A stranded wire welding wire capable of inhibiting solidification cracks of high-strength aluminum alloy and a preparation method thereof

By using a variety of solid core welding wires and powder alloying technologies, the grains are refined and the ratio of zirconium welding wire is controlled, and combined with the use of borax layer, the problem of solidification cracks in high-strength aluminum alloy welding is solved, and the weld strength and welding performance are improved. Reduces production costs and is suitable for a variety of welding methods.

CN116160150BInactive Publication Date: 2024-11-19HUAZHONG UNIV OF SCI & TECH

Patent Information

Application Number
CN202211105367.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

High-strength aluminum alloys are prone to solidification cracks during welding. The existing welding wires are costly, complicated in the process of preparation, and difficult to meet performance requirements. The existing welding wires are not strong enough to suppress cracks.

Method used

A variety of solid core welding wires are used as raw materials, and the grains are refined by adding powder alloying, and the ratio of zirconium welding wires is controlled to suppress solidification cracks. The combination of borax layer and powder is used to improve weld molding and arc stability.

Benefits of technology

Effectively suppress solidification cracks during high-strength aluminum alloy welding, improve weld strength and welding performance, reduce production costs, and is suitable for high-speed wire feeding and various welding methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116160150B_ABST
    Figure CN116160150B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field related to welding materials, and discloses a stranded welding wire capable of suppressing solidification cracks of high-strength aluminum alloys and a preparation method thereof. The stranded welding wire comprises a central wire, a peripheral wire and flux, wherein the central wire is formed by twisting a plurality of solid welding wires; the peripheral wire is arranged at the periphery of the central wire, and comprises a plurality of solid welding wires, wherein the peripheral wires are twisted together around the central wire to form a welding wire body of the stranded welding wire, and the flux is extruded and filled in the gaps between the solid welding wires constituting the welding wire body; the plurality of solid welding wires constituting the central wire include zirconium welding wire and aluminum alloy welding wire. The present invention improves the strength of the weld and overcomes the problem of joint softening by refining the grains. In addition, the degree of grain refinement is controlled by the proportion of zirconium welding wire in the central wire, and is easy to adjust.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field related to welding materials, and more specifically, relates to a stranded wire welding wire capable of suppressing solidification cracks of high-strength aluminum alloys and a preparation method thereof. Background Art

[0002] Aluminum alloys have the advantages of low density, high specific strength and strong plastic deformation ability, and are widely used in automobile manufacturing, rail transportation, aerospace and other fields. Among various aluminum alloys, high-strength aluminum alloys (such as 2 series and 7 series) have the advantages of higher specific strength, specific stiffness, better stress corrosion resistance, higher fracture toughness and excellent processing performance. They are widely used in aerospace, weapons and equipment, transportation and other fields, especially in the aerospace field. It occupies a very important position and is one of the most important structural materials in this field. However, although this high-strength aluminum alloy has a high specific strength, its welding performance is poor. Solidification cracks are very likely to occur during fusion welding, which seriously damages its mechanical properties and limits its industrial application.

[0003] Among the existing welding wires for inhibiting solidification cracks in aluminum alloy welding, Al-Si welding wire is widely used in actual production processes because of its good casting performance and easy wire making process. It is easy to form a large amount of low-melting eutectic during welding, and its "healing effect" is used to reduce the tendency of solidification cracks. However, its strength is not high and it is difficult to meet the production needs in fields with high performance requirements. Therefore, the development of new flux-cored welding wires and improved solid welding wires are two important directions for inhibiting solidification cracks in the welding process of high-strength aluminum alloys. Patent 201911420553.1 discloses an aluminum alloy welding wire containing TiB2 particles for solving the problem of welding cracking of 7 series aluminum alloys. However, in the preparation process of the welding material, TiB2 is combined with the aluminum matrix in the form of added particles. The wettability of the enhanced particles and the matrix is ​​not good during welding, which easily leads to a decrease in the bonding strength of the interface and limits its production and use. At the same time, the welding wire is extruded from the ingot after casting, and vacuum degassing is required during the casting process. The manufacturing cost is high and the process is complicated, which is not conducive to its promotion and use. Summary of the invention

[0004] In view of the above defects or improvement needs of the prior art, the present invention provides a stranded wire welding wire capable of suppressing solidification cracks of high-strength aluminum alloy and a preparation method thereof, which selects a variety of solid welding wires as raw materials, adds powder for alloying, suppresses solidification cracks in the welding process of high-strength aluminum alloy, improves weld strength by refining grains, and overcomes the problem of joint softening. In addition, the degree of grain refinement is controlled by the proportion of zirconium welding wire in the center wire, which is easy to adjust.

[0005] To achieve the above object, according to one aspect of the present invention, there is provided a stranded wire welding wire capable of suppressing solidification cracks of a high-strength aluminum alloy, the stranded wire welding wire comprising a central wire, a peripheral wire and a flux, the central wire being formed by twisting a plurality of solid wires; the peripheral wire being arranged at the periphery of the central wire, comprising a plurality of solid wires, the peripheral wires being twisted together around the central wire to form a wire body of the stranded wire welding wire, the flux being extruded and filled in gaps between the solid wires constituting the wire body;

[0006] The multiple solid welding wires constituting the central wire include zirconium welding wire and aluminum alloy welding wire.

[0007] Furthermore, the central wire is formed by twisting three solid welding wires, and the peripheral wires include six solid welding wires; the powder includes an alloying agent, an activating agent and a combustion aid.

[0008] Furthermore, the alloying agent includes the following components in mass fractions: 1.2 to 4.9 parts of metal Cu powder, 1.2 to 2.9 parts of metal Mg, 0.07 to 0.6 parts of metal Mn powder and 0.05 to 0.4 parts of metal Cr powder; the activating agent includes the following components in mass fractions: 3 to 12 parts of titanium dioxide, 5 to 12 parts of chromium oxide, 0 to 12 parts of sodium fluoride, 0 to 11 parts of lithium fluoride, 0 to 8 parts of potassium fluorozirconate, 0.1 to 1.0 parts of sodium stearate and 0.1 to 1.0 parts of cerium oxide; the combustion aid includes the following components in mass fractions: 0 to 4 parts of potassium chlorate, 0 to 2 parts of magnesium oxide and 0.1 to 1 parts of rare earth scandium zirconium alloy powder, wherein the mass ratio of rare earth scandium to zirconium is 3:1.

[0009] Furthermore, the diameter of the central wire is 1.015 to 1.030 times the diameter of the solid welding wire constituting the peripheral wire.

[0010] Furthermore, the alloying agent comprises the following components in parts by mass: 1.2 to 4.2 parts of Cu powder, 1.2 to 2.5 parts of Mg powder, 0.3 to 0.5 parts of Mn powder, and 0.2 to 0.4 parts of Cr powder; the activating agent comprises the following components in parts by mass: 5 to 10 parts of titanium dioxide, 5 to 10 parts of chromium oxide, 5 to 8 parts of sodium fluoride, 4 to 10 parts of lithium fluoride, 2 to 8 parts of potassium fluorozirconate, 0.1 to 0.8 parts of sodium stearate, and 0.1 to 0.6 parts of cerium oxide; the combustion aid comprises the following components in parts by mass: 2 to 3 parts of potassium chlorate, 1 to 2 parts of magnesium oxide, and 0.1 to 1 part of rare earth scandium zirconium alloy powder.

[0011] Furthermore, a borax layer is formed on the central wire and the peripheral wires, and the powder adheres to the gaps between the solid welding wires through the borax layer.

[0012] Furthermore, the thickness of the borax layer is 0.25-0.50 μm.

[0013] Further, the central wire includes one zirconium welding wire and two aluminum alloy welding wires, and the peripheral wires include six aluminum alloy welding wires; or,

[0014] The central wire includes two zirconium welding wires and one aluminum alloy welding wire, and the peripheral wires include six aluminum alloy welding wires; or,

[0015] The central wire includes three strands of zirconium welding wire, and the peripheral wire includes six strands of SAl2319 aluminum alloy welding wire.

[0016] According to another aspect of the present invention, a method for preparing a stranded welding wire capable of suppressing solidification cracks in a high-strength aluminum alloy is provided. The method is used to prepare the stranded welding wire capable of suppressing solidification cracks in a high-strength aluminum alloy as described above.

[0017] Furthermore, after a borax layer is formed on the surface of the central wire and the peripheral wire through expansion treatment, the powder is squeezed into the gap between the welding wires at a temperature of 150° C. to 200° C.

[0018] In general, compared with the prior art, the above technical solutions conceived by the present invention mainly have the following beneficial effects:

[0019] 1. The solid welding wire constituting the center wire includes a zirconium welding wire. By controlling the proportion of the zirconium welding wire in the center wire, the zirconium content in the weld deposited metal is changed, thereby controlling the degree of grain refinement, and ultimately inhibiting solidification cracks during high-strength aluminum alloy welding. In addition, the gap between the center wire and the gap between the center wire and the peripheral wire are filled with powder, which plays a role in improving weld formation, stabilizing the arc, increasing penetration, and reducing spatter.

[0020] 2. Zr reacts with the substrate to form Al3Zr. The metallurgical chemical reaction is [Zr] + 3Al → Al3Zr. The generated Al3Zr phase can serve as a nucleation core to promote the formation of fine equiaxed crystals of α-Al. The fine equiaxed grains are easier to coordinate the deformation between the grains, thereby inhibiting solidification cracks. The fine Al3Zr phase With Al matrix They have similar crystal structures and therefore have good crystal coherence. At the same time, since the Al3Zr phase is generated by in-situ reaction rather than being added into the matrix, the interface between the two phases is clean and pollution-free. In addition, Al3Zr particles can pin dislocations, prevent dislocation movement, and improve joint strength.

[0021] 3. Compared with solid core welding wire, the stranded wire welding wire for suppressing solidification cracks of high-strength aluminum alloy has flexible composition adjustment, simple production process and low cost; at the same time, compared with flux-cored welding wire, the stranded wire welding wire has good wire feeding performance and is suitable for high-speed wire feeding and high-current welding.

[0022] 4. The stranded wire welding wire that inhibits solidification cracks in high-strength aluminum alloys selects a variety of solid welding wires as raw materials and adds powder alloying. On the basis of inhibiting solidification cracks in the welding process of high-strength aluminum alloys, it improves the weld strength by refining the grains and overcomes the softening problem of the joints.

[0023] 5. Add activator to the stranded wire welding wire to inhibit solidification cracks of high-strength aluminum alloy, improve weld formation, increase penetration, reduce welding spatter, significantly improve arc stability, and be suitable for all-position welding during gas shielded welding.

[0024] 6. The stranded wire welding wire for suppressing solidification cracks of high-strength aluminum alloy can be made into a diameter of 1.6 mm for gas shielded welding or laser arc hybrid welding, and can also be made into a diameter of 3.6 mm for high current welding, further improving production efficiency.

[0025] 7. The stranded wire welding wire for suppressing solidification cracks of high-strength aluminum alloy of the present invention has a simple production process, small equipment investment and low production cost, thus overcoming the problems of large production investment, high production cost and high price of flux-cored welding wire.

[0026] 8. The stranded wire welding wire for suppressing solidification cracks of high-strength aluminum alloys of the present invention can be of any length and can also be wound into a coil. It is suitable for continuous automatic welding. In addition to being used for gas shielded welding, it can also be used for various welding methods such as laser wire filling welding and laser arc hybrid welding. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic cross-sectional view of a stranded wire welding wire capable of suppressing solidification cracks of a high-strength aluminum alloy provided by the present invention, wherein 1 is a center wire, 2 is a peripheral wire, and 3 is powder;

[0028] Figure 2 It is a metallographic structure diagram of the weld metal under the action of the stranded wire welding wire capable of suppressing solidification cracks of high-strength aluminum alloy provided by the present invention;

[0029] Figure 3 (a), (b), and (c) are SEM images of Al3Zr phase, Al, and Zr generated by stranded wire, respectively. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0031] See also Figure 1 , Figure 2 and Figure 3 The present invention provides a stranded welding wire capable of suppressing solidification cracks of high-strength aluminum alloys. The stranded welding wire comprises a central wire 1, a peripheral wire 2 and a flux 3. The central wire 1 is formed by twisting a plurality of solid welding wires; the peripheral wire 2 is arranged at the periphery of the central wire 1 and comprises a plurality of solid welding wires. The peripheral wire 2 is twisted around the central wire 1 to form a welding wire body of the stranded welding wire. The flux 3 is extruded and filled in the gaps between the solid welding wires constituting the welding wire body. The plurality of solid welding wires constituting the central wire 1 include a zirconium welding wire and an aluminum alloy welding wire.

[0032] In this embodiment, the central wire 1 is formed by twisting three solid welding wires, and the peripheral wire 2 includes six solid welding wires; the powder includes an alloying agent, an activating agent and a combustion aid, wherein the alloying agent includes the following components in mass fractions: 1.2 to 4.9 parts of metal Cu powder, 1.2 to 2.9 parts of metal Mg, 0.07 to 0.6 parts of metal Mn powder and 0.05 to 0.4 parts of metal Cr powder. The activating agent includes the following components in mass fractions: 3 to 12 parts of titanium dioxide, 5 to 12 parts of chromium oxide, 0 to 12 parts of sodium fluoride, 0 to 11 parts of lithium fluoride, 0 to 8 parts of potassium fluorozirconate, 0.1 to 1.0 parts of sodium stearate and 0.1 to 1.0 parts of cerium oxide. The combustion aid includes the following components in mass fractions: The combustion aid includes the following components in mass fractions: 2 to 3 parts of potassium chlorate, 1 to 2 parts of magnesium oxide and 0.1 to 1 parts of rare earth scandium zirconium alloy powder.

[0033] The cross-section of the stranded welding wire is circular, with a diameter of 1.6 mm to 3.6 mm; the center of the circular cross-section is the cross-section of the central wire 1, and the cross-sections of the peripheral wires 2 are distributed around it. The diameter of the central wire 1 is 1.015 to 1.030 times the diameter of the peripheral wire 2, and the gaps between the cross-sections of the central wire 1 and the peripheral wire 2 are filled with powder.

[0034] The center wire 1 is formed by twisting three solid welding wires, and the three solid welding wires are composed of zirconium welding wire and aluminum alloy welding wire. By controlling the proportion of zirconium welding wire in the center wire 1 formed by twisting three solid welding wires, the zirconium content in the weld deposited metal is changed to control the grain refinement, and finally the solidification cracks in the high-strength aluminum alloy welding process are suppressed. At the same time, the gap between the center wire and the gap between the center wire and the peripheral wire are filled with powder, which plays a role in improving weld formation, stabilizing the arc, increasing the penetration depth, reducing spatter, promoting combustion, and purifying the weld metal. The mass fraction of zirconium in the zirconium wire is not less than 99.9%, and the mass fraction of aluminum in the aluminum alloy welding wire is not less than 99%.

[0035] In one embodiment, the alloying agent includes the following components in mass fractions: 1.2-4.2 parts of Cu powder, 1.2-2.5 parts of Mg powder, 0.3-0.5 parts of Mn powder, and 0.2-0.4 parts of Cr powder; the activating agent includes the following components in mass fractions: 5-10 parts of titanium dioxide, 5-10 parts of chromium oxide, 5-8 parts of sodium fluoride, 4-10 parts of lithium fluoride, 2-8 parts of potassium fluorozirconate, 0.1-0.8 parts of sodium stearate, and 0.1-0.6 parts of cerium oxide. The combustion aid includes the following components in mass fractions: 2-3 parts of potassium chlorate, 1-2 parts of magnesium oxide, and 0.1-1 parts of rare earth scandium zirconium alloy powder.

[0036] Metal powders such as Mg powder, Cu powder, Mn powder, Cr powder, etc. are added in the form of high-purity metal powders with a mass purity greater than 99.9%. The metal powders are spherical or nearly spherical, with a powder particle size of 30 to 50 μm and an oxygen content of less than 50 ppm.

[0037] Among them, the content of TiO2 in the titanium dioxide component of the active agent is not less than 97% by mass, the content of Cr2O3 in the chromium oxide component is not less than 96% by mass, the content of NaF in the sodium fluoride component is not less than 95% by mass, the content of LiF in the lithium fluoride component is not less than 97% by mass, the content of potassium fluorozirconate is not less than 95% by mass, and the content of sodium stearate is CH3(CH2) by mass. 16 COONa is not less than 98%, CeO2 is not less than 99% by mass, KClO3 is not less than 97% by mass, MgO is not less than 98% by mass, the scandium-zirconium alloy powder has a scandium-zirconium mass ratio of 3:1, and the mass purity of scandium and zirconium is 99.9-99.99%.

[0038] Impurities that may affect the performance of the medicine powder are not allowed to be contained in the medicine powder, and the particle size of the medicine powder prepared by mixing treatment does not exceed 50 μm.

[0039] The components and functions of the welding wire are as follows:

[0040] Zr: It reacts with the substrate to form Al3Zr. Its metallurgical chemical reaction is [Zr]+3Al→Al3Zr. The generated Al3Zr phase can serve as a nucleation core to promote the formation of fine equiaxed crystals of α-Al. The fine equiaxed grains are easier to coordinate the deformation between the grains, thereby inhibiting solidification cracks. Fine Al3Zr phase With Al matrix They have similar crystal structures and therefore have good crystal coherence. At the same time, since the Al3Zr phase is generated by in-situ reaction rather than being added into the matrix, the interface between the two phases is clean and pollution-free. In addition, Al3Zr particles can pin dislocations, prevent dislocation movement, and improve joint strength.

[0041] The main functions of the alloy powder in the above-mentioned powder are as follows:

[0042] Cu: plays a role in solid solution strengthening and improves the mechanical properties of the alloy;

[0043] Mg: It is beneficial to improve the hardness of the weld without significantly reducing the plasticity;

[0044] Mn: plays a role in microalloying and toughness, reduces the corrosion sensitivity of the weld, and especially improves the resistance to stress corrosion cracking;

[0045] Cr: has similar effects to Mn, and has a synergistic effect when added together with Mn.

[0046] The main functions of the active agent in the above-mentioned powder are as follows:

[0047] The role of titanium dioxide is to stabilize the arc, improve weld formation, and increase weld penetration. At the same time, the addition of titanium dioxide can improve the bonding strength between the flux and the wire. The role of chromium oxide is mainly to improve weld formation and increase weld penetration. The role of lithium fluoride and sodium fluoride is to stabilize the arc, reduce the content of diffuse hydrogen in the deposited metal, and improve weld formation. The role of potassium fluorozirconate is to stabilize the arc and reduce the content of diffuse hydrogen in the deposited metal. The role of cerium oxide is to reduce the surface tension of the molten droplet, promote the transition of the molten droplet and reduce spatter. Sodium stearate is mainly used as a lubricant to improve the wire feeding performance of the welding wire and increase the bonding strength between the flux and the wire.

[0048] The main functions of the combustion aid in the above-mentioned powder are as follows:

[0049] Among the welding wires considered, the melting points of zirconium welding wire and aluminum alloy welding wire are quite different (the melting point of zirconium welding wire is 1800℃, and the melting point of aluminum welding wire is 600℃). Therefore, potassium chlorate is added to improve the combustion performance of the welding wire body and ensure that the welding wire can be fully melted during the welding process. At the same time, magnesium oxide can promote the combustion of the welding wire. Rare earth scandium zirconium alloy powder can not only promote the combustion of the welding wire, but also purify the weld metal as a rare earth element.

[0050] The present invention also provides a method for preparing the stranded wire welding wire capable of inhibiting solidification cracking of high-strength aluminum alloy as described above, the preparation method mainly comprising the following steps:

[0051] (1) Use commercially available solid welding wire and clean the oil and rust on the surface of the welding wire.

[0052] (2) Three solid core welding wires are twisted together to form a center wire, and an existing twisting machine is used to complete the center wire twisted wire welding wire blank.

[0053] (3) Mix the drug powder in an existing conventional powder mixer for 10 to 20 minutes according to the formula, and grind the mixed powder in a ball mill until it can pass through a 460-mesh sieve (with a diameter not exceeding 30 μm) to obtain drug powder. The drug powder is composed of an alloying agent, an active agent and a combustion aid, the alloying agent includes the following components in mass fractions: 1.2 to 4.2 parts of Cu powder, 1.2 to 2.5 parts of Mg powder, 0.3 to 0.5 parts of Mn powder, and 0.2 to 0.4 parts of Cr powder; the active agent includes the following components in mass fractions: 5 to 10 parts of titanium dioxide, 5 to 10 parts of chromium oxide, 5 to 8 parts of sodium fluoride, 4 to 10 parts of lithium fluoride, 2 to 8 parts of potassium fluorozirconate, 0.1 to 0.8 parts of sodium stearate, and 0.1 to 0.6 parts of cerium oxide; the combustion aid includes the following components in mass fractions: 2 to 3 parts of potassium chlorate, 1 to 2 parts of magnesium oxide, and 0.1 to 1 parts of rare earth scandium zirconium alloy powder.

[0054] The powder contains impurities that do not affect the performance. At the same time, the powder particles have a certain degree of adhesion when extruded and filled onto the stranded wire, making the powder easy to stick to the gaps between the wires.

[0055] (4) The stranded wire blank is subjected to boronization treatment according to the existing conventional process, so that a borax layer with a thickness of 0.25 to 0.50 μm adheres to its surface, and then dried at a drying temperature between 100°C and 150°C. The boronization treatment is driven by a wire drawing machine, so that the welding wire passes through the boronization tank used in the existing welding wire production to complete the boronization. The surface of the boronized welding wire is bright black. The borax on the surface of the boronized welding wire has a certain degree of adhesion, which can make the powder firmly adhere to the gap between the welding wires; at the same time, borax is a non-corrosive flux. During welding, the flux can reduce the melting point of the oxide, enhance the fluidity of the metal, and improve the welding quality.

[0056] (5) The boronized stranded wire blank is immediately passed through a powder box containing powder (the surface temperature of the stranded wire is between 100°C and 150°C) to press the powder into the gaps between the stranded wires. Driven by an existing wire drawing machine, the stranded wire blank enters from one end of the powder box and exits from the other end. The exit end is provided with an existing wire drawing die. The stranded wire blank passes through the wire drawing die. The inner hole diameter of the wire drawing die outlet is 0.01mm to 0.04mm larger than the diameter of the stranded wire. The powder is squeezed into the gaps between the stranded wires by using the taper of the front end of the inner hole of the wire drawing die, and the powder is firmly bonded to the gaps between the wires by using the adhesion of borax.

[0057] (6) The obtained stranded wire with powder filled in the gap is driven by a wire drawing machine and passed through a sizing and polishing die to complete the center wire stranded wire.

[0058] (7) The finished stranded wire is used as the intermediate wire and the 6-strand aluminum alloy wire is used as the peripheral wire, and a stranding machine is used to strand the wire into a plurality of stranded wire blanks. The diameters of the peripheral wires are the same, and the diameter of the intermediate wire is 1.015 to 1.030 times the diameter of the peripheral wire.

[0059] (8) Repeat steps (4)-(5) for the multi-stranded wire blank obtained in step (7) to complete the boronized powder pressing treatment. Driven by a wire drawing machine, the obtained stranded wire with gaps filled with powder is passed through a sizing and polishing die to complete the multi-stranded wire, and commercially available polishing oil is added according to the existing welding wire production process to obtain a finished stranded wire that inhibits solidification cracks in high-strength aluminum alloys. The inner hole diameter of the above-mentioned sizing and polishing die is 0 to 0.01 mm smaller than the diameter of the stranded wire. After passing through the die, the powder adhered to the outer wire surface of the stranded wire is cleaned, and the surface reveals a metallic luster, which is conducive to conductivity during welding. The above-mentioned steps (4)-(6) use a wire drawing machine to drive the stranded wire to move along the direction of the wire, and are completed continuously using the same wire drawing machine.

[0060] The stranded wire welding wire provided in this embodiment can be used in gas shielded welding, laser wire welding, laser arc hybrid welding, etc. The welding wire provided in this embodiment can be of any length and can also be wound into a coil, and is suitable for a variety of welding methods such as gas shielded welding, laser wire welding, laser arc hybrid welding, etc.

[0061] The present invention is further described in detail below with reference to several specific embodiments.

[0062] Embodiment 1:

[0063] A method for preparing a stranded wire welding wire capable of suppressing solidification cracking of a high-strength aluminum alloy provided in Example 1 of the present invention mainly comprises the following steps:

[0064] (1) Select one zirconium welding wire with a diameter of 0.2 mm and model ERZr2, and two aluminum alloy welding wires with a diameter of 0.2 mm and model SAl2319, and ensure that the oil and rust on the surface of the welding wires are clean.

[0065] (2) One strand of zirconium welding wire and two strands of aluminum alloy welding wire are used as raw materials for making the center wire, and an existing stranding machine is used to complete the center wire stranded wire blank.

[0066] (3) The alloying agent in the powder includes the following components by mass: 3.8 parts of Cu powder, 1.8 parts of Mg powder, 0.5 parts of Mn powder, and 0.2 parts of Cr powder. The active agent includes the following components by mass: 10 parts of titanium dioxide, 8 parts of chromium oxide, 5 parts of sodium fluoride, 8 parts of lithium fluoride, 5 parts of potassium fluorozirconate, 0.3 parts of sodium stearate, and 0.2 parts of cerium oxide. The combustion aid includes 3 parts of potassium chlorate, 2 parts of magnesium oxide, and 0.8 parts of rare earth scandium zirconium alloy powder. The powder contains impurities that do not affect the performance. According to the above formula, weigh the powders of each component, mix them in a conventional powder mixer for 15 minutes, and use a ball mill to ball mill the mixed powder until it can pass through a 460 mesh sieve (the particle size does not exceed 30 μm) to obtain powder. At the same time, when the powder particles are squeezed and filled into the gaps between the stranded wires, they have a certain degree of adhesion, so that the powder is easy to adhere to the gaps between the wires.

[0067] (4) The prepared stranded wire blank is subjected to boronization treatment according to the existing process, so that a borax layer with a thickness of 0.25 to 0.50 μm adheres to the surface of the stranded wire blank, and then dried at a drying temperature between 100° C. and 150° C.

[0068] (5) The boronized stranded wire blank is immediately passed through a powder box containing powder (the surface temperature of the stranded wire is between 100°C and 150°C) to press the powder into the gaps between the stranded wires. Driven by an existing wire drawing machine, the stranded wire blank enters from one end of the powder box and exits from the other end. The exit end is provided with an existing wire drawing die. The stranded wire blank passes through the wire drawing die. The inner hole diameter of the wire drawing die outlet is 0.02mm to 0.05mm larger than the diameter of the stranded wire. The powder is squeezed into the gaps between the stranded wires by using the taper of the front end of the inner hole of the wire drawing die, and the powder is firmly bonded to the gaps between the wires by using the adhesion of borax.

[0069] (6) The obtained stranded wire with powder filled in the gap is driven by a wire drawing machine and passed through a sizing and polishing die to complete the center wire stranded wire.

[0070] (7) The central stranded wire welding wire completed in step (6) is selected as the intermediate wire, and 6 strands of SAl2319 aluminum alloy welding wire with a diameter of 0.6 mm are used as the outer wires, and the diameter of the central wire is 1.015 to 1.030 times the diameter of the outer wire. The existing stranding machine is used to complete the multi-strand stranded wire welding wire blank.

[0071] (8) Repeat steps (4)-(5) for the multi-stranded wire blank obtained in step (7) to complete the boronization powder pressing treatment. Driven by a wire drawing machine, the obtained stranded wire with gaps filled with powder is passed through a sizing and polishing die to complete the multi-stranded wire. According to the existing welding wire production process, commercially available polishing oil is added, and the powder adhered to the outer wire surface of the stranded wire is cleaned, revealing a metallic luster on the surface, and a finished stranded wire with a diameter of 1.6 mm that inhibits solidification cracks of high-strength aluminum alloy is obtained. The inner hole diameter of the above-mentioned sizing and polishing die is 0 to 0.01 mm smaller than the diameter of the stranded wire.

[0072] Embodiment 2:

[0073] A method for preparing a stranded wire welding wire capable of suppressing solidification cracking of a high-strength aluminum alloy provided in Example 2 of the present invention mainly comprises the following steps:

[0074] (1) Two zirconium welding wires are selected, both with a diameter of 0.3 mm, model ERZr2, and one aluminum alloy welding wire is selected, with a diameter of 0.3 mm, model SAl2319.

[0075] (2) Two zirconium welding wires and one aluminum alloy welding wire are used as raw materials for making the center wire, and an existing stranding machine is used to complete the center wire stranding welding wire blank.

[0076] (3) The alloying agent in the powder includes the following components by mass: 4.0 parts of Cu powder, 1.6 parts of Mg powder, 0.4 parts of Mn powder, 0.3 parts of Cr powder, and the balance is an active agent; wherein the active agent includes the following components by mass: 8 parts of titanium dioxide, 6 parts of chromium oxide, 6 parts of sodium fluoride, 10 parts of lithium fluoride, 4 parts of potassium fluorozirconate, 0.4 parts of sodium stearate, and 0.4 parts of cerium oxide, and the combustion aid includes 2 parts of potassium chlorate, 1 part of magnesium oxide, and 0.5 parts of rare earth scandium zirconium alloy powder. The powder contains impurities that do not affect the performance. According to the above formula, weigh the powders of each component, mix them in a conventional powder mixer for 12 minutes, and use a ball mill to ball mill the mixed powder until it can pass through a 460 mesh sieve (particle size does not exceed 30μm) to obtain powder powder. At the same time, when the powder particles are squeezed and filled into the gaps between the stranded wires, they have a certain degree of adhesion, so that the powder is easy to adhere to the gaps between the wires.

[0077] (4) The prepared stranded wire blank is subjected to boronization treatment according to the existing process, so that a borax layer with a thickness of 0.25 to 0.50 μm adheres to the surface of the stranded wire blank, and then dried at a drying temperature between 120° C. and 170° C.

[0078] (5) The boronized stranded wire billet is immediately passed through a powder box containing powder (the surface temperature of the stranded wire is between 120°C and 170°C) to press the powder into the gaps between the stranded wires. Driven by an existing wire drawing machine, the stranded wire billet enters from one end of the powder box and exits from the other end. The exit end is provided with an existing wire drawing die. The stranded wire billet passes through the wire drawing die. The inner hole diameter of the wire drawing die outlet is 0.02mm to 0.05mm larger than the diameter of the stranded wire. The powder is squeezed into the gaps between the stranded wires by using the taper of the front end of the inner hole of the wire drawing die, and the powder is firmly bonded to the gaps between the wires by using the adhesion of borax.

[0079] (6) The obtained stranded wire with powder filled in the gap is driven by a wire drawing machine and passed through a sizing and polishing die to complete the center wire stranded wire.

[0080] (7) The central stranded wire welding wire completed in step (6) is selected as the intermediate wire, and 6 strands of SAl2319 aluminum alloy welding wire with a diameter of 0.8 mm are used as the outer wires, and the diameter of the central wire is 1.015 to 1.030 times the diameter of the outer wire. The existing stranding machine is used to complete the multi-strand stranded wire welding wire blank.

[0081] (8) Repeat steps (4)-(5) for the multi-stranded wire blank obtained in step (7) to complete the boronization powder pressing treatment. Driven by a wire drawing machine, the obtained stranded wire with gaps filled with powder is passed through a sizing and polishing die to complete the multi-stranded wire, and commercially available polishing oil is added according to the existing welding wire production process. The powder adhered to the outer wire surface of the stranded wire is cleaned, and the surface is exposed to metallic luster, thereby obtaining a stranded wire product with a diameter of 2.4 mm that inhibits solidification cracks of high-strength aluminum alloy. The inner hole diameter of the above-mentioned sizing and polishing die is 0 to 0.01 mm smaller than the diameter of the stranded wire.

[0082] Example 3

[0083] A method for preparing a stranded wire welding wire capable of suppressing solidification cracking of a high-strength aluminum alloy provided in Example 3 of the present invention mainly comprises the following steps:

[0084] (1) Select three strands of zirconium welding wire, all with a diameter of 0.4 mm and model ERZr2.

[0085] (2) Three zirconium welding wires are used as the raw material for making the center wire, and the existing stranding machine is used to complete the center wire stranding welding wire blank.

[0086] (3) The alloying agent in the powder includes the following components by mass: 4.2 parts of Cu powder, 1.4 parts of Mg powder, 0.3 parts of Mn powder, 0.4 parts of Cr powder, and the balance is an active agent; wherein the active agent includes the following components by mass: 9 parts of titanium dioxide, 7 parts of chromium oxide, 5 parts of sodium fluoride, 9 parts of lithium fluoride, 6 parts of potassium fluorozirconate, 0.6 parts of sodium stearate, and 0.5 parts of cerium oxide. The combustion aid includes 1 part of potassium chlorate, 0.8 parts of magnesium oxide and 0.3 parts of rare earth scandium zirconium alloy powder. The powder contains impurities that do not affect the performance. According to the above formula, weigh the powders of each component, mix them in a conventional powder mixer for 20 minutes, and use a ball mill to ball mill the mixed powder until it can pass through a 460 mesh sieve (particle size does not exceed 30μm) to obtain powder. At the same time, when the powder particles are squeezed and filled into the gaps between the stranded wires, they have a certain degree of adhesion, so that the powder is easy to adhere to the gaps between the wires.

[0087] (4) The prepared stranded wire blank is subjected to boronization treatment according to the existing process, so that a borax layer with a thickness of 0.25 to 0.50 μm adheres to the surface of the stranded wire blank, and then dried at a drying temperature between 150° C. and 200° C.

[0088] (5) The boronized stranded wire blank is immediately passed through a powder box containing powder (the surface temperature of the stranded wire is between 150°C and 200°C) to press the powder into the gaps between the stranded wires. Driven by an existing wire drawing machine, the stranded wire blank enters from one end of the powder box and exits from the other end. The exit end is provided with an existing wire drawing die. The stranded wire blank passes through the wire drawing die. The inner hole diameter of the wire drawing die outlet is 0.02mm to 0.05mm larger than the diameter of the stranded wire. The powder is squeezed into the gaps between the stranded wires by using the taper of the front end of the inner hole of the wire drawing die, and the powder is firmly bonded to the gaps between the wires by using the adhesion of borax.

[0089] (6) The obtained stranded wire with powder filled in the gap is driven by a wire drawing machine and passed through a sizing and polishing die to complete the center wire stranded wire.

[0090] (7) A completed center wire stranded wire welding wire is selected as the intermediate wire, and 6 strands of SAl2319 aluminum alloy welding wire with a diameter of 1.2 mm are used as the outer wires. The diameter of the center wire is 1.015 to 1.030 times the diameter of the outer wire. The existing stranding machine is used to complete the multi-strand stranded wire welding wire blank.

[0091] Repeat steps (4)-(5) for the multi-stranded wire blank obtained in step (7) to complete the boronized powder pressing treatment. Driven by a wire drawing machine, the obtained stranded wire with gaps filled with powder is passed through a sizing and polishing die to complete the multi-stranded wire, and commercially available polishing oil is added according to the existing welding wire production process. The powder adhered to the outer wire surface of the stranded wire is cleaned, and the surface is exposed to metallic luster, thereby obtaining a stranded wire product with a diameter of 3.6 mm that can inhibit solidification cracks of high-strength aluminum alloy. The inner hole diameter of the above-mentioned sizing and polishing die is 0 to 0.01 mm smaller than the diameter of the stranded wire.

[0092] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A stranded wire welding wire capable of suppressing solidification cracking of high-strength aluminum alloy, characterized in that: The stranded welding wire comprises a central wire, a peripheral wire and powder, wherein the central wire is formed by twisting a plurality of solid welding wires; the peripheral wire is arranged at the periphery of the central wire, and comprises a plurality of solid welding wires, wherein the peripheral wires are twisted together around the central wire to form a welding wire body of the stranded welding wire, and the powder is squeezed and filled in the gaps between the solid welding wires constituting the welding wire body; The multiple solid welding wires constituting the central wire include zirconium welding wire and aluminum alloy welding wire; the central wire includes one zirconium welding wire and two aluminum alloy welding wires, and the peripheral wires include six aluminum alloy welding wires; or, The central wire includes two zirconium welding wires and one aluminum alloy welding wire, and the peripheral wires include six aluminum alloy welding wires; or, The central wire includes three strands of zirconium welding wire, and the peripheral wire includes six strands of SAl2319 aluminum alloy welding wire.

2. The stranded wire welding wire capable of suppressing solidification cracking of high-strength aluminum alloy according to claim 1, characterized in that: The central wire is formed by twisting three solid welding wires, and the peripheral wires include six solid welding wires; the powder includes an alloying agent, an activating agent and a combustion aid.

3. The stranded wire welding wire capable of suppressing solidification cracking of high-strength aluminum alloy as claimed in claim 2, characterized in that: The alloying agent comprises the following components in parts by mass: 1.2 to 4.9 parts of metal Cu powder, 1.2 to 2.9 parts of metal Mg, 0.07 to 0.6 parts of metal Mn powder and 0.05 to 0.4 parts of metal Cr powder; the activating agent comprises the following components in parts by mass: 3 to 12 parts of titanium dioxide, 5 to 12 parts of chromium oxide, 0 to 12 parts of sodium fluoride, 0 to 11 parts of lithium fluoride, 0 to 8 parts of potassium fluorozirconate, 0.1 to 1.0 parts of sodium stearate and 0.1 to 1.0 parts of cerium oxide; the combustion aid comprises the following components in parts by mass: 0 to 4 parts of potassium chlorate, 0 to 2 parts of magnesium oxide and 0.1 to 1 parts of rare earth scandium zirconium alloy powder; the mass ratio of scandium to zirconium in the rare earth scandium zirconium alloy powder is 3:1, and the mass purity of scandium and zirconium is 99.9 to 99.99%.

4. The stranded wire welding wire capable of suppressing solidification cracking of high-strength aluminum alloy according to claim 1, characterized in that: The diameter of the central wire is 1.015 to 1.030 times the diameter of the solid welding wire constituting the peripheral wire.

5. The stranded wire welding wire capable of suppressing solidification cracking of high-strength aluminum alloy as claimed in claim 2, characterized in that: The alloying agent comprises the following components in parts by mass: 1.2 to 4.2 parts of Cu powder, 1.2 to 2.5 parts of Mg powder, 0.3 to 0.5 parts of Mn powder, and 0.2 to 0.4 parts of Cr powder; the activating agent comprises the following components in parts by mass: 5 to 10 parts of titanium dioxide, 5 to 10 parts of chromium oxide, 5 to 8 parts of sodium fluoride, 4 to 10 parts of lithium fluoride, 2 to 8 parts of potassium fluorozirconate, 0.1 to 0.8 parts of sodium stearate, and 0.1 to 0.6 parts of cerium oxide; the combustion aid comprises the following components in parts by mass: 0 to 3 parts of potassium chlorate, 0 to 2 parts of magnesium oxide, and 0.1 to 1 parts of rare earth scandium zirconium alloy powder.

6. The stranded wire welding wire capable of suppressing solidification cracking of high-strength aluminum alloy according to any one of claims 1 to 5, characterized in that: A borax layer is formed on the central wire and the peripheral wires, and the powder adheres to the gaps between the solid welding wires through the borax layer.

7. The stranded wire welding wire capable of suppressing solidification cracking of high-strength aluminum alloy according to claim 6, characterized in that: The thickness of the borax layer is 0.25-0.50 μm.

8. A method for preparing a stranded wire welding wire capable of suppressing solidification cracking of a high-strength aluminum alloy, characterized in that: The preparation method is used to prepare the stranded wire welding wire capable of suppressing solidification cracks of high-strength aluminum alloy as described in any one of claims 1 to 7.

9. The method for preparing a stranded wire welding wire capable of suppressing solidification cracking of a high-strength aluminum alloy as claimed in claim 8, characterized in that: After a borax layer is formed on the surface of the central wire and the peripheral wire through expansion treatment, powder is squeezed into the gap between the welding wires at a temperature of 150° C. to 200° C.

Citation Information

Patent Citations

  • Aluminium alloy welding wire containing TiB2 particles

    CN111112875A

  • High titanium / zirconium filler wire for aluminium alloys and method of welding

    CA2340827A1

  • Activated stranded wire welding wire for increasing penetration depth

    CN104227270A

  • Aluminum alloy welding wire and preparation method thereof

    CN106238952A

  • Cable formula welding wire

    CN207043592U

Cited By

  • Method and experimental device capable of inhibiting solidification cracks of high-strength aluminum alloy

    CN120962137A

  • Experimental device and method for swinging light beam assisted arc double-wire welding of high-strength aluminum alloy

    CN121042712A

  • Double-wire composite welding device and welding method for coupling light beam swing with TIG electric arc