Preparation and application of a pyrolytic biochar / geopolymer composite material

The pyrolytic biochar/dipolymer composite material prepared by mixing fly ash, straw powder with potassium hydroxide and pyrolyzed, solved the problem of poor performance of existing materials in removing lead ions in water and passivating soil lead. , efficient adsorption and passivation are achieved, and excellent removal and passivation effects are shown in particular under pyrolysis conditions of 300°C to 700°C.

CN116173905BActive Publication Date: 2024-11-22XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310280974.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-11-22
Estimated Expiration
2043-03-21

AI Technical Summary

Technical Problem

Existing lead adsorption materials do not perform well in removing lead ions in water and passivating lead in soil, especially the biochar produced by direct pyrolysis has fewer pores and surfactant groups, making it difficult to effectively adsorption and passivation.

Method used

Fly ash, straw powder and aqueous solution of potassium hydroxide were mixed, and pyrolyzed, washed and dried in a nitrogen atmosphere to prepare a pyrolyzed biochar/diol polymer composite material, which was used to use the strong alkaline environment of diol polymer to treat biology. The carbon is modified to form a composite material with a higher specific surface area and pore structure.

Benefits of technology

It significantly improves the removal rate of lead ions in water and the passivation ability of soil lead by composite materials, and achieves efficient adsorption and passivation, especially when the pyrolysis temperature is 300℃~700℃, the removal rate and passivation rate are relatively high. High level.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116173905B_ABST
    Figure CN116173905B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a pyrolysis biochar / geopolymer composite material, wherein wheat straw is crushed and mixed evenly with fly ash, potassium hydroxide solution is added and placed in a stirring device for mixing, and a biochar / geopolymer composite material precursor is obtained after curing, and the precursor is placed in a nitrogen atmosphere for pyrolysis, and then washed, dried, and granulated to obtain a pyrolysis biochar / geopolymer composite material. The amount of straw powder, potassium hydroxide, and distilled water is 5% to 35%, 65% to 85%, and 30% to 90% of the fly ash mass, respectively, the pyrolysis temperature is 300° C. to 700° C., and the pyrolysis time is 2 hours; the obtained pyrolysis biochar / geopolymer composite material is used for the adsorption and removal of lead ions in water and the in-situ passivation of soil lead, and both show good effects. The method has the advantages of simple process, low cost, resource utilization of solid waste, and environmental friendliness, and the obtained composite material has broad application prospects in the treatment of heavy metal-contaminated water and soil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of solid waste resource utilization and heavy metal contaminated water and soil treatment, and specifically relates to the preparation of a pyrolytic biochar / geopolymer composite material, and the application of the prepared pyrolytic biochar / geopolymer composite material for adsorbing lead ions in water and in-situ passivating lead in soil. Background Art

[0002] Since the reform and opening up, my country's industrialization process has accelerated, resulting in a large amount of heavy metal lead polluting wastewater and land. Lead ions can cause damage to the liver and kidneys or lead to neurological disorders by interacting with the sulfhydryl groups of proteins in organisms [1]. Excessive lead can cause a variety of toxic symptoms in plants. [2] , such as stunted development, chlorosis and blackening of roots. Lead can inhibit plant photosynthesis, destroy mineral nutrition and water balance, change hormone status, and affect cell membrane structure and permeability. For this reason, my country attaches great importance to the management of lead-contaminated water and soil, and has successively promulgated the "Action Plan for Water Pollution Prevention and Control" and the "Action Plan for Soil Pollution Prevention and Control". Therefore, it is imperative to carry out the management of lead-contaminated water and soil. Among the many methods for the treatment of lead-contaminated water, the adsorption method has been widely used due to its advantages such as simple operation and low cost. Materials with lead ion adsorption characteristics can usually passivate lead pollutants in the soil. Therefore, adsorption materials have become a hot topic in the field of lead-contaminated water and soil management. At present, researchers at home and abroad have developed a variety of lead adsorption materials including clay minerals, organic polymers, biochar, etc., and have achieved fruitful research results [2-5]. Among them, biochar is a porous carbon material generated by pyrolysis of biomass raw materials under anaerobic or anoxic conditions. It has the advantages of a wide range of raw material sources, can effectively reduce greenhouse gas emissions, and can improve soil fertility and crop yields [6-8]. Therefore, it has received widespread attention in the adsorption and removal of Pb(II) in water and in situ passivation of soil lead. However, the biochar obtained by direct pyrolysis has fewer pores and surface active groups, and its adsorption and passivation properties are not ideal, so it needs certain modification. Ding et al. [9] further modified hickory biochar with NaOH. After modification, the specific surface area, cation exchange capacity and thermal stability of biochar were significantly improved. The modified biochar showed better heavy metal adsorption capacity (2.6 to 5.8 times) than the original biochar; Deng et al.

[10] studied chitosan and pyromellitic anhydride modified biochar. The new modified biochar has more surface functional groups.

[0003] Geopolymers are a type of amorphous to semi-crystalline inorganic polymer aluminosilicates produced by dissolution and polycondensation of siliceous and aluminous raw materials such as calcined clay minerals or fly ash under the action of a strong alkaline activator. 4- Tetrahedron and [AlO4] 5-The tetrahedrons are connected by covalent bonds formed by shared vertex oxygen atoms to form a zeolite-like porous anionic framework structure, which means that it has ion exchange and adsorption properties similar to zeolites. Pang Yu

[11] reported the effect of circulating fluidized bed fly ash-based polymers on Pb 2+ The results showed that with the increase of the dosage, the removal rate of lead ions by geopolymer increased first and then leveled off. When the dosage was 0.5 g / L, the removal rate of lead ions was 92.01%. When the pH value was 5, the removal rate of lead ions by geopolymer was 92.01%. 2+ The maximum adsorption capacity is 93.72 mg / g. The above research results also indicate that geopolymers have potential application prospects in soil heavy metal passivation and remediation.

[0004] The applicant systematically reviewed a large number of domestic and foreign patents and literature and found no relevant reports on biochar / geopolymer composites and their adsorption and removal of lead in water and in-situ passivation of soil lead.

[0005] The following are the references given by the inventor:

[0006] 【1】Needleman H. Lead poisoning[J]. Annu.Rev.Med., 2004, 55: 209-222.

[0007] [2] He Jiakang, Wang Baoming, Wu Bingyu, et al. Research progress on the adsorption of Pb(Ⅱ) by attapulgite[J]. Industrial Water Treatment, 2020, 40(08): 11-16.

[0008] 【3】Wang Luxing, Zhou Xintao, Luo Zhongqiu, et al. Adsorption of heavy metal Pb in wastewater by agricultural and forestry wastes 2+ Research progress on properties and mechanisms of [J]. Materials Review, 2020, 34(17): 17115-17123.

[0009] 【4】Miao Jiabing, Guo Zhaohua, Wang Yongwang, et al. Adsorption of Pb in wastewater by polyacrylamide composites. 2+ Research progress[J]. Industrial Water Treatment, 2018, 38(06): 6-11.

[0010] 【5】Zhang Xiaoying, Chen Su, Liu Ying, et al. Research progress on charcoal aging and its effect on heavy metal adsorption and fixation [J / OL]. Journal of Agricultural Resources and Environment: 1-15 [2023-03-08].

[0011] 【6】Colantoni A,Evic N,Lord R,et al.Characterization of biocharsproduced from pyrolysis of pelletized agricultural residues[J].Renew.Sust.Energ.Rev.,2016,64:187-194。

[0012] 【7】Mohanty S K,Cantrell K B,Nelson K L,et al.Efficacy of biochar toremove Escherichia coli from stormwater under steady and intermittent flow[J].Water res.,2014,61:288-296。

[0013] 【8】Fang J,Zhan L,Ok Y S,et al.Minireview of potential applications ofhydrochar derived from hydrothermal carbonization of biomass[J].J.Ind.Eng.Chem.,2018,57:15-21。

[0014] 【9】Ding Z,Xin H,Wan Y,et al.Removal of lead,copper,cadmium,zinc,andnickel from aqueous solutions by alkali-modified biochar:Batch and columntests[J].J.Ind.Eng.Chem.,2016,33:239-245。

[0015]

[10] Deng J,Liu Y,Liu S,et al.Competitive adsorption of Pb(II),Cd(II)and Cu(II)onto chitosan-pyromellitic dianhydride modified biochar[J].J.Colloid Interface Sci.,2017,506:355-364。

[0016]

[11] Pang Yu. Preparation of fly ash-based polymer in circulating fluidized bed and its adsorption of Pb 2+ Research on performance[D]. Shanxi University, 2021.

[0017]

[12] Huang Yi, Wu Di, Yao Xia, Li Xuan, Deng Zixuan, Tan Rui. In situ synthesis of zeolite by (Na, K)-based geopolymer and its passivation of soil Cu 2+ 、Zn 2+ Research on pollution performance[J]. Journal of Hunan City University (Natural Science Edition), 2022, 31(03): 74-78. Summary of the invention

[0018] The purpose of the present invention is to provide a method for preparing a pyrolysis biochar / geopolymer composite material, and to apply the prepared composite material to adsorb and remove lead ions in water or in-situ passivation of soil lead.

[0019] In order to achieve the above tasks, the present invention adopts the following technical solutions:

[0020] A method for preparing a pyrolytic biochar / geopolymer composite material, characterized in that fly ash, straw powder and an aqueous solution of potassium hydroxide are placed in a stirring device for mixing to form a uniformly mixed slurry, and a biochar / geopolymer precursor is obtained through curing, and then pyrolyzed in a nitrogen atmosphere, washed and dried to obtain a pyrolytic biochar / geopolymer composite material; wherein: the amount of straw powder, potassium hydroxide and water accounts for 5% to 35%, 65% to 85% and 30% to 90% of the fly ash mass, respectively, the pyrolysis temperature is 300° C. to 700° C., and the pyrolysis time is 2 hours.

[0021] The specific steps include:

[0022] (1) Weigh fly ash according to the formula and place it in an automatic mixer with a set program;

[0023] (2) Weigh the straw according to the formula amount, crush it with a crusher, pass it through a 100-mesh sieve, and add it to the automatic mixer described in step (1) to fully dry mix;

[0024] (3) Weighing solid potassium hydroxide according to the formula amount;

[0025] (4) Weighing water according to the formula amount, dissolving solid potassium hydroxide in the water;

[0026] (5) After the potassium hydroxide solution is cooled to room temperature, it is added to the mixer described in step (2) and stirred for 10 minutes to obtain a uniform slurry;

[0027] (6) The slurry was placed in a plastic film sealed bag, placed in a constant temperature box at 80° C. for 8 h, then taken out and cured at room temperature for 48 h to obtain a biochar / geopolymer composite material precursor;

[0028] (7) placing the precursor of step (6) into a tubular furnace and pyrolyzing it under a nitrogen atmosphere, setting the heating rate to 10°C / min, the pyrolysis temperature to 300°C to 700°C, and the pyrolysis time to 2h to obtain a product;

[0029] (8) The product obtained in step (7) was rinsed alternately with distilled water and anhydrous ethanol, filtered until the filtrate was neutral, placed in a constant temperature drying oven at 105° C. for 12 h, and granulated to obtain particles with a particle size of 0.250 mm to 0.600 mm, thereby obtaining a pyrolysis biochar / geopolymer composite material.

[0030] The applicant's experiments show that the prepared pyrolysis biochar / geopolymer composite material can be used for adsorbing lead ions in water and in-situ passivation of lead in soil.

[0031] The specific application includes the following steps:

[0032] (1) A certain amount of pyrolyzed biochar / geopolymer composite material is placed in a container with a certain volume and a concentration of C o The Pb(NO3)2 solution was shaken in a water bath constant temperature shaker for 24 hours, centrifuged, and the Pb in the supernatant was detected by ICP. 2+ concentration, and calculated the removal rate and adsorption amount of lead ions in water by pyrolysis biochar / geopolymer composites;

[0033] (2) A certain amount of pyrolytic biochar / geopolymer composite particles was added to simulated lead-contaminated soil. After mixing evenly, distilled water was added to maintain 50% of the field water holding capacity. The soil was taken out after 7 days, air-dried, and the effective lead in the soil was extracted with diethyltriaminepentaacetic acid. The lead ion concentration in the extract was detected by ICP, and the passivation rate of soil lead by the pyrolytic biochar / geopolymer composite was calculated.

[0034] The innovation of the present invention lies in the ingenious use of the strong alkaline environment of geopolymer to perform alkali modification on biochar, and at the same time, the high temperature environment required for preparing biochar is used to promote further polycondensation of geopolymer to obtain more porous structures, thereby obtaining a pyrolytic biochar / geopolymer composite material for adsorbing and removing lead ions in water or in situ passivating soil lead. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is the process flow of preparation and application of pyrolysis biochar / geopolymer composite materials;

[0036] Figure 2 is a scanning electron microscope photograph of the pyrolysis biochar / geopolymer composite material prepared in Preparation Example 3;

[0037] Figure 3It is the adsorption removal rate and adsorption amount of lead ions in water by the pyrolysis biochar / geopolymer composite material in Example 1-3.

[0038] Figure 4 It is the passivation rate of soil lead by the pyrolyzed biochar / geopolymer composite material in Application Examples 1-3.

[0039] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. DETAILED DESCRIPTION

[0040] In the following examples, the applicant provides examples of the preparation of pyrolysis biochar / geopolymer composite materials and their application in the adsorption and removal of lead ions in water or in-situ passivation of soil lead.

[0041] It should be noted that the following embodiments are only for the inventor to better explain the present invention, and the present invention is not limited to these embodiments.

[0042] The main raw materials used in the preparation of pyrolytic biochar / geopolymer composite materials are industrial solid waste fly ash, agricultural solid waste wheat straw powder and potassium hydroxide, among which the dosage of straw powder, potassium hydroxide and water is based on the mass of fly ash; the dosage of straw powder is 5% to 35% of the mass of fly ash, the dosage of potassium hydroxide is 65% to 85% of the mass of fly ash, and the dosage of water is 30% to 90% of the mass of fly ash. The pyrolysis atmosphere is N2, the pyrolysis temperature is 300℃ to 700℃, and the pyrolysis time is 2h.

[0043] The specific preparation is as follows:

[0044] (1) Wheat straw was collected from local farmland, dried, crushed, and passed through a 100-mesh sieve for later use.

[0045] (2) Fly ash: Grade I fly ash from the Sanmenxia Power Plant in Henan Province was used. The fly ash was dried in an oven at 105°C for 10 h. The main oxide composition (mass percentage) of the fly ash is shown in Table 1.

[0046] Table 1: Oxide composition of fly ash (wt%)

[0047] Oxide <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO <![CDATA[Na2O]]> MgO <![CDATA[K2O]]> <![CDATA[SO3]]> <![CDATA[TiO2]]> Loss Impurities wt% 52.77 29.14 5.81 4.49 0.48 0.98 2.53 0.81 1.44 0.84 margin

[0048] (3) Potassium hydroxide was purchased from Sinopharm Chemical Reagent Co., Ltd., analytical grade reagent.

[0049] Preparation Example 1:

[0050] Accurately weigh 200g of fly ash raw material and use it as the measurement basis (100%). Using the external blending method, the mass of straw powder is 20% of the mass of fly ash, the amount of potassium hydroxide is 75% of the mass of fly ash, and the mass of water is 50% of the mass of fly ash.

[0051] Before preparation, potassium hydroxide solution is prepared with water and potassium hydroxide for later use.

[0052] Place fly ash and straw powder in an automatic mixer, then pour in the prepared potassium hydroxide solution, mix and stir evenly, and form a uniform slurry after reaction; then put the slurry into a plastic film sealed bag, seal it, place it in a constant temperature box at 80°C for 8 hours, then take it out, and cure it at room temperature for 48 hours to obtain a biochar / geopolymer composite material precursor. Then weigh 30g of the above precursor and place it in a tubular furnace, set the pyrolysis atmosphere to N2, the pyrolysis temperature to 300°C, and the pyrolysis time to 2 hours. After the pyrolysis is completed, take it out, rinse it with distilled water and anhydrous ethanol alternately, and filter it until the filtrate is neutral. After drying at 105°C for 12 hours, crush and granulate it to obtain particles with a particle size of 0.25mm to 0.60mm, which is recorded as 30PBCGC-300.

[0053] Preparation Example 2:

[0054] Accurately weigh 200g of fly ash raw material and use it as the measurement basis (100%). Using the external admixture method, the mass of straw powder is 20% of the mass of fly ash, the amount of solid potassium hydroxide is 75% of the mass of fly ash, and the mass of water is 50% of the mass of fly ash.

[0055] Before preparation, potassium hydroxide solution is prepared with water and potassium hydroxide for later use.

[0056] Place fly ash and straw powder in an automatic mixer, then pour in the prepared potassium hydroxide solution, mix and stir evenly, and form a uniform slurry after reaction; then put the slurry into a plastic film sealed bag, seal it, place it in a constant temperature box at 80°C for 8 hours, then take it out, and cure it at room temperature for 48 hours to obtain a biochar / geopolymer composite material precursor. Then weigh 30g of the above precursor and place it in a tubular furnace, set the pyrolysis atmosphere to N2, the pyrolysis temperature to 500°C, and the pyrolysis time to 2 hours. After the pyrolysis is completed, take it out, rinse and filter it alternately with distilled water and anhydrous ethanol until the filtrate is neutral, dry it at 105°C for 12 hours, and then crush and granulate it to obtain particles with a particle size of 0.25mm to 0.60mm, recorded as 30PBCGC-500.

[0057] Preparation Example 3:

[0058] Accurately weigh 200g of fly ash raw material and use it as the measurement basis (100%). Using the external admixture method, the mass of straw powder is 20% of the mass of fly ash, the amount of solid potassium hydroxide is 75% of the mass of fly ash, and the mass of water is 50% of the mass of fly ash.

[0059] Before preparation, potassium hydroxide solution is prepared with water and potassium hydroxide for later use.

[0060] Place fly ash and straw powder in an automatic mixer, then pour in the prepared potassium hydroxide solution, mix and stir evenly, and form a uniform slurry through reaction; then put the slurry into a plastic film sealed bag, seal it, place it in a constant temperature box and cure it at 80°C for 8 hours, then take it out, and cure it at room temperature for 48 hours to obtain a biochar / geopolymer composite material precursor. Then weigh 30g of the above precursor and place it in a tubular furnace. The pyrolysis atmosphere is set to N2, the pyrolysis temperature is 700°C, and the pyrolysis time is 2h. After the pyrolysis is completed, take it out, rinse it alternately with distilled water and anhydrous ethanol, and filter it until the filtrate is neutral. After drying at 105°C for 12 hours, crush and granulate it to obtain particles with a particle size of 0.25mm to 0.60mm, which is denoted as 30PBCGC-700. Its scanning electron microscope photo is shown as follows Figure 2 As shown in Figure 2, it can be seen that the long columnar biochar particles are embedded in the geopolymer matrix, forming abundant pores, which provide material transmission channels for lead ion adsorption / passivation.

[0061] The inventors have proved through experiments that the pyrolysis biochar / geopolymer composite material prepared in the embodiment can efficiently adsorb and remove Pb in water. 2+ And in situ passivation of Pb(II) in soil, specifically according to the following steps:

[0062] (1) A certain amount of pyrolyzed biochar / geopolymer composite material is placed in a container with a certain volume and a concentration of C o The Pb(NO3)2 solution was shaken in a water bath constant temperature shaker for 24 hours, centrifuged, and the supernatant was taken and the Pb in it was detected by ICP. 2 + The concentration is C t , and calculated the removal rate and adsorption amount of lead ions in water by pyrolysis biochar / geopolymer composites;

[0063] (2) A certain amount of pyrolytic biochar / geopolymer composite particles was added to simulated lead-contaminated soil. After mixing evenly, distilled water was added to maintain 50% of the field water holding capacity. The soil was taken out after 7 days, air-dried, and the effective lead in the soil was extracted with diethyltriaminepentaacetic acid. The lead ion concentration in the extract was detected by ICP, and the passivation rate of soil lead by the pyrolytic biochar / geopolymer composite was calculated.

[0064] Application experiment example 1:

[0065] (1) Adsorption: 0.05 g of the pyrolysis biochar / geopolymer composite material sample (30PBCGC-300) prepared in Preparation Example 1 was accurately weighed and added to 100 mL of a 100 mg / L lead nitrate solution. The mixture was shaken in a water bath constant temperature shaker for 24 h and then centrifuged. The Pb content in the supernatant was detected by ICP. 2+concentration, and calculated that its removal rate and adsorption capacity for lead ions were 68.12% and 136.14 mg / g respectively;

[0066] (2) In-situ passivation: 3.6 g of the pyrolysis biochar / geopolymer composite material sample (30PBCGC-300) prepared in Preparation Example 1 was accurately weighed, 40 g of simulated lead-contaminated soil was added, and distilled water was added to maintain 50% of the field water holding capacity after mixing. After 7 days, the sample was taken out and air-dried. The effective lead in the soil was then leached with diethyltriaminepentaacetic acid. The lead ion concentration in the extract was detected by ICP, and the passivation rate for soil lead was calculated to be 32.68%.

[0067] Application experiment example 2:

[0068] (1) Adsorption: 0.05 g of the pyrolysis biochar / geopolymer composite material sample (30PBCGC-300) prepared in Preparation Example 2 was accurately weighed and added to 100 mL of a 100 mg / L lead nitrate solution. The mixture was shaken in a water bath constant temperature shaker for 24 h and then centrifuged. The Pb content in the supernatant was detected by ICP. 2+ concentration, and calculated that its removal rate and adsorption capacity for lead ions were 77.46% and 154.92 mg / g respectively;

[0069] (2) In situ passivation: 3.6 g of the pyrolysis biochar / geopolymer composite material sample (30PBCGC-500) prepared in Preparation Example 2 was accurately weighed, 40 g of simulated lead-contaminated soil was added, and distilled water was added to maintain 50% of the field water holding capacity after mixing. After 7 days, the sample was taken out and air-dried. The effective lead in the soil was then leached with diethyltriaminepentaacetic acid. The lead ion concentration in the extract was detected by ICP, and the passivation rate for soil lead was calculated to be 52.15%.

[0070] Application experiment example 3:

[0071] (1) Adsorption: 0.05 g of the pyrolysis biochar / geopolymer composite material sample (30PBCGC-700) prepared in Preparation Example 3 was accurately weighed and added to 100 mL of a 100 mg / L lead nitrate solution. The mixture was shaken in a water bath constant temperature shaker for 24 h and then centrifuged. The Pb content in the supernatant was detected by ICP. 2+ concentration, and calculated that its removal rate and adsorption capacity for lead ions were 99.99% and 199.98 mg / g respectively;

[0072] (2) In-situ passivation: 3.6 g of the pyrolysis biochar / geopolymer composite material sample (30PBCGC-700) prepared in Preparation Example 3 was accurately weighed, 40 g of simulated lead-contaminated soil was added, and distilled water was added to maintain 50% of the field water holding capacity after mixing. After 7 days, it was taken out, air-dried, and then the effective lead in the soil was leached with diethyltriaminepentaacetic acid. The lead ion concentration in the extract was detected by ICP, and the passivation rate of soil lead was calculated to be 76.33%. In addition, the addition of 30PBCGC-700 increased the available potassium content in the soil from 411.19 mg / kg to 1007.96 mg / kg, indicating that it can effectively increase the potassium nutrient content in the soil while passivating heavy metals.

Claims

1. Application of a pyrolyzed biochar / geopolymer composite material for adsorbing lead ions in water and in-situ passivation of lead in soil, characterized in that: The specific implementation is as follows: (1) 0.05 g of pyrolyzed biochar / geopolymer composite material was placed in 100 mL of 100 mg / L Pb(NO3)2 solution, shaken in a water bath constant temperature shaker for 24 h, centrifuged, and the Pb in the supernatant was detected by ICP. 2+ concentration, and calculate the removal rate and adsorption amount of lead ions in water by pyrolyzed biochar / geopolymer composites; or, (2) 3.6 g of pyrolytic biochar / geopolymer composite particles were added to 40 g of simulated lead-contaminated soil, mixed evenly, and then distilled water was added to maintain 50% of the field water capacity. After 7 days, the soil was taken out and air-dried. The effective lead in the soil was then leached with diethyltriaminepentaacetic acid. The lead ion concentration in the extract was detected by ICP, and the passivation rate of the pyrolytic biochar / geopolymer composite material on soil lead was calculated. The method for preparing the pyrolysis biochar / geopolymer composite material specifically comprises the following steps: (1) Weigh fly ash according to the formula and place it in an automatic mixer with a set program; (2) Weigh the straw according to the formula amount, dry it, crush it with a grinder, pass it through a 100-mesh sieve, add it to the automatic mixer described in step (1), and dry-mix it evenly; (3) Weigh solid potassium hydroxide according to the formula; (4) Weigh water according to the formula amount and dissolve solid potassium hydroxide in the water; (5) After the potassium hydroxide solution is cooled to room temperature, it is added to the mixer described in step (2) and stirred for 10 minutes to obtain a uniform slurry; (6) The slurry was placed in a plastic film sealed bag, placed in a constant temperature box at 80°C for 8 hours, and then taken out and cured at room temperature for 48 hours to obtain a biochar / geopolymer composite material precursor; (7) placing the precursor of step (6) into a tubular furnace and pyrolyzing it under a nitrogen atmosphere, setting the heating rate to 10°C / min, the pyrolysis temperature to 300°C to 700°C, and the pyrolysis time to 2h to obtain a product; (8) The product obtained in step (7) was rinsed alternately with distilled water and anhydrous ethanol, filtered until the filtrate was neutral, placed in a constant temperature drying oven at 105° C. for 12 h, and granulated to obtain particles with a particle size of 0.250 mm to 0.600 mm, thereby obtaining a pyrolysis biochar / geopolymer composite material; Among them: the amount of straw powder, potassium hydroxide and water accounts for 5% to 35%, 65% to 85% and 30% to 90% of the fly ash mass respectively; The oxide mass percentages of the fly ash are as follows: SiO2: 52.77%, Al2O3: 29.14%, Fe2O3: 5.81%, CaO: 4.49%, Na2O: 0.48%, MgO: 0.98%, K2O: 2.53%, SO3: 0.81%, TiO2: 1.44%, Loss: 0.84%, the balance is unavoidable impurities.