A gray environmentally friendly polycarbonate film and preparation method thereof

By using a gray environmentally friendly polycarbonate film formula containing additives of sodium methoxide, dimethyl phosphite and acrylamide on the meter window and nameplate, the environmental pollution caused by printing color difference and hydrolysis of cyanochloride is solved, and the environmental pollution caused by hydrolysis of cyanochloride is achieved. Film materials with high light transmittance and flame retardant properties.

CN116162340BActive Publication Date: 2024-11-12JIANGSU HANYANG NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211530607.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2024-11-12
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

The gray film materials on existing meter windows and nameplates have large color differences due to environmental and temperature changes during the printing process, and the light stabilizer used contains easily hydrolyzed cyanochloride, resulting in reduced light transmittance and environmental pollution.

Method used

A gray environmentally friendly polycarbonate film is used, and its formulation includes polycarbonate resin, colorants, additives and titanium dioxide. Sodium methoxide, dimethyl phosphite and acrylamide are added to the additive to reduce the side effects of hydrolysis of tripyrocyanochloride , and control the temperature by specific pretreatment methods to enhance flame retardant performance.

Benefits of technology

The color difference uniformity and stability of the gray film is achieved, the waste and environmental pollution in production are reduced, strict environmental protection standards are met, and the light transmittance and flame retardant properties of the film are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a gray environmentally friendly polycarbonate film, in parts by weight, the raw materials of each component of the polycarbonate film are: 93-96 parts of polycarbonate resin, 0.15-0.2 parts of colorant, 3.5-4.5 parts of auxiliary agent, and 3-4 parts of titanium dioxide; wherein, the auxiliary agent contains light stabilizer GW-944, and cyanuric chloride is contained in the GW-944; wherein, the auxiliary agent also contains sodium methoxide, dimethyl phosphite and acrylamide. The components of the gray film produced by the present invention have good compatibility, and each component can be evenly dispersed in the substrate to form a homogeneous system. When used, there is no precipitate on the surface, non-toxic, harmless, pollution-free, and meets the strict environmental protection standards such as EU ROHS, REACH, TCO&Blue Angel. Compared with traditional transparent PC printing gray ink, its mechanical properties are more superior, the appearance quality is better, the color is more stable and consistent, and it can be recycled again, reducing the effect of the generation of waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of film preparation, in particular to a grey environmentally friendly polycarbonate film and a preparation method thereof. Background Art

[0002] At present, the film material used on the windows and nameplates of electric meters is generally polycarbonate. The preparation process is often to first use polycarbonate to prepare a transparent film, and then use gray ink to print it to obtain the target product. However, in actual operation, it is found that due to the influence of factors such as environment and temperature, when using gray ink for printing, there will be a large color difference (△E>1) between different batches, and the maximum yield of transparent printed gray is about 98%. Therefore, defective products will be produced in the actual production process, and due to the color difference, the qualified rate of the produced products will also be reduced.

[0003] In addition, various additives are added to the film materials used in the windows and nameplates of electric meters currently on the market. Among them, in order to prevent film aging, the use of hindered amine light stabilizers is a conventional choice. Hindered amine light stabilizers have low volatility, high thermal stability, and good compatibility with resins, and are widely used in the field of films. However, the film used on the windows and nameplates of electric meters needs to have a certain light transmittance, so the light stabilizer GW-944 with good light transmittance is selected. However, it is found during use that it contains a certain amount of easily hydrolyzed cyanuric chloride, which will produce impurities after hydrolysis, resulting in poor light transmittance of the product film. If it is removed, on the one hand, the toxicity of cyanuric chloride will cause physical harm to the staff; on the other hand, wastewater containing cyanuric chloride will also be produced, which will consume dissolved oxygen in the water, accelerate the eutrophication of the water body, and then cause environmental pollution. Therefore, a gray environmentally friendly polycarbonate film and its preparation method are urgently needed to solve the above problems. Summary of the invention

[0004] The object of the present invention is to provide a grey environmentally friendly polycarbonate film and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a gray environmentally friendly polycarbonate film, wherein the raw materials of the components of the polycarbonate film are, by weight: 93-96 parts of polycarbonate resin, 0.15-0.2 parts of colorant, 3.5-4.5 parts of auxiliary agent, and 3-4 parts of titanium dioxide;

[0006] Wherein, the auxiliary agent contains light stabilizer GW-944, and the GW-944 contains cyanuric chloride;

[0007] The auxiliary agent also contains sodium methoxide, dimethyl phosphite and acrylamide.

[0008] When selecting a light stabilizer, the present invention takes light transmittance into consideration, and therefore can only select light stabilizer GW-944, which is selected because it has better light transmittance than other light stabilizers. Since GW-944 contains a certain amount of cyanuric chloride, the present invention adds sodium methoxide, dimethyl phosphite and acrylamide to the types of auxiliary agents, and by adding these three raw materials, cyanuric chloride is fully utilized, thereby reducing the side effects of cyanuric chloride hydrolysis and ensuring the quality of the product.

[0009] Preferably, the colorant includes carbon black, titanium yellow or a mixture of the two.

[0010] Preferably, the raw materials of the colorant components are, by weight, 0.08-1 part of carbon black and 0.08-0.1 part of titanium yellow, for example, 0.085 part, 0.09 part, 0.095 part, etc. of carbon black and 0.085 part, 0.09 part, 0.095 part, etc. of titanium yellow.

[0011] Adding an appropriate amount of carbon black as a colorant to the gray pellet formula can give the polycarbonate gray film a certain antistatic effect, making the gray film more stable in the back-end processing.

[0012] Preferably, the auxiliary agent also includes a lubricant;

[0013] The lubricant includes an internal lubricant and an external lubricant;

[0014] Preferably, the components of the lubricant are, by weight, 0.1-0.2 parts of internal lubricant and 0.2-0.4 parts of external lubricant, for example, 0.12 parts, 0.14 parts, 0.16 parts, 0.18 parts, etc. of internal lubricant, and 0.22 parts, 0.24 parts, 0.26 parts, 0.28 parts, 0.30 parts, 0.32 parts, 0.34 parts, 0.36 parts, 0.38 parts, etc. of external lubricant.

[0015] A method for preparing a gray environmentally friendly polycarbonate film, the preparation method is as follows:

[0016] The colorant and titanium dioxide are mixed, polycarbonate resin and additives are added, the mixture is stirred evenly, melt-granulated, and dried to obtain the polycarbonate film;

[0017] The additive needs to be pretreated first, and the pretreatment method is as follows:

[0018] S1, mixing sodium methoxide, dimethyl phosphite and acrylamide, heating and keeping warm, to obtain an intermediate;

[0019] S2. Mix GW-944 with acetone, add the intermediate in batches, then increase the temperature to complete the pretreatment.

[0020] Preferably, in step S1, the added temperature is 58-60°C, such as 58.5°C, 59°C, 59.5°C, etc.;

[0021] In step S2, the temperature is raised to 60-80°C, such as 65°C, 70°C, 75°C, etc.

[0022] Preferably, after drying, the mixture is fed into an extruder and then melt-extruded through a T-die.

[0023] Preferably, after being extruded through a T-die, three-roll calendering and shaping are performed, and then film drawing is performed to obtain the polycarbonate film.

[0024] Preferably, GW-944 is mixed with acetone, half of the intermediate by weight is added at 0-5°C, and the remaining intermediate by weight is added at 40-45°C. For example, half of the intermediate by weight is added at temperatures such as 0.1°C, 0.2°C, 0.3°C, 0.4°C, and the remaining intermediate is then added at temperatures such as 41°C, 42°C, 43°C, 44°C.

[0025] Since the used light stabilizer contains a certain amount of cyanuric chloride, the present invention removes it by adding sodium methoxide, dimethyl phosphite and acryloyl. During the reaction, the temperature needs to be controlled to be 0-5°C and 40-45°C. The sodium methoxide, dimethyl phosphite and acryloyl added in batches can react with cyanuric chloride to obtain a triazine-based phosphorus flame retardant, thereby enhancing the flame retardant performance of the product.

[0026] Compared with the prior art, the beneficial effects achieved by the present invention are: the gray film formula raw materials are directly granulated into gray granules, which ensures the uniformity and stability of the gray color, and reduces the limitation of the subsequent production requiring several material tanks to dry the materials. The components of the gray film produced by the present invention have good compatibility, and the components can be evenly dispersed in the substrate to form a homogeneous system. When used, there is no precipitate on the surface, and it is non-toxic, harmless, and pollution-free, and meets the strict environmental protection standards of EU ROHS, REACH, TCO & Blue Angel, etc.

[0027] Compared with traditional transparent PC printing gray ink, it has more superior mechanical properties, better appearance quality, more stable and consistent color, and can be recycled to reduce waste generation.

[0028] The present invention provides a preparation method of GW-944, and the preparation method is as follows:

[0029] Dissolve cyanuric chloride in ice toluene solution, add tert-octylamine, control the pH between 6-8, react for 3 hours, add N,N′-di(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine after the reaction, heat to react at 65°C, pH between 8-9, heat to 170-180°C after the reaction, react for 8 hours, and then obtain GW-94.

[0030] Since the boiling point of cyanuric chloride is 190° C., a certain amount of cyanuric chloride residue will be generated during the preparation process, thereby affecting the effect of the light stabilizer. The present invention removes the residual cyanuric chloride by pretreating the light stabilizer, thereby ensuring the comprehensive performance of the product. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] A grey environmentally friendly polycarbonate film, wherein the raw materials of the components of the polycarbonate film are, by weight: 93 parts of polycarbonate resin, 0.15 parts of colorant, 3.5 parts of auxiliary agent, and 3 parts of titanium dioxide;

[0034] The auxiliary agent contains light stabilizer GW-944, and the GW-944 contains cyanuric chloride;

[0035] The auxiliary agent also contains sodium methoxide, dimethyl phosphite and acrylamide.

[0036] In parts by weight, the raw materials of each component of the colorant are: 0.08 parts of carbon black and 0.08 parts of titanium yellow.

[0037] The auxiliary agent also includes a lubricant;

[0038] The lubricant includes an internal lubricant and an external lubricant.

[0039] In terms of weight, the raw materials of each component of the lubricant are: 0.1 part of internal lubricant and 0.2 part of external lubricant.

[0040] The preparation method is as follows:

[0041] S1, mixing sodium methoxide, dimethyl phosphite and acrylamide, heating to 58° C., and keeping the temperature to obtain an intermediate;

[0042] S2. Mix GW-944 and acetone, add half of the intermediate by weight at 0°C, add the remaining intermediate by weight at 40°C, then raise the temperature to 60°C, and the pretreatment is completed.

[0043] S3, mixing the colorant and titanium dioxide, adding polycarbonate resin and additives, stirring evenly, melt granulating, drying, feeding into an extruder, and then passing through a T-die, extruding through the T-die, and then calendering and shaping by three rollers, and then drawing a film to obtain the polycarbonate film.

[0044] Example 2

[0045] The raw material components are different from those in Example 1 only in that, in this example, 94 parts of polycarbonate resin, 0.16 parts of colorant, 3.6 parts of auxiliary agent, 3.3 parts of titanium dioxide, 0.09 parts of carbon black, 0.09 parts of titanium yellow, 0.15 parts of internal lubricant, and 0.25 parts of external lubricant are used;

[0046] The preparation method is different from Example 1 only in that the heating to 59°C in step S1 is performed; step S2 is to mix GW-944 with acetone, add half the weight of the intermediate at 1°C, add the remaining weight of the intermediate at 42°C, then heat to 63°C, and the pretreatment is completed.

[0047] Example 3

[0048] The raw material components are different from those in Example 1 only in that, in this example, 95 parts of polycarbonate resin, 0.17 parts of colorant, 3.8 parts of auxiliary agent, 3.4 parts of titanium dioxide, 0.095 parts of carbon black, 0.095 parts of titanium yellow, 0.17 parts of internal lubricant, and 0.3 parts of external lubricant are used;

[0049] The preparation method is different from Example 1 only in that the heating to 59.5°C in step S1 is performed; step S2 is to mix GW-944 with acetone, add half the weight of the intermediate at 3°C, add the remaining weight of the intermediate at 44°C, then heat to 67°C, and the pretreatment is completed.

[0050] Example 4

[0051] The raw material components are different from those in Example 1 only in that, in this example, 95 parts of polycarbonate resin, 0.17 parts of colorant, 3.8 parts of auxiliary agent, 3.6 parts of titanium dioxide, 0.09 parts of carbon black, 0.1 parts of titanium yellow, 0.16 parts of internal lubricant, and 0.35 parts of external lubricant are used;

[0052] The preparation method is different from Example 1 only in that the heating to 60°C in step S1 is performed; step S2 is to mix GW-944 with acetone, add half the weight of the intermediate at 4°C, add the remaining weight of the intermediate at 44°C, then heat to 78°C, and the pretreatment is completed.

[0053] Example 5

[0054] The raw material components are different from those in Example 1 only in that, in this example, 96 parts of polycarbonate resin, 0.2 parts of colorant, 4.5 parts of auxiliary agent, 4 parts of titanium dioxide, 1 part of carbon black, 0.1 parts of titanium yellow, 0.2 parts of internal lubricant, and 0.4 parts of external lubricant are used;

[0055] The preparation method is different from Example 1 only in that the heating to 60°C in step S1 is performed; step S2 is to mix GW-944 with acetone, add half the weight of the intermediate at 5°C, add the remaining weight of the intermediate at 45°C, then heat to 80°C, and the pretreatment is completed.

[0056] Example 6

[0057] The raw material components are different from those in Example 1 only in that, in this example, 95 parts of polycarbonate resin, 0.17 parts of colorant, 3.8 parts of auxiliary agent, 3.6 parts of titanium dioxide, 0.1 parts of carbon black, 0.1 parts of titanium yellow, 0.19 parts of internal lubricant, and 0.4 parts of external lubricant are used;

[0058] The preparation method is different from Example 1 only in that the heating to 57°C in step S1 is performed; step S2 is to mix GW-944 with acetone, add half the weight of the intermediate at 5°C, add the remaining weight of the intermediate at 43°C, and then heat to 75°C to complete the pretreatment.

[0059] Comparative Example 1

[0060] The product is obtained by printing the most common polycarbonate resin film on the market with gray pigment.

[0061] Comparative Example 2

[0062] The only difference from Example 1 in terms of raw material components is that in this example, the auxiliary agent does not contain sodium methoxide, dimethyl phosphite and acrylamide;

[0063] The preparation method is:

[0064] The colorant and titanium dioxide are mixed, and polycarbonate resin and additives are added. After being mixed and stirred evenly, they are melt-granulated, dried, and sent to an extruder. After being extruded through a T-die, three-roll calendering and shaping are performed, and then film drawing is performed to obtain the polycarbonate film.

[0065] experiment

[0066] The electric meter windows and nameplates prepared in Examples 1-6 and Comparative Examples 1-2 were tested for color difference, and the results were as follows:

[0067] Test example Color difference (△E) Test example Color difference (△E) Example 1 △E<1 Example 5 △E<1 Example 2 △E<1 Example 6 △E<1 Example 3 △E<1 Comparative Example 1 △E>1 Example 4 △E<1 Comparative Example 2 △E<1

[0068] Table 1

[0069] The color yield test was conducted on the electric meter windows and nameplates prepared in Examples 1-6 and Comparative Examples 1-2, and the results were as follows:

[0070] Test example Color yield (%) Test example Color yield (%) Example 1 99.5% Example 5 99.5% Example 2 99.5% Example 6 99.5% Example 3 99.5% Comparative Example 1 98% Example 4 99.5% Comparative Example 2 99.5%

[0071] Table 2

[0072] The flame retardant properties of the films prepared in Examples 1-6 and Comparative Examples 1-2 were tested, and the results were as follows:

[0073] Test example Flame retardant properties Test example Flame retardant properties Example 1 excellent Example 5 excellent Example 2 excellent Example 6 excellent Example 3 excellent Comparative Example 1 generally Example 4 excellent Comparative Example 2 generally

[0074] Table 3

[0075] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A grey environmentally friendly polycarbonate film, Features: In terms of weight, the raw materials of the components of the polycarbonate film are: 93-96 parts of polycarbonate resin, 0.15-0.2 parts of colorant, 3.5-4.5 parts of auxiliary agent, and 3-4 parts of titanium dioxide; The auxiliary agent contains light stabilizer GW-944, and the GW-944 contains cyanuric chloride; The auxiliary agent also contains sodium methoxide, dimethyl phosphite and acrylamide; The additive needs to be pretreated first, and the pretreatment method is as follows: S1, mixing sodium methoxide, dimethyl phosphite and acrylamide, heating and keeping warm, to obtain an intermediate; S2, GW-944 is mixed with acetone, half of the intermediate is added at 0-5°C, and the remaining intermediate is added at 40-45°C, and the pretreatment is completed; Wherein, in step S1, the added temperature is 58-60°C.

2. A grey environmentally friendly polycarbonate film according to claim 1, Features: The colorant includes one of carbon black and titanium yellow or a mixture of the two.

3. A grey environmentally friendly polycarbonate film according to claim 2, Features: In parts by weight, the raw materials of the colorant components are: 0.08-1 part of carbon black and 0.08-0.1 part of titanium yellow.

4. The gray environmentally friendly polycarbonate film according to claim 1, Features: The auxiliary agent also includes a lubricant; The lubricant includes an internal lubricant and an external lubricant.

5. A grey environmentally friendly polycarbonate film according to claim 4, Features: In terms of weight, the raw materials of the components of the lubricant are: 0.1-0.2 parts of internal lubricant and 0.2-0.4 parts of external lubricant.

6. A method for preparing a gray environmentally friendly polycarbonate film, Features: The preparation method is as follows: The colorant and titanium dioxide are mixed, polycarbonate resin and additives are added, the mixture is stirred evenly, melt-granulated, and dried to obtain the polycarbonate film; The additive needs to be pretreated first, and the pretreatment method is as follows: S1, mixing sodium methoxide, dimethyl phosphite and acrylamide, heating and keeping warm, to obtain an intermediate; S2, GW-944 is mixed with acetone, half of the intermediate is added at 0-5°C, and the remaining intermediate is added at 40-45°C, and the pretreatment is completed; Wherein, in step S1, the adding temperature is 58-60°C; and the GW-944 contains cyanuric chloride.

7. A method for preparing a gray environmentally friendly polycarbonate film according to claim 6, Features: After drying, it is sent to the extruder and then melted and extruded through a T-type die.

8. The method for preparing a gray environmentally friendly polycarbonate film according to claim 7, Features: After being extruded through a T-shaped die, three-roll calendering and shaping are performed, and then film drawing is performed to obtain the polycarbonate film.