Method for clarifying medium borosilicate glass, medium borosilicate glass and its application
A clarification method using NaCl, CeO2, and CaF2 in a ladder-shaped pipe system effectively addresses bubble discharge issues in medium-borosilicate glass, producing high-quality, non-toxic glass suitable for pharmaceutical applications.
Patent Information
- Application Number
- CN202310111431.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-02-14
AI Technical Summary
The high melting temperature of medium-borosilicate glass results in large viscosity, making it difficult to discharge bubbles, leading to defects in the finished glass, and existing clarifiers like arsenic trioxide and antimony trioxide are toxic and environmentally harmful.
A clarification method using a clarifier composition of NaCl, CeO2, and CaF2, with a clarification system featuring a ladder-shaped pipe and heating elements to facilitate bubble discharge, combined with a temperature-controlled process.
The method achieves effective bubble removal, producing high-quality medium-borosilicate glass with reduced bubbles and improved transparency, while being non-toxic and environmentally friendly.
Smart Images

Figure CN116161853B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of glass, and in particular to a medium-borosilicate glass clarification method, medium-borosilicate glass and applications thereof. Background Art
[0002] At present, with the development of my country's pharmaceutical industry, higher requirements have been put forward for the pharmaceutical packaging industry. The sodium-lime glass and low-borosilicate glass that were originally used in large quantities in the pharmaceutical glass industry have been gradually replaced by medium-borosilicate glass. Medium-borosilicate glass has good chemical stability and good acid and alkali resistance, and is a very commonly used pharmaceutical packaging material at this stage. However, due to the high melting temperature of the batch of medium-borosilicate glass, the viscosity of the glass liquid after melting is large, and the bubbles in it are not easy to discharge, resulting in small bubbles, gas lines and other defects in the finished glass. In order to discharge bubbles, it is necessary to use a clarifier to generate gas to expel the gas generated in the glass liquid, or to increase the diameter of the bubbles in the glass liquid so that the bubbles float up and escape from the glass liquid, thereby discharging the tiny bubbles in the glass liquid.
[0003] Commonly used clarifiers in the industry include arsenic trioxide, antimony trioxide, nitrates, sulfates, fluorides, chlorides, cerium oxide, etc. Arsenic trioxide and antimony trioxide are commonly used excellent clarifiers, but there are strict restrictions on highly toxic substances such as arsenic and antimony in pharmaceutical glass. On the other hand, a large amount of sulfate or use as a clarifier will cause environmental pollution or aggravate the erosion of kiln refractory materials.
[0004] CN112624605A discloses a medium borosilicate glass clarifier, which contains NaCl, CaF2, Na2SiF6 and optionally CeO2; wherein, relative to 100 parts by weight of the glass clarifier, the content of NaCl in the glass clarifier is greater than 30 parts by weight, the content of CaF2 is less than 50 parts by weight, the content of Na2SiF6 is less than 20 parts by weight, and the content of CeO2 is less than 5 parts by weight; the total content of NaCl, CaF2 and Na2SiF6 is greater than 95 parts by weight; the weight ratio of NaCl to CaF2 is (0.6-1.8):1, and the weight ratio of CaF2 to Na2SiF6 is (0.2-4):1. However, its clarification effect is still not ideal.
[0005] Therefore, it has become an inevitable trend to develop a glass clarification process that is non-toxic and harmless and has good clarification effect. Summary of the invention
[0006] The purpose of the present invention is to provide a medium-borosilicate glass clarification method which is non-toxic and harmless and has good clarification effect.
[0007] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for clarifying medium borosilicate glass, the method comprising: melting a glass raw material composition containing a clarifier to obtain glass liquid, introducing the glass liquid into a clarification system for clarification treatment to obtain clarified glass liquid;
[0008] Wherein, the clarifier contains NaCl, CeO2, CaF2, and NaNO3, and based on the total weight of the clarifier, the content of NaCl is 23.5-29.5% by weight, the content of CeO2 is 6-8% by weight, the content of CaF2 is 26-30% by weight, and the content of NaNO3 is 36.5-40.5% by weight;
[0009] The clarification system includes a clarification pipe horizontally arranged to circulate the glass liquid, the inner lower wall of the clarification pipe is provided with a ladder body, and the outer wall of the clarification pipe corresponding to the ladder body is provided with a heating element for heating the clarification pipe to allow bubbles in the glass liquid flowing through the surface of the ladder body to escape.
[0010] Preferably, based on the total weight of the clarifier, the content of NaCl is 25.5-27.5% by weight, the content of CeO2 is 6.5-7.8% by weight, the content of CaF2 is 26.8-29% by weight, and the content of NaNO3 is 38-39% by weight.
[0011] More preferably, the content of the clarifier is 0.5-3 wt % based on the total weight of the glass raw material composition.
[0012] Preferably, during the clarification process, the temperature of the clarification pipeline is controlled to be 1600°C-1650°C.
[0013] Preferably, the inner diameter of the clarification pipe is d, the distance h between the upper surface of the ladder body and the inner upper wall of the clarification pipe is not less than 0.5d, and the upper surface of the ladder body is horizontal;
[0014] The lower surface of the ladder body is in contact with the inner lower wall of the clarification pipe.
[0015] Alternatively, the lower surface of the ladder body is integrally formed with the inner lower wall of the clarification pipe.
[0016] More preferably, the angle θ between the inclined surface of the ladder and the horizontal plane is 5°-15°;
[0017] There is a height difference P between the top of the inclined surface of the ladder and the upper surface of the ladder.
[0018] Preferably, the inner diameter d of the clarification pipe is 100 mm-200 mm, and the flow rate of the molten glass when flowing through the clarification pipe is 200 Kg / h-800 Kg / h.
[0019] Preferably, the length of the clarification pipeline is L, and the length of the ladder is l, wherein l≥L / 3.
[0020] Preferably, the clarification system further comprises a molding control device, which comprises a temperature control pipe, a stirring barrel, and a discharge pipe.
[0021] The temperature control pipe is horizontally connected to the clarification pipe to control the temperature of the glass liquid after flowing through the clarification pipe;
[0022] One end of the stirring barrel is connected to the temperature control pipe, and the other end is connected to the discharge pipe, and the stirring barrel is used to stir the glass liquid;
[0023] The temperature of the temperature control pipe is controlled at 1320°C-1360°C, the temperature of the stirring barrel is controlled at 1300°C-1340°C, and the temperature of the discharge pipe is controlled at 1280°C-1320°C.
[0024] A second aspect of the present invention provides a medium-borosilicate glass, which is obtained by subjecting clarified glass liquid to a forming annealing treatment, wherein the clarified glass liquid is clarified glass liquid obtained by the clarification method provided in the first aspect of the present invention.
[0025] The third aspect of the present invention provides application of the medium-borosilicate glass provided in the second aspect in the medical field.
[0026] The clarification method provided by the present invention adds the clarifier provided by the present invention to the glass raw material composition, and performs clarification treatment in conjunction with the clarification system provided by the present application with a ladder body, so that the glass liquid can continuously discharge bubbles at different stages of the clarification system to obtain clarified glass liquid with excellent clarification effect. The medium-borosilicate glass prepared by using the clarified glass liquid has significantly reduced number of bubbles, and the prepared medium-borosilicate glass has excellent properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a schematic structural diagram of a clarification system provided by the present invention according to a preferred embodiment;
[0028] Figure 2 It is a schematic structural diagram of a clarification pipeline and a ladder body provided by the present invention according to a preferred embodiment.
[0029] Description of Reference Numerals
[0030] 1. Clarifying pipe, 2. Ladder, 3. Heating element, 4. Temperature control pipe, 5. Mixing barrel, 6. Discharging pipe, 7. Cooling pipe, 801. First heating device, 802. Second heating device, 803. Third heating device, 901. First flange, 902. Second flange, 903. Third flange, 904. Fourth flange. DETAILED DESCRIPTION
[0031] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0032] As mentioned above, the present invention provides a method for clarifying medium borosilicate glass, the method comprising: melting a glass raw material composition containing a clarifier to obtain glass liquid, introducing the glass liquid into a clarification system for clarification treatment to obtain clarified glass liquid;
[0033] Wherein, the clarifier contains NaCl, CeO2, CaF2, and NaNO3, and based on the total weight of the clarifier, the content of NaCl is 23.5-29.5% by weight, the content of CeO2 is 6-8% by weight, the content of CaF2 is 26-30% by weight, and the content of NaNO3 is 36.5-40.5% by weight;
[0034] The clarification system includes a clarification pipe horizontally arranged to circulate the glass liquid, the inner lower wall of the clarification pipe is provided with a ladder body, and the outer wall of the clarification pipe corresponding to the ladder body is provided with a heating element for heating the clarification pipe to allow bubbles in the glass liquid flowing through the surface of the ladder body to escape.
[0035] The clarification method provided by the present invention adds the clarifier provided by the present invention to the glass raw material composition, and performs clarification treatment in conjunction with the clarification system provided by the present application with a ladder body, so that the glass liquid can continuously discharge bubbles at different stages of the clarification system to obtain clarified glass liquid with excellent clarification effect. The medium-borosilicate glass prepared by using the clarified glass liquid has significantly reduced bubble number and excellent performance.
[0036] According to a preferred embodiment of the present invention, based on the total weight of the clarifier, the content of NaCl is 25.5-27.5% by weight, the content of CeO2 is 6.5-7.8% by weight, the content of CaF2 is 26.8-29% by weight, and the content of NaNO3 is 38-39% by weight. The clarifier in this preferred embodiment can not only improve the clarification effect, but also has a certain decolorization effect, can weaken the coloring effect of iron compounds in the glass on the glass, and make the obtained medium borosilicate glass clearer and more transparent.
[0037] It should be noted that commonly used clarifiers in the industry include arsenic trioxide, antimony trioxide, nitrates, sulfates, fluorides, chlorides, cerium oxide, etc. Arsenic trioxide and antimony trioxide are commonly used excellent clarifiers. However, pharmaceutical glass has strict restrictions on highly toxic substances such as arsenic and antimony, and a large amount of sulfate or used as a clarifier will cause environmental pollution or aggravate the erosion of kiln refractory materials. The clarifier provided by the present invention does not contain the above-mentioned highly toxic substances and sulfates, and is a non-toxic, harmless and environmentally friendly clarifier. In addition, the content of NaNO3 in the clarifier provided by the present invention is not higher than 39% by weight. It is added as an additive to the glass raw material composition. In the process of melting the glass raw material composition in the kiln to obtain glass liquid, it has little corrosiveness to the kiln refractory materials.
[0038] According to a preferred embodiment of the present invention, the glass raw material composition comprises a substance capable of providing SiO2, a substance capable of providing Al2O3, a substance capable of providing Na2O, a substance capable of providing K2O, a substance capable of providing Li2O, a substance capable of providing CaO, a substance capable of providing BaO, a substance capable of providing CeO2, a substance capable of providing Cl element, and a substance capable of providing F element, and the composition ratio of the glass raw material composition is such that the glass produced has a content of 70-76% by weight of SiO2, and a content of 1% by weight of Al2O3, and a content of 2% by weight of Na2O3, and a content of 1% by weight of K2O, and a content of 2% by weight of Li2O. The content of I2O3 is 5-7% by weight, the content of B2O3 is 10-12% by weight, the content of Na2O is 6-8% by weight, the content of K2O is 0.9-2.3% by weight, the content of Li2O is 0.01-0.5% by weight, the content of CaO is 0.5-1.2% by weight, the content of BaO is 1-1.5% by weight, the content of CeO2 is 0.05-0.2% by weight, the content of Cl element is 0.1-0.2% by weight, and the content of F element is 0.1-0.2% by weight.
[0039] According to a preferred embodiment of the present invention, based on the total weight of the glass raw material composition, the content of the clarifier is 0.5-3% by weight, and further, the content of the clarifier is preferably 2-3% by weight. In this preferred case, the added amount of clarifier has a better clarification effect on the obtained clarified glass liquid.
[0040] According to a preferred embodiment of the present invention, the method for using the clarifier comprises: uniformly mixing the clarifier with other components in the glass raw material composition, and then melting the uniformly mixed materials to obtain glass liquid.
[0041] According to a more preferred embodiment of the present invention, the method for using the clarifier includes: firstly mixing the clarifier with the component of the substance capable of providing SiO2 to obtain an intermediate material, then mixing the intermediate material with other components in the glass raw material composition to obtain an intermediate material, and then melting the uniformly mixed materials to obtain glass liquid. Since the amount of the clarifier is relatively small, the clarifier is first mixed with a component with a higher content, such as a substance capable of providing SiO2, to obtain an intermediate material, and then the intermediate material is mixed with other components, so that the clarifier can be mixed more uniformly, effectively avoiding the problem that the clarifier is difficult to mix uniformly due to the small amount of the clarifier.
[0042] According to a preferred embodiment of the present invention, Figure 1 As shown, the heating element 3 is a heating coil, and the number of the heating coils is multiple. Further preferably, the number of the heating coils is three, which are respectively arranged on the outer wall of the clarification pipe 1 corresponding to two side surfaces and one plane of the ladder body 2.
[0043] According to a preferred embodiment of the present invention, Figure 2 As shown, the inner diameter of the clarification pipe 1 is d, the distance h between the upper surface of the ladder body 2 and the inner upper wall of the clarification pipe 1 is not less than 0.5d, the upper surface of the ladder body 2 is horizontal; the lower surface of the ladder body 2 is in contact with the inner lower wall of the clarification pipe 1. Under the preferred condition, the distance h between the upper surface of the ladder body 2 and the inner upper wall of the clarification pipe 1 can make the glass liquid flow through the surface of the ladder body 2 in a relatively thin form, and at the same time, the flow rate of the glass liquid will not be too small to make it difficult to flow.
[0044] According to a preferred embodiment of the present invention, Figure 2As shown, the inner diameter of the clarification pipe 1 is d, the distance h between the upper surface of the ladder body 2 and the inner upper wall of the clarification pipe 1 is not less than 0.5d, the upper surface of the ladder body 2 is horizontal, and the top of the inclined surface of the ladder body 2 is lower than the upper surface of the ladder body 2; the lower surface of the ladder body 2 is in contact with the inner lower wall of the clarification pipe 1, and the lower surface of the ladder body 2 is integrally formed with the inner lower wall of the clarification pipe 1. Under the preferred condition, the distance h between the upper surface of the ladder body 2 and the inner upper wall of the clarification pipe 1 can make the glass liquid flow through the surface of the ladder body 2 in a thinner form, and at the same time, the flow rate of the glass liquid will not be too small to make it difficult to flow.
[0045] According to a preferred embodiment of the present invention, Figure 2 As shown, the angle θ between the inclined surface of the ladder body 2 and the horizontal plane is 5°-15°. In a particularly preferred embodiment of the present invention, the angle θ between the inclined surface of the ladder body 2 and the horizontal plane is 10°. Under this preferred condition, when the glass liquid flows through the surface of the ladder body 2, it is easier to discharge bubbles.
[0046] According to a preferred embodiment of the present invention, Figure 2 As shown, there is a height difference P between the top of the inclined surface of the ladder body and the upper surface of the ladder body, that is, the top of the inclined surface of the ladder body 2 is lower than the upper surface P of the ladder body 2. The present invention has no special requirements on the numerical range of P, as long as a certain height difference is formed between the inclined surface of the ladder body and the upper surface of the ladder body, preferably, 0.2(dh)≤P≤0.4(dh), wherein d is the inner diameter of the clarification pipeline 1, and h is the distance between the upper surface of the ladder body and the inner upper wall of the clarification pipeline.
[0047] According to a preferred embodiment of the present invention, Figure 2 As shown, the inner diameter d of the clarification pipe 1 is 100mm-200mm, and the flow rate of the molten glass when flowing through the clarification pipe 1 is 200Kg / h-800Kg / h. Further preferably, the inner diameter d of the clarification pipe 1 is 145mm-185mm, and the flow rate of the molten glass when flowing through the clarification pipe 1 is 300Kg / h-650Kg / h. Under this preferred condition, the molten glass can flow through the surface of the ladder body 2 in a thinner form, and at the same time, the flow rate of the molten glass will not be too small to make it difficult to flow, so that the bubbles in the molten glass can be discharged to a greater extent.
[0048] According to a preferred embodiment of the present invention, Figure 2 As shown, the length of the clarification pipeline 1 is L, and the length of the ladder body 2 is l, wherein l≥L / 3. In this preferred case, the glass liquid can discharge more bubbles.
[0049] According to a preferred embodiment of the present invention, Figure 1 As shown, the clarification system also includes a molding control device, which includes a temperature control pipe 4, a stirring barrel 5, and a discharge pipe 6. The temperature control pipe 4 is horizontally connected to the clarification pipe 1 to regulate the temperature of the glass liquid after flowing through the clarification pipe 1; one end of the stirring barrel 5 is connected to the temperature control pipe 4, and the other end is connected to the discharge pipe 6. The stirring barrel 5 is used to stir the glass liquid to achieve a homogenization effect. The temperature of the temperature control pipe 4 is controlled to 1320℃-1360℃, the temperature of the stirring barrel 5 is controlled to 1300℃-1340℃, and the temperature of the discharge pipe 6 is controlled to 1280℃-1320℃. In this preferred case, the temperature and state of the clarified glass liquid used for molding are uniform.
[0050] According to a more preferred embodiment of the present invention, Figure 1 As shown, the temperature control pipe 4 is connected to the clarification pipe 1 via a first flange 901 .
[0051] According to a more preferred embodiment of the present invention, Figure 1 As shown, the temperature control pipeline 4 includes at least two horizontally connected pipelines, and the pipelines are connected by a second flange 902.
[0052] According to a more preferred embodiment of the present invention, Figure 1 As shown, a third flange 903 is provided at the top of the mixing barrel 5 , and the mixing barrel 5 is connected to the discharge pipe 6 via a fourth flange 904 .
[0053] By heating the first flange 901, the second flange 902, the third flange 903 and the fourth flange 904 respectively, the temperature of the temperature control pipe 4 and the mixing barrel 5 can be controlled. Figure 1 As shown, the first flange 901, the second flange 902, the third flange 903 and the fourth flange 904 are also connected by a cooling pipe 7. In this preferred case, the temperature of the temperature control pipe 4 and the mixing barrel 5 can be controlled more accurately.
[0054] According to a more preferred embodiment of the present invention, Figure 1 As shown, the side of the mixing barrel 5 is further provided with a first heating device 801 and a second heating device 802, and the top of the mixing barrel 5 is further provided with a third heating device 803, wherein the third heating device 803 is arranged on the third flange 903, and the first heating device 801, the second heating device 802, and the third heating device 803 are used to heat the upper part of the mixing barrel 5 to prevent the impurities volatilized from the glass liquid due to the low temperature of the upper part of the mixing barrel 5
[0055] According to a preferred embodiment of the present invention, the temperature of the melt treatment is 1550°C-1700°C, and the treatment time is 300min-400min. It should be noted that the present invention has no particular limitation on the method of melt treatment. For example, the melt treatment can be carried out in a kiln conventionally used by those skilled in the art.
[0056] According to a preferred embodiment of the present invention, during the clarification process, the temperature of the clarification pipe 1 is controlled to be 1600° C.-1650° C. Under this preferred condition, the clarification effect of the clarification process on the glass liquid is better.
[0057] According to a preferred embodiment of the present invention, the clarification pipe 1 is made of a platinum-rhodium alloy, wherein the platinum content of the platinum-rhodium alloy is 80wt% to 95wt%, and the rhodium content is 5wt% to 20wt%. For example, the platinum content of the platinum-rhodium alloy is 90wt%, and the rhodium content is 10wt%.
[0058] The second aspect of the present invention provides a medium-borosilicate glass, which is obtained by subjecting clarified glass liquid to a forming annealing treatment, wherein the clarified glass liquid is clarified glass liquid obtained by the clarification method provided in the first aspect of the present invention.
[0059] The third aspect of the present invention provides the application of the medium-borosilicate glass provided in the second aspect in the medical field.
[0060] The present invention will be described in detail below through examples. The experimental methods used in the following examples are conventional methods unless otherwise specified; the reagents, materials, etc. used in the following examples are all commercially available unless otherwise specified.
[0061] In the following examples, the clarifier is prepared from analytically pure substances of each component according to corresponding proportions.
[0062] Example 1
[0063] The glass raw material composition containing the clarifier is melted to obtain glass liquid, and the glass liquid is introduced into Figure 1 The clarification system shown in the figure is subjected to clarification treatment to obtain clarified glass liquid; wherein the temperature of the melting treatment is 1600° C. and the treatment time is 350 min; during the clarification treatment, the temperature of the clarification pipe 1 is controlled to be 1620° C., the temperature of the temperature control pipe 4 is controlled to be 1340° C., the temperature of the stirring barrel 5 is controlled to be 1320° C., the temperature of the discharge pipe 6 is controlled to be 1300° C., and the flow rate of the glass liquid in the clarification pipe 1 in the clarification system is 400 Kg / h;
[0064] The clarified glass liquid was introduced into a mold for molding, and then annealed at 570° C. for 30 minutes and cooled to room temperature (25° C.) to obtain medium-borosilicate glass B1.
[0065] Wherein, the clarifier contains NaCl, CeO2, CaF2, and NaNO3, and based on the total weight of the clarifier, the content of NaCl is 26.5 weight %, the content of CeO2 is 7.1 weight %, the content of CaF2 is 27.9 weight %, and the content of NaNO3 is 38.5 weight %;
[0066] Based on the total weight of the glass raw material composition, the content of the clarifier is 2 weight %. The composition ratio of the glass raw material composition is such that the component contents of the prepared medium borosilicate glass are as shown in Table 1.
[0067] Table 1
[0068] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[B2O3]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> <![CDATA[Li2O]]> CaO BaO <![CDATA[CeO2]]> Cl F weight% 72.45 6.01 11.23 7.2 1.6 0.1 0.7 0.4 0.15 0.15 0.15
[0069] like Figure 1 As shown, the clarification system includes a clarification pipeline 1, a ladder body 2 arranged on the lower wall of the clarification pipeline 1, a heating element 3, a temperature control pipeline 4 horizontally connected to the clarification pipeline 1, a stirring barrel 5 and a discharge pipe 6.
[0070] The clarification pipeline 1 is a platinum channel, the pipeline length L is 2000mm, the pipeline inner diameter d is 165mm, the length l of the ladder body 2 is 1700mm, the angle θ between the inclined surface of the ladder body 2 and the horizontal plane is 10°, the distance h between the upper surface of the ladder body and the inner upper wall of the clarification pipeline is 85mm, and the top of the inclined surface of the ladder body 2 is 25mm lower than the upper surface P of the ladder body 2;
[0071] The heating element 3 is a heating coil, and the number of the heating coils is 3, which are respectively arranged on the outer wall of the clarification pipe 1 corresponding to the left stage, the plane stage, and the right stage of the ladder body 2;
[0072] The temperature control pipe 4 is 2000 mm long and has an inner diameter of 215 mm. The temperature control pipe 4 is connected to the clarification pipe 1 via a first flange 901. The temperature control pipe 4 comprises two horizontally connected pipes, which are connected via a second flange 902.
[0073] The top of the mixing barrel 5 is provided with a third flange 903, the mixing barrel 5 is connected to the discharge pipe 6 via a fourth flange 904, and the first flange 901, the second flange 902, the third flange 903 and the fourth flange 904 are also connected via a cooling pipe 7;
[0074] The side of the mixing barrel 5 is further provided with a first heating device 801 and a second heating device 802 , and the top of the mixing barrel 5 is further provided with a third heating device 803 , wherein the third heating device 803 is arranged on the third flange 903 .
[0075] Embodiment 2-6
[0076] Medium borosilicate glasses B2-B6 were prepared by referring to the method of Example 1. The difference is that the component ratios of the clarifiers are different. The component ratios of the clarifiers used to prepare the medium borosilicate glasses B2-B6 are shown in Table 2.
[0077] Table 2
[0078] B2 B3 B4 B5 B6 NaCl / wt% 24.1 29.2 40.2 22.3 19.5 <![CDATA[CeO2 / wt%]]> 6.2 7.8 2.0 2.0 2.0 <![CDATA[CaF2 / wt%]]> 29.5 26.3 25.3 40.5 18.0 <![CDATA[NaNO3 / wt%]]> 40.2 36.7 32.5 35.2 60.5
[0079] Example 7
[0080] Medium borosilicate glass B7 was prepared by referring to the method of Example 1, except that the amount of the clarifier was different. Based on the total weight of the glass raw material composition, the content of the clarifier was 0.5 wt %.
[0081] Example 8
[0082] Medium borosilicate glass B8 was prepared by referring to the method of Example 1, except that the amount of the clarifier was different. Based on the total weight of the glass raw material composition, the content of the clarifier was 3 wt %.
[0083] Comparative Example 1
[0084] Medium borosilicate glass DB1 was prepared by referring to the method of Example 1, except that the clarifier was NaCl.
[0085] Comparative Example 2
[0086] Medium borosilicate glass DB2 was prepared by referring to the method of Example 1, except that the clarifier was CeO2.
[0087] Comparative Example 3
[0088] Medium borosilicate glass DB3 was prepared by referring to the method of Example 1, except that the clarifier was CaF2.
[0089] Comparative Example 4
[0090] Medium borosilicate glass DB4 was prepared by referring to the method of Example 1, except that the clarifier was NaNO3.
[0091] Comparative Example 5
[0092] Medium borosilicate glass B8 was prepared by referring to the method of Example 1, except that the amount of the clarifier was different. Based on the total weight of the glass raw material composition, the content of the clarifier was 0.2 wt %.
[0093] Comparative Example 6
[0094] Medium borosilicate glass B8 was prepared by referring to the method of Example 1, except that there was no ladder structure in the clarification pipeline of the clarification system, and the remaining structures and step parameters were the same as those of Example 1.
[0095] The following performance tests were performed on the medium-borosilicate glass obtained in the above examples and comparative examples according to the following methods. The test results are shown in Table 3.
[0096] Appearance color: Under bright natural light, visually inspect the color of the medium borosilicate glass obtained in the above embodiments and comparative examples.
[0097] Number of bubbles: Use a vernier caliper to detect the number of bubbles with a diameter greater than 0.10 mm in the medium borosilicate glass prepared in the above embodiments and comparative examples.
[0098] Density: The density was tested according to GB / T14901-94 using a density meter purchased from Qinhuangdao Xianhe Technology Development Co., Ltd., model MD-5 sinking-floating ratio density meter.
[0099] Thermal expansion coefficient: The borosilicate glass obtained in the above embodiments and comparative examples was cut and ground into sample strips of 4 mm*4 mm*25.40 mm, and its thermal expansion coefficient was measured. The thermal expansion coefficient of the glass was determined by the differential method. The measuring instrument was a DIL2012STD dilatometer purchased from ORTON, and the temperature measurement range was selected as 30°C-380°C.
[0100] Alkali resistance: According to the test of "YBB00352004-2015 Determination of glass resistance to corrosion by boiling mixed alkali aqueous solution", the alkali resistance of medicinal borosilicate glass should not be lower than level 2.
[0101] Acid resistance: According to the first method of "YBB00342004-2015 Determination of resistance of glass to boiling hydrochloric acid erosion", the acid resistance of medicinal borosilicate glass should meet level 1.
[0102] Table 3
[0103]
[0104]
[0105] Table 3 (Continued)
[0106]
[0107] It can be seen from the results in Table 3 that the clarification method provided by the present invention can improve the clarification effect and ensure the quality of the medium-borosilicate glass while ensuring that the medium-borosilicate glass meets the acid resistance and alkali resistance requirements for pharmaceutical use.
[0108] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for clarifying medium borosilicate glass, characterized in that: The clarification method comprises: melting a glass raw material composition containing a clarifier to obtain glass liquid, introducing the glass liquid into a clarification system for clarification treatment to obtain clarified glass liquid; Wherein, the clarifier contains NaCl, CeO2, CaF2, and NaNO3, and based on the total weight of the clarifier, the content of NaCl is 23.5-29.5% by weight, the content of CeO2 is 6-8% by weight, the content of CaF2 is 26-30% by weight, and the content of NaNO3 is 36.5-40.5% by weight; The clarification system comprises a clarification pipe arranged horizontally for circulating the glass liquid, the inner lower wall of the clarification pipe is provided with a ladder body, and the outer wall of the clarification pipe corresponding to the ladder body is provided with a heating element for heating the clarification pipe so that bubbles in the glass liquid flowing through the surface of the ladder body can escape; The temperature of the clarification pipeline is controlled to be 1600° C.-1650° C.; the inner diameter d of the clarification pipeline is 100 mm-200 mm, and the flow rate of the glass liquid when flowing through the clarification pipeline is 200 kg / h-800 kg / h; The clarification system further includes a molding control device, which includes a temperature control pipe, a stirring barrel, and a discharge pipe; the temperature control pipe is horizontally connected to the clarification pipe to control the temperature of the glass liquid after flowing through the clarification pipe; one end of the stirring barrel is connected to the temperature control pipe, and the other end is connected to the discharge pipe, and the stirring barrel is used to stir the glass liquid; The temperature of the temperature control pipe is controlled at 1320°C-1360°C, the temperature of the stirring barrel is controlled at 1300°C-1340°C, and the temperature of the discharge pipe is controlled at 1280°C-1320°C.
2. The clarification method according to claim 1, characterized in that Based on the total weight of the clarifier, the content of NaCl is 25.5-27.5% by weight, the content of CeO2 is 6.5-7.8% by weight, the content of CaF2 is 26.8-29% by weight, and the content of NaNO3 is 38-39% by weight.
3. The clarification method according to claim 1 or 2, characterized in that: Based on the total weight of the glass raw material composition, the content of the clarifier is 0.5-3% by weight.
4. The clarification method according to claim 1 or 2, characterized in that: The inner diameter of the clarification pipeline is d, the distance h between the upper surface of the ladder body and the inner upper wall of the clarification pipeline is not less than 0.5d, and the upper surface of the ladder body is horizontal; The lower surface of the ladder body is in contact with the inner lower wall of the clarification pipe. Alternatively, the lower surface of the ladder body is integrally formed with the inner lower wall of the clarification pipe.
5. The clarification method according to claim 4, characterized in that: The angle θ between the inclined surface of the ladder and the horizontal plane is 5°-15°; There is a height difference P between the top of the inclined surface of the ladder and the upper surface of the ladder.
6. The clarification method according to claim 1 or 2, characterized in that: The length of the clarification pipeline is L, and the length of the ladder is l, wherein l≥L / 3.
7. A medium borosilicate glass, characterized in that: The medium-borosilicate glass is obtained by subjecting clarified glass liquid to a forming and annealing treatment, wherein the clarified glass liquid is clarified glass liquid obtained by the clarification method described in any one of claims 1 to 6.
8. Application of the medium-borosilicate glass according to claim 7 in the medical field.