A smelting method for producing flaw detection steel without RH process
By optimizing the converter and LF furnace processes in flaw detection steel production, limiting S content, using low N scrap steel, controlling the steel output temperature and time, using argon blowing and pure aluminum deoxygenation, combined with metal manganese fine-tuning alloy and calcium treatment, the solution is solved The problem of high RH process cost achieves low cost, low N and low H smelting, simplifying the process flow and reducing the cost of steelmaking.
Patent Information
- Application Number
- CN202310324041.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-03-30
AI Technical Summary
The RH process required in the production of flaw detection steel leads to an increase of 30-40 yuan/ton, resulting in a decrease in economic benefits, and it is difficult for the existing technology to effectively eliminate the vacuum treatment smelting process.
By optimizing process parameters in converters and LF furnaces, limiting the S content of the furnace, using low N scrap steel, controlling the steel outlet temperature and time, using argon blowing and pure aluminum deoxygenation, combining metal manganese fine-tuning alloy and calcium treatment, avoiding the increase Nitrogen and hydrogen increase to achieve low N and low H smelting, reduce inclusion content, and continuously casting using a double slow cooling system.
It realizes the production of low-N and low-H flaw detection steel at low cost, simplifies the process flow, improves operability, reduces the cost of steelmaking, and ensures the quality of the steel.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steelmaking, in particular to a smelting method for producing flaw detection steel without RH process. Background Art
[0002] Ultrasonic flaw detection is an effective method for inspecting the internal quality of steel. If the size of inclusions, internal crack size, and the content of harmful gas elements N and H in steel exceed the standard, the flaw detection results will show that they are unqualified. Generally, steels with high internal quality requirements, such as container steel and bridge steel, will require qualified flaw detection in the delivery technical conditions. For steels delivered by flaw detection, in order to ensure the internal quality, after the primary refining in the converter, the "LF+RH" composite refining process is generally required. The LF furnace has a good function of removing inclusions, while the RH vacuum furnace has a good ability to remove harmful gases such as N and H, and can further reduce the inclusion content. The "LF+RH" secondary refining is a conventional smelting process for flaw detection steel, but the cost of secondary refining is high. The production cost of molten steel after RH furnace treatment increases by 30-40 yuan / t. Therefore, there is basically no description with strong operability on how to cancel the vacuum treatment for smelting flaw detection steel. How to solve the problem of producing flaw detection steel by the "converter-LF-continuous casting" process requires new technology support. Summary of the invention
[0003] The purpose of the present invention is to provide a smelting method for producing flaw detection steel without the RH process, in order to solve the problem that the current flaw detection steel production needs to go through the RH process, but the cost of the flaw detection steel processed by the RH process increases by 30-40 yuan per ton, resulting in excessively high production cost of the flaw detection steel and reduced economic benefits.
[0004] A smelting method for producing flaw detection steel by using a RH-free process of the present invention comprises the following steps:
[0005] (1) Converter smelting
[0006] A. Limit the sulfur content entering the converter: Use low-sulfur hot metal, and put the hot metal into the furnace after slagging. The amount of slag in the hot metal entering the furnace should be ≤0.5‰, the sulfur content of the hot metal entering the converter should be ≤0.005%, and the sulfur content of the converter end point should be ≤0.007%;
[0007] B. Use low-N scrap steel in converter: Use low-N recycled scrap steel, requiring scrap steel N≤50ppm, and use steelmaking scrap billets, cut steel scrap and steel bar packing blocks that are not industrially used and are free of oil and dirt. Industrial packing blocks are not allowed;
[0008] C. Requirements for converter low-phosphorus smelting and endpoint control: tapping temperature 1580-1610℃, tapping time ≥4min10s; tapping oxygen ≤450ppm, tapping P ≤0.010%;
[0009] D. The bottom blowing gas of the converter is argon during the whole blowing process. The bottom blowing argon flow rate is 3000-3600L / min in the early stage of the blowing process and 4800-5400L / min in the late stage of the blowing process. After the oxygen lance stops supplying oxygen at the end of smelting, the bottom blowing and post-stirring are ≥2min when the tilting angle of the converter is at zero position. The bottom blowing argon flow rate of the converter during the post-stirring process is 4800L / min.
[0010] E. Requirements for converter deoxidation alloying and alloy baking: alloy baking time ≥ 9min, alloy baking temperature ≥ 400℃, alloying with metallic manganese, Mn after argon controlled at the limit value -0.10%, ferrosilicon quantitatively added 100Kg / furnace;
[0011] (2) LF furnace refining
[0012] A.LF uses pure aluminum for deoxidation: pure aluminum is added at one time, the amount of pure aluminum is 2.3-2.5Kg / t, the refining adopts high basicity and large slag operation, the slag basicity is ≥8.0, the amount of lime is added at 10-15Kg / t, and the slag layer thickness is 40-80mm;
[0013] B.LF fine-tuning alloy control: Use clean metal manganese to fine-tune Mn, high manganese or manganese alloys are not allowed, and avoid alloy nitrogen addition;
[0014] C. Refining time control: The refining process and power supply end time are controlled within 40-45 minutes;
[0015] D. LF calcium treatment: wire feeding rate is 3-3.5m / t. After wire feeding, cover agent is added immediately and soft blowing is performed. The soft blowing time is required to be ≥25min.
[0016] (3) Continuous casting
[0017] The superheat degree of the continuous casting process is controlled at 20-30℃, the pulling speed is constant, and the "ingot + steel plate" double slow cooling system is adopted, with the ingot slow cooling time ≥48h + the steel plate slow cooling time ≥24h.
[0018] In the present invention, the converter Mn alloying and LF fine-tuning alloying both use metal Mn with a Mn content of ≥97%.
[0019] The smelting equipment requirements of the present invention are as follows: the converter smoke hood and the LF water-cooled furnace cover are not allowed to leak, the deoxidizer and slag-making agent of the refined material must be dry, and the baking temperature is ≥100°C.
[0020] The use requirements of the ladle and the middle ladle in the present invention are as follows: in order to avoid the residual water in the new ladle and the new middle ladle entering the molten steel to cause H increase, the used ladle must be used, and the use of the new ladle is not allowed; in order to avoid H increase of the new middle ladle, avoid the production of flaw detection steel in the first furnace of continuous casting, and put the flaw detection steel in the second furnace of continuous casting and thereafter for production, and produce non-flaw detection steel in the first furnace of continuous casting.
[0021] The present invention is limited to the production of flaw detection steel plates with a rolling thickness of ≤80 mm. For flaw detection steel plates with a thickness greater than 80 mm, the RH process cannot be exempted.
[0022] The process principle of the method of the present invention is as follows:
[0023] (1) Converter smelting process
[0024] A. The purpose of limiting the S content entering the converter is to reduce the converter terminal S (i.e., the LF furnace initial S) by limiting the S entering the converter and reducing the molten iron slag, so that the LF furnace can achieve no desulfurization or less desulfurization, thereby reducing the desulfurization amount of the LF furnace. The LF furnace desulfurization requires strong stirring. The strong stirring process is prone to nitrogen absorption by the molten steel due to the large exposed surface of the molten steel.
[0025] B. Use low-N scrap steel in converter: The types of scrap steel used are scrap billets, cut steel and steel bar blocks produced within the steel mill. Industrial blocks are not allowed. Industrial blocks have complex sources and contain large amounts of oil and non-steel substances such as sludge, which are particularly prone to increase in N.
[0026] C. Requirements for converter low-phosphorus smelting and endpoint control: tapping temperature 1580-1610℃, tapping time ≥4min10s; tapping oxygen ≤450ppm, tapping P ≤0.010%. Standard melting composition P of steel grade ≤0.020%, low P smelting is achieved by tightening the P control range; because the higher the endpoint temperature, the easier it is to cause nitrogen increase, under the premise of meeting the converter deoxidation and alloying requirements, the endpoint temperature is 1580-1610℃.
[0027] D. Argon is used as the bottom blowing gas during the entire blowing process of the converter: Argon is used as the bottom blowing gas throughout the blowing process, the argon supply intensity is increased during the blowing process, and high-intensity argon blowing is continued after the oxygen supply is stopped at the end point to reduce the increase in nitrogen during the smelting process. Strong stirring after the end point can reduce carbon and oxygen accumulation, thereby further reducing the oxygen content of the steel.
[0028] F. The purpose of converter deoxidation alloying and alloy baking requirements is to use metallic manganese with low impurity elements (Mn content ≥ 97%) to reduce the nitrogen increase caused by alloying elements; the purpose of ferrosilicon quantitative addition (i.e. reduced addition) is to avoid nitrogen increase caused by strong deoxidation during the steelmaking process.
[0029] (2) LF refining process
[0030] A.LF uses pure aluminum for deoxidation: aluminum is added once after the LF furnace enters the station, because the inclusions after aluminum deoxidation are in flocculent form and are not easy to float up. Adding it once after entering the station can ensure that there is sufficient time after adding aluminum to promote the floating of inclusions after aluminum deoxidation. The basicity of the slag; the higher the basicity of the slag, the more conducive it is to the adsorption of inclusions, and the high basicity can reduce the oxidation of the slag, promote diffusion deoxidation in the refining process, and the slag layer has a suitable thickness to prevent the exposed molten steel from absorbing nitrogen.
[0031] B.LF fine-tuning alloy control: Use relatively clean metal manganese to fine-tune Mn, high manganese or manganese alloys are not allowed, and avoid alloy nitrogen addition.
[0032] C. LF calcium treatment: Calcium treatment can spheroidize inclusions and MnS, and avoid the formation of cracks in the rolling process due to the strip-shaped inclusions, which will cause non-conformity in NDT. The main purpose of adding covering agent immediately after calcium treatment is to keep the slag in a molten state, which is more conducive to further adsorption of inclusions during the soft blowing process. Because the slag layer is thick, it is easy to form a crust as the ambient temperature decreases when the power supply and argon blowing process are stopped. After the slag hardens, it does not have the function of adsorbing inclusions.
[0033] (3) Continuous casting process
[0034] The superheat during continuous casting is controlled at 20-30℃, and the pulling speed is constant. In order to release the internal stress and H of the billet and steel plate, the "bill + steel plate" double slow cooling system is adopted, and the slow cooling time of the billet + steel plate is ≥48h and 24h respectively. The general design idea adopts a low superheat of 12-25℃ to control segregation, but the viscosity of low superheated molten steel is high, and inclusions are not easy to float, which is not conducive to the metallurgical function of the tundish. From the perspective of controlling segregation and tundish metallurgy, the superheat is controlled at 20-30℃.
[0035] After the RH furnace treatment, the molten steel can generally achieve the harmful gas element N content ≤ 35ppm, H content ≤ 2ppm, electrolytic inclusions in the steel ≤ 50ppm, and metallographic inclusions A\B\C\D in the steel ≤ 1.5 respectively. The present invention studies the RH function, and the RH mainly completes the degassing of the molten steel, that is, reducing the content of N and H elements, and further removing inclusions. By optimizing the smelting raw materials, converters and LF smelting tasks, the tasks of removing harmful elements such as N and H and reducing the content of inclusions can be decomposed, thereby achieving the purpose of producing flaw detection steel without RH process in the present invention and reducing the steelmaking production cost.
[0036] The beneficial effects of the method of the present invention are as follows:
[0037] (1) The present invention realizes low N and low H smelting without RH process, which directly reduces the cost of steelmaking process;
[0038] (2) The process flow of the present invention is simple and clear, highly operable and easy to control. DETAILED DESCRIPTION
[0039] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely exemplary of the technical solution of the present invention and do not limit the present invention in any form. Any changes or equivalent substitutions that do not deviate from the concept of the present invention are included in the protection scope of the present invention.
[0040] Example 1
[0041] This embodiment takes the production of Q345R steel as an example to explain the present invention; the finished steel plate requires P≤0.020%; S≤0.005%; the planned rolling thickness specification is 30mm, and the smelting process is as follows:
[0042] A smelting method for producing flaw detection steel by a RH-free process in this embodiment includes the following steps:
[0043] (1) Converter smelting
[0044] A. Limit the sulfur content entering the converter: Use low-sulfur hot metal, put the hot metal into the furnace after slagging, the amount of slag in the hot metal entering the furnace is 0.5‰, the sulfur content of the hot metal entering the converter is 0.005%, the final sulfur content of the converter is 0.007% (that is, the initial sulfur content of the LF furnace), and the corresponding desulfurization amount of the LF furnace is ≥0.002%. The desulfurization amount is relatively low, and the LF furnace does not need strong stirring to force desulfurization;
[0045] B. Use low-N scrap steel in converter: The scrap steel types include scrap billets, cut steel and steel bar blocks produced within the steel mill. Industrial blocks are not allowed.
[0046] C. Requirements for converter low-phosphorus smelting and endpoint control: tapping temperature 1580℃, tapping time 4min10s; tapping oxygen 450ppm, tapping P 0.010%;
[0047] D. The bottom blowing gas of the converter is argon during the whole blowing process. The bottom blowing argon flow rate is 3000L / min in the early stage of the blowing process and 4800L / min in the late stage of the blowing process. After the oxygen lance stops supplying oxygen at the end of smelting, the bottom blowing and post-stirring are performed for 2.5 minutes (post-stirring is required when the furnace tilting angle is at zero position). The bottom blowing argon flow rate of the converter during the post-stirring process is 4800L / min.
[0048] E. Requirements for converter deoxidation alloying and alloy baking: The alloy must be baked (baking time 9.5min, baking temperature 480℃), and alloying is completed with metal manganese. The Mn after argon is controlled at a limit of about -0.10%, and ferrosilicon is quantitatively added at 100Kg / furnace;
[0049] (2) LF refining
[0050] A.LF uses pure aluminum for deoxidation, pure aluminum is added at one time, the amount of pure aluminum is 2.3Kg / t, and refining adopts high basicity and large slag operation; the slag basicity is 8.0, the amount of lime is added at 10Kg / t, and the slag layer thickness is 60mm;
[0051] B.LF fine-tuning alloy control, using relatively clean metal manganese to fine-tune Mn, high manganese and other manganese alloys are not allowed to avoid alloy nitrogen addition;
[0052] C. LF calcium treatment: wire feeding rate is 3m / t. After wire feeding, cover agent is added immediately and soft blowing is performed. The soft blowing time is 25min.
[0053] (3) Continuous casting
[0054] The continuous casting process adopts high superheat pouring, the superheat is controlled at 20℃, and the pulling speed is constant. In order to facilitate the release of internal stress and H of the ingot and steel plate, the "ingot + steel plate" double slow cooling system is adopted, and the ingot slow cooling time is 48h + the steel plate slow cooling time is 24h.
[0055] In this embodiment, the converter hood and LF water-cooled furnace cover of the smelting equipment are in good condition, and there is no water leakage in the equipment. The refined material is deoxidized and slag is dried.
[0056] In this embodiment, the ladle and the middle ladle are used as follows: the ladle is a red ladle that has been used in circulation, and the first continuous casting furnace (i.e., the first casting furnace is a non-destructive steel grade) avoids the production of flaw detection steel in the first casting furnace. The smelting furnace number is the third continuous casting furnace.
[0057] The rolling thickness specification limit in this embodiment is 30 mm.
[0058] After the ingots were obtained by the smelting method of the present invention, 15 Q345R flaw detection steel plates with a thickness of 30 mm were rolled in this embodiment. After flaw detection: a total of 15 plates were rolled, and all the flaw detection tests were qualified.
[0059] Example 2
[0060] This embodiment takes the production of Q345qD steel as an example to explain the present invention; the finished steel plate requires P≤0.018%; S≤0.004%; the planned rolling thickness specification is 50mm, and the smelting process is as follows:
[0061] A smelting method for producing flaw detection steel by a RH-free process in this embodiment includes the following steps:
[0062] (1) Converter smelting
[0063] A. Limit the sulfur content entering the converter: Use low-sulfur hot metal, put the hot metal into the furnace after slagging, the amount of slag in the hot metal entering the furnace is 0.4‰, the sulfur content of the hot metal entering the converter is 0.005%, the final sulfur content of the converter is 0.006% (that is, the initial sulfur content of the LF furnace), and the corresponding desulfurization amount of the LF furnace is ≥0.002%. The desulfurization amount is relatively low, and the LF furnace does not need strong stirring to force desulfurization;
[0064] B. Use low-N scrap steel in converter: The scrap steel types include scrap billets, cut steel and steel bar blocks produced within the steel mill. Industrial blocks are not allowed.
[0065] C. Requirements for converter low-phosphorus smelting and endpoint control: tapping temperature 1590℃, tapping time 4min30s; tapping oxygen 430ppm, tapping P 0.009%;
[0066] D. The bottom blowing gas of the converter is argon during the whole blowing process. The bottom blowing argon flow rate is 3300L / min in the early stage of the blowing process and 5000L / min in the late stage of the blowing process. After the oxygen lance stops supplying oxygen at the end of smelting, the bottom blowing and post-stirring are performed for 2.5min (post-stirring is required when the furnace tilting angle is at zero position). The bottom blowing argon flow rate of the converter during the post-stirring process is 4800L / min.
[0067] E. Requirements for converter deoxidation alloying and alloy baking: The alloy must be baked (baking time 9.6min, baking temperature 500℃), and alloying is completed with metal manganese. The Mn after argon is controlled at a limit of about -0.10%, and ferrosilicon is quantitatively added at 100Kg / furnace;
[0068] (2) LF refining
[0069] A.LF uses pure aluminum for deoxidation, pure aluminum is added at one time, the amount of pure aluminum is 2.4Kg / t, and refining adopts high basicity and large slag operation; the slag basicity is 9.0, the amount of lime is added at 12Kg / t, and the slag layer thickness is 60mm;
[0070] B.LF fine-tuning alloy control, using relatively clean metal manganese to fine-tune Mn, high manganese and other manganese alloys are not allowed to avoid alloy nitrogen addition;
[0071] C. LF calcium treatment: wire feeding rate is 3.4m / t. After wire feeding, cover agent is added immediately and soft blowing is performed. The soft blowing time is 30min.
[0072] (3) Continuous casting
[0073] The continuous casting process adopts high superheat pouring, the superheat is controlled at 27℃, and the pulling speed is constant. In order to facilitate the release of internal stress and H of the ingot and steel plate, the "ingot + steel plate" double slow cooling system is adopted, and the ingot slow cooling time is 50h + the steel plate slow cooling time is 26h.
[0074] In this embodiment, the converter hood and LF water-cooled furnace cover of the smelting equipment are in good condition, and there is no water leakage in the equipment. The refined material is deoxidized and slag is dried.
[0075] In this embodiment, the ladle and the middle ladle are used as follows: the ladle is a red ladle that has been used in circulation, and the first continuous casting furnace (i.e., the first casting furnace is a non-destructive steel grade) avoids the production of flaw detection steel in the first casting furnace. The smelting furnace number is the fourth continuous casting furnace.
[0076] In this embodiment, the rolling thickness specification is limited to 50 mm.
[0077] After the ingots were obtained by the smelting method of the present invention, 12 Q345qD flaw detection steel plates with a thickness of 50 mm were rolled in this embodiment. After flaw detection: a total of 12 pieces were rolled, and all the flaw detection tests were qualified.
[0078] Example 3
[0079] This embodiment takes the production of Q370R steel as an example to explain the present invention; the finished steel plate requires P≤0.016%; S≤0.003%; the planned rolling thickness specification is 80mm, and the smelting process is as follows:
[0080] A smelting method for producing flaw detection steel by a RH-free process in this embodiment includes the following steps:
[0081] (1) Converter smelting
[0082] A. Limit the sulfur content entering the converter: Use low-sulfur hot metal, and put it into the furnace after slagging. The amount of slag in the hot metal entering the furnace is 0.35‰. The sulfur content of hot metal entering the converter is 0.003%, and the final sulfur content of the converter is 0.004% (that is, the initial sulfur content of the LF furnace). The corresponding desulfurization amount of the LF furnace is ≥0.001%. The desulfurization amount is relatively low, and the LF furnace does not need strong stirring to force desulfurization;
[0083] B. Use low-N scrap steel in converter: The scrap steel types include scrap billets, cut steel and steel bar blocks produced within the steel mill. Industrial blocks are not allowed.
[0084] C. Requirements for converter low-phosphorus smelting and endpoint control: tapping temperature 1610℃, tapping time 4min40s; tapping oxygen 400ppm, tapping P 0.008%;
[0085] D. The bottom blowing gas of the converter is argon during the whole blowing process. The bottom blowing argon flow rate is 3600L / min in the early stage of the blowing process and 5400L / min in the late stage of the blowing process. After the oxygen lance stops supplying oxygen at the end of smelting, the bottom blowing and post-stirring are performed for 2.8min (post-stirring is required when the furnace tilting angle is at zero position). The bottom blowing argon flow rate of the converter during the post-stirring process is 4800L / min.
[0086] E. Requirements for converter deoxidation alloying and alloy baking: The alloy must be baked (baking time 9.8min, baking temperature 520℃), and alloying is completed with metal manganese. The Mn after argon is controlled at a limit of about -0.10%, and ferrosilicon is quantitatively added at 100Kg / furnace;
[0087] (2) LF refining
[0088] A.LF uses pure aluminum for deoxidation, pure aluminum is added at one time, the amount of pure aluminum is 2.5Kg / t, and refining adopts high basicity and large slag operation; the slag basicity is 9.5, the amount of lime is added at 15Kg / t, and the slag layer thickness is 80mm;
[0089] B.LF fine-tuning alloy control, using relatively clean metal manganese to fine-tune Mn, high manganese and other manganese alloys are not allowed to avoid alloy nitrogen addition;
[0090] C. LF calcium treatment: wire feeding rate is 3.5m / t. After wire feeding, cover agent is added immediately and soft blowing is performed. The soft blowing time is 35min.
[0091] (3) Continuous casting
[0092] The continuous casting process adopts high superheat pouring, the superheat is controlled at 30℃, and the pulling speed is constant. In order to facilitate the release of internal stress and H of the ingot and steel plate, the "ingot + steel plate" double slow cooling system is adopted, and the ingot slow cooling time is 55h + the steel plate slow cooling time is 28h.
[0093] In this embodiment, the converter hood and LF water-cooled furnace cover of the smelting equipment are in good condition, and there is no water leakage in the equipment. The refined material is deoxidized and slag is dried.
[0094] In this embodiment, the ladle and the middle ladle are used as follows: the ladle is a red ladle that has been used in circulation, and the first continuous casting furnace (i.e., the first casting furnace is a non-destructive steel grade) avoids the production of flaw detection steel in the first casting furnace. The smelting furnace number is the fourth continuous casting furnace.
[0095] The rolling thickness specification limit in this embodiment is 80 mm.
[0096] After the ingots were obtained by the smelting method of the present invention, 10 Q370R flaw detection steel plates with a thickness of 80 mm were rolled in this embodiment. After flaw detection: a total of 10 plates were rolled, and all the flaw detection tests were qualified.
Claims
1. A smelting method for producing flaw detection steel without RH process, characterized in that The steps include: (1) Converter smelting A. Limit the sulfur content entering the converter: Use low-sulfur hot metal, and put the hot metal into the furnace after slagging. The amount of slag in the hot metal entering the furnace should be ≤0.5‰, the sulfur content of the hot metal entering the converter should be ≤0.005%, and the sulfur content of the converter end point should be ≤0.007%; B. Use low-N scrap steel in converter: Use low-N recycled scrap steel, requiring scrap steel N≤50ppm, and use steelmaking scrap billets, cut steel scrap and steel bar packing blocks that are not industrially used and are free of oil and dirt. Industrial packing blocks are not allowed; C. Requirements for converter low-phosphorus smelting and endpoint control: tapping temperature 1580-1610℃, tapping time ≥4min10s; tapping oxygen ≤450ppm, tapping P ≤0.010%; D. The bottom blowing gas of the converter is argon during the whole blowing process. The bottom blowing argon flow rate is 3000-3600L / min in the early stage of the blowing process and 4800-5400L / min in the late stage of the blowing process. After the oxygen lance stops supplying oxygen at the end of smelting, the bottom blowing and post-stirring are ≥2min when the tilting angle of the converter is at zero position. The bottom blowing argon flow rate of the converter during the post-stirring process is 4800L / min. E. Requirements for converter deoxidation alloying and alloy baking: alloy baking time ≥ 9min, alloy baking temperature ≥ 400℃, alloying with metallic manganese, Mn after argon controlled at the limit value -0.10%, ferrosilicon quantitatively added 100Kg / furnace; (2) LF furnace refining A.LF uses pure aluminum for deoxidation: pure aluminum is added at one time, the amount of pure aluminum is 2.3-2.5Kg / t, the refining adopts high basicity and large slag operation, the slag basicity is ≥8.0, the amount of lime is added at 10-15Kg / t, and the slag layer thickness is 40-80mm; B.LF fine-tuning alloy control: Use clean metal manganese to fine-tune Mn, high manganese or manganese alloys are not allowed, and avoid alloy nitrogen addition; C. Refining time control: The refining process and power supply end time are controlled within 40-45 minutes; D. LF calcium treatment: wire feeding rate is 3-3.5m / t. After wire feeding, cover agent is added immediately and soft blowing is performed. The soft blowing time of argon is required to be ≥25min. (3) Continuous casting The superheat degree of the continuous casting process is controlled at 20-30℃, the pulling speed is constant, and the "ingot + steel plate" double slow cooling system is adopted, and the ingot slow cooling time is ≥48h + the steel plate slow cooling time is ≥24h; the metal manganese alloying in the converter and the LF fine-tuning alloy are both made of metal manganese with a Mn content of ≥97%; in the above steps, the smelting equipment requirements are: the converter smoke hood and the LF water-cooled furnace cover are not allowed to leak, the deoxidizer and slag-making agent of the refined material must be dry, and the baking temperature is ≥100℃; the use requirements of the ladle and the middle ladle: in order to avoid the residual water in the new ladle and the new middle ladle entering the molten steel to cause H increase, the used ladle must be used, and the new ladle is not allowed to be used; in order to avoid H increase in the new middle ladle, avoid the production of flaw detection steel in the first furnace of the opening, and put the flaw detection steel in the second furnace of the continuous casting and later production, and the first furnace of the continuous casting produces non-flaw detection steel; the rolling thickness of the flaw detection steel is ≤80mm.