the lack of dielectric materials that are beneficial to dielectric loss and the weight characteristics of pure CoO, it needs further improvement.
[0004] Studies have shown that adding carbon-based materials to transition metals and their oxides is an effective way to enhance dielectric properties. A currently reported method for preparing a nano-cobalt oxide / graphene composite absorbing coating uses graphene to achieve better absorbing effects, but it has a high preparation cost. Summary of the invention
[0005] In order to overcome the above technical problems, the purpose of the present invention is to provide a method and application of preparing CoO / Co-carrying lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon, and reducing cobalt tetraoxide to cobalt oxide and cobalt by carbon and hydrogen to obtain cobalt oxide / cobalt-carrying lotus biomass carbon material. The method has the characteristics of simple process and low cost.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A CoO / Co-carried lotus pod biomass carbon material is prepared by reducing Co3O4 with hydrogen and carbon. The material is in irregular block shape, and a layer of small particles is wrapped around the outer layer of the block particles. Characterization shows that the irregular block is C and the small particles are Co3O4. The CoO / Co-carried lotus pod biomass carbon material is obtained by reducing Co3O4 under hydrogen.
[0008] A method for preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon, comprising the following steps:
[0009] (1) Pre-carbonizing the lotus pod (LP) in a tube furnace, then washing with HCl, filtering and drying; stirring the dried LP with KOH and a small amount of water, vacuum drying, activating the LP in a tube furnace, washing with hydrochloric acid, filtering and drying, and obtaining lotus pod biomass carbon;
[0010] (2) dissolving the lotus biomass carbon in step (1) in deionized water, adding Co(NO3)2, stirring magnetically, adding ammonia water, stirring, and obtaining a LP / Co3O4 solution;
[0011] (3) placing the LP / Co3O4 solution obtained in step (2) into a drying oven, keeping warm, washing with deionized water, and drying to obtain LP / Co3O4;
[0012] (4) The material obtained in step 3 is placed in hydrogen at a certain pressure to reduce Co3O4 through the reduction effect of hydrogen and carbon.
[0013] In the step (1), the mass ratio of LP to KOH is 1:3.
[0014] In the step (1), pre-carbonization is performed at 500° C. for 2 h in a tubular furnace, and the dried LP and KOH are stirred with a small amount of water and vacuum dried, and then activated at 800° C. for 1-3 h in a tubular furnace.
[0015] In the step (2), the mass ratio of lotus pod biomass carbon to Co(NO3)2 is about 1:29; the mass ratio of lotus pod biomass carbon to deionized water is 1:500; and the volume ratio of deionized water to ammonia water is 5:4.
[0016] In the step (2), stirring is performed for 100 min.
[0017] In the step (3), the mixture is kept in a drying oven at 180° C. for 8-12 hours and washed with deionized water for 3-4 times.
[0018] In the step (4), the hydrogen pressure ranges from 2 to 8 MPa.
[0019] The LP / CoO / Co material generated after reduction in step (4) is used as an absorbing material.
[0020] Beneficial effects of the present invention.
[0021] The outstanding substantial feature of the present invention is that carbon materials are obtained from the pyrolysis of eco-friendly biomass, and a cobalt oxide-carrying lotus biomass carbon material is successfully prepared by a simple liquid phase chemical method, so that Co3O4 particles are uniformly attached to the lotus biomass carbon, and the lotus biomass carbon is a porous material, and the dielectric properties of the ferromagnetic material can be adjusted to enhance the wave absorption effect. Co3O4 can be reduced to CoO and Co by carbon and hydrogen under certain conditions. The method is simple to operate, the conditions are easy to control, and the production cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Scanning electron microscope images of the LP / Co3O4 material prepared in the present invention and after reduction in Examples 1, 2, and 3.
[0023] Figure 2 XRD patterns of the LP / Co3O4 material prepared in the present invention and the LP / Co3O4 materials prepared in Examples 1, 2 and 3 after reduction. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The method for preparing LP / Co3O4 is characterized in that it is reduced to cobalt oxide and cobalt using carbon and hydrogen at a certain temperature and pressure.
[0026] The specific steps are as follows:
[0027] (1) 1-3 g of lotus pods were pre-carbonized in a tube furnace at 500 °C for 2 h, cooled, washed with HCl, filtered and dried.
[0028] (2) Add 3-5 g KOH to 1-3 g of dried LP and a small amount of water, stir and vacuum dry for 2-3 days.
[0029] (3) 4 to 6 g of the material obtained in step (2) was activated in a tube furnace at 800° C. for 1 to 3 h, washed with hydrochloric acid, filtered and dried to obtain lotus biomass carbon.
[0030] (4) Weigh 20-50 mg of lotus biomass carbon, add 1-1.5 g of Co(NO3)2 to 20 ml of deionized water, stir with magnetic force, add 15-20 ml of ammonia water, stir for 100-150 min. Keep in a drying oven at 150-200 °C for 10 h. After taking out, wash with deionized water 3-5 times and dry.
[0031] (5) Place 1-2 g LP / Co3O4 into the hydrogen storage platform and keep it warm at 200-500°C and 2-8 MPa for 2 h.
[0032] In the following embodiments:
[0033] Example 1
[0034] The specific steps for synthesizing LP / Co3O4 / CoO materials are as follows:
[0035] (1) 1-3 g of lotus pods were pre-carbonized in a tube furnace at 500°C for 2 h, cooled, washed with HCl, filtered and dried.
[0036] (2) Add 3-5 g KOH to 1-3 g of dried LP and a small amount of water, stir and vacuum dry for 2-3 days.
[0037] (3) 4 to 6 g of the material obtained in step (2) was activated in a tube furnace at 800° C. for 1 to 3 h, washed with hydrochloric acid, filtered and dried to obtain lotus biomass carbon.
[0038] (4) Weigh 20-50 mg of lotus biomass carbon, add 1-1.5 g of Co(NO3)2 to 20 ml of deionized water, stir with magnetic force, add 15-20 ml of ammonia water, stir for 100-150 min. Keep in a drying oven at 150-200 °C for 10 h. After taking out, wash with deionized water 3-5 times and dry.
[0039] (5) Place 1-2 g LP / Co3O4 into the hydrogen storage platform and keep it warm at 200°C and 2-5 MPa for 2 h.
[0040] The LP / Co3O4 prepared in Example 1 was kept at 200°C and 2-5MPaH2 for 2h, and then analyzed using an X-ray diffractometer. The results showed that diffraction peaks of C, Co3O4 and CoO appeared. By comparing with helium conditions at the same temperature and pressure, it was shown that Co3O4 reduced CoO under the action of H2, and C had no reducing effect on Co3O4 at lower temperatures.
[0041] Example 2
[0042] The specific steps for synthesizing LP / CoO materials are as follows:
[0043] (1) 1-3 g of lotus pods were pre-carbonized in a tube furnace at 500°C for 2 h, cooled, washed with HCl, filtered and dried.
[0044] (2) Add 3-5 g KOH to 1-3 g of dried LP and a small amount of water, stir and vacuum dry for 2-3 days.
[0045] (3) 4 to 6 g of the material obtained in step (2) was activated in a tube furnace at 800° C. for 1 to 3 h, washed with hydrochloric acid, filtered and dried to obtain lotus biomass carbon.
[0046] (4) Weigh 20-50 mg of lotus biomass carbon, add 1-1.5 g of Co(NO3)2 to 20 ml of deionized water, stir with magnetic force, add 15-20 ml of ammonia water, stir for 100-150 min. Keep in a drying oven at 150-200 °C for 10 h. After taking out, wash with deionized water 3-5 times and dry.
[0047] (5) Place 1-2 g LP / Co3O4 into the hydrogen storage platform and keep it at 300°C and 2-5 MPa for 2 h.
[0048] The LP / Co3O4 prepared in Example 2 was placed under conditions of 300°C and 2-5 MPa, and then analyzed using an X-ray diffractometer. The results showed that diffraction peaks of C and CoO appeared, indicating that Co3O4 was completely reduced to CoO.
[0049] Example 3
[0050] The specific steps for synthesizing LP / CoO / Co materials are as follows:
[0051] (1) 1-3 g of lotus pods were pre-carbonized in a tube furnace at 500 °C for 2 h, cooled, washed with HCl, filtered and dried.
[0052] (2) Add 3-5 g KOH to 1-3 g of dried LP and a small amount of water, stir and vacuum dry for 2-3 days.
[0053] (3) 4 to 6 g of the material obtained in step (2) was activated in a tube furnace at 800° C. for 1 to 3 h, washed with hydrochloric acid, filtered and dried to obtain lotus biomass carbon.
[0054] (4) Weigh 20-50 mg of lotus biomass carbon, add 1-1.5 g of Co(NO3)2 to 20 ml of deionized water, stir with magnetic force, add 15-20 ml of ammonia water, stir for 100-150 min. Keep in a drying oven at 150-200 °C for 10 h. After taking out, wash with deionized water 3-5 times and dry.
[0055] (5) Place 1-2 g LP / Co3O4 into the hydrogen storage platform and keep it warm at 400°C and 2-5 MPa for 2 h.
[0056] The LP / Co3O4 prepared in Example 3 was placed under conditions of 400°C and 2-5 MPa, and then analyzed using an X-ray diffractometer. The results showed that diffraction peaks of C, CoO and Co appeared, indicating that part of CoO was reduced to Co elemental substance.
[0057] The test results of implementation cases 1-3 show that as the temperature increases, the particle size of the surface particles of the LP / CoO / Co material prepared by the method of the present invention decreases accordingly, and is reduced to different substances by C and H2 at different temperatures. When the temperature is low, H2 mainly plays a reducing role to reduce Co3O4 to CoO, and at high temperatures, C and H2 play a reducing role together.
[0058] In summary, the above are only embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0059] like Figure 1 As shown. Figure 1 It can be seen that as the temperature increases, the particle size of the particles carried on the surface of lotus biomass carbon continues to decrease.
[0060] like Figure 2 As shown. Figure 2 It can be seen that with the increase of temperature, Co3O4 is gradually reduced and is reduced to CoO and Co by hydrogen and carbon at 400℃.
Claims
1. A method for preparing CoO / Co-carried lotus biomass carbon absorbing material by reducing Co3O4 with hydrogen and carbon, characterized in that: The following steps are involved: (1) The lotus pod LP is placed in a tube furnace for pre-carbonization, and then washed with HCl, filtered and dried; the dried LP is stirred with KOH and a small amount of water, vacuum dried, activated in a tube furnace, washed with hydrochloric acid, filtered and dried, and the lotus pod biomass carbon is obtained; (2) dissolving the lotus biomass carbon in step (1) in deionized water, adding Co(NO3)2, stirring magnetically, adding ammonia water, stirring, and obtaining a LP / Co3O4 solution; (3) placing the LP / Co3O4 solution obtained in step (2) into a drying oven, keeping warm, washing with deionized water, and drying to obtain LP / Co3O4; (4) placing the material obtained in step (3) in hydrogen at a certain pressure to reduce Co3O4 by the reduction action of hydrogen and carbon; In the step (4), LP / Co3O4 is placed in a hydrogen storage platform and kept at 200°C, 300°C or 400°C and 2-5 MPa for 2 hours.
2. The method for preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon according to claim 1, characterized in that: In the step (1), the mass ratio of LP to KOH is 1:
3.
3. The method for preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon according to claim 1, characterized in that: In the step (1), pre-carbonization is performed at 500° C. for 2 h in a tubular furnace, and the dried LP is stirred with KOH and a small amount of water, dried under vacuum, and then activated at 800° C. for 1-3 h in a tubular furnace.
4. The method for preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon according to claim 1, characterized in that: In the step (2), the mass ratio of the lotus pod biomass carbon to Co(NO3)2 is 1:29; the mass ratio of the lotus pod biomass carbon to deionized water is 1:500; and the volume ratio of deionized water to ammonia water is 5:
4.
5. The method for preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon according to claim 1, characterized in that: The stirring time in step (2) is 100 min.
6. The method for preparing CoO / Co-carried lotus biomass carbon material by reducing Co3O4 with hydrogen and carbon according to claim 1, characterized in that: In the step (3), the mixture is kept in a drying oven at 180° C. for 8-12 hours and washed with deionized water for 3-4 times.