A flux-cored filling wire and process for double-wire arc additive manufacturing of high entropy alloys

Through the dual-core filled wire and double-wire arc additive manufacturing process, combined with the three-dimensional motion platform and wire feeding mechanism, the problems of complex wire feeding structure and large heat input in high-entropy alloy arc additive manufacturing are solved, achieving high efficiency and low Cost high entropy alloy manufacturing ensures high performance and composition uniformity of the material.

CN116175000BActive Publication Date: 2024-11-19SHANDONG SHISHANG WELDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310286637.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-11-19
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

In the existing high-entropy alloy arc additive manufacturing technology, the double wire feeding structure is complex, the wire feeding ability is poor, and the double-arc heat input leads to roughening of the parts and reducing the performance, making it difficult to achieve high efficiency, high quality and low cost. High entropy alloy manufacturing.

Method used

Using double flux-core filled wire and double wire arc additive manufacturing technology, the combination of 304 stainless steel and nickel-based 625 flux-core welding wire is used to achieve efficient welding and wire feeding, controlling welding current and protecting gas Flow rate ensures component regulation and tissue optimization of high-entropy alloys.

Benefits of technology

It realizes high-efficiency, high-quality and low-cost high-entropy alloy manufacturing, uniform weld composition, excellent material performance, low cost, suitable for rapid printing of large parts, and simple and controllable technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116175000B_ABST
    Figure CN116175000B_ABST
Patent Text Reader

Abstract

A flux core filling wire and a process method for double-wire arc additive manufacturing of high entropy alloys, relating to the field of additive manufacturing. The outer skin of the flux core filling wire 1 is 304 stainless steel outer skin, and the mass percentage of each element of the core powder is: the mass percentage of metal cobalt powder is 40% to 80%, and the mass percentage of metal aluminum powder is 20% to 60%. The filling rate is 40wt.% to 50wt.%; the outer skin of the flux core filling wire 2 is nickel-based 625 outer skin, and the mass percentage of each element of the core powder is: the mass percentage of metal copper powder is 0 to 100%, and the mass percentage of metal manganese powder is 0 to 100%; the filling rate is 20wt.% to 30wt.%. The control current range is 150A to 200A. The wire feeding speed is 1.1m / min to 2.5m / min. Ensure that the alloy phase is composed of face-centered cubic and body-centered cubic, effectively inhibit the generation of intermetallic compounds, and enhance the comprehensive performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of additive manufacturing, and in particular to a flux-cored filling wire and a process method for double-wire arc additive manufacturing of high-entropy alloys. Background Art

[0002] High entropy alloys, also known as multi-principal alloys, are generally composed of five or more equimolar or nearly equimolar elements, and the molar amount of each element is between 5% and 35%. Compared with traditional alloys, high entropy alloys have high strength, high hardness, good high temperature resistance and corrosion resistance, and have broad application prospects in aerospace, nuclear industry, ships and other fields.

[0003] Arc additive manufacturing is an advanced manufacturing technology developed in recent years and an important branch of additive manufacturing technology. It is based on the discrete-deposition principle, uses arc as the heat source to melt wire, and directly prepares solid parts by layer-by-layer deposition. It has the advantages of high efficiency, high flexibility and low cost that are difficult to match with traditional manufacturing technology, and provides a new path with important potential for efficient, high-quality and low-cost manufacturing of high-entropy alloy parts.

[0004] Through the search of existing high-entropy alloy arc additive manufacturing technology, it is found that among the high-entropy alloy filling wires and process methods for arc additive manufacturing, the patent (patent number 202210401510.4) discloses a method for preparing Al-Co-Cr-Fe-Ni high-entropy alloys for arc additive manufacturing. By designing a cable welding wire (Co-Cr-Fe-Ni) and a pure Al welding wire, a double-wire co-feeding method is used to additively manufacture Al-Co-Cr-Fe-Ni high-entropy alloys. This method can flexibly control the content of a single element Al, but the disadvantage is that the composition of the four main alloy elements Co, Cr, Fe and Ni cannot be freely controlled, and the cable wire structure is relatively complex, and the wire feeding is poor.

[0005] The patent (patent number 201810192636.9) discloses a method for additive manufacturing of high entropy alloy dual arc fuses, designs and prepares a high entropy alloy cored wire, and uses dual arcs to collaboratively melt dual wires to additively manufacture high entropy alloys. The limitations of this method are: the dual arcs used have large heat input, which can easily cause coarsening of the workpiece structure and reduced performance, and the coordinated control between the two independent power supplies is relatively complex.

[0006] Therefore, designing a filler wire and process method for arc additive manufacturing of high-entropy alloys to achieve efficient, high-quality and low-cost manufacturing of high-entropy alloys is a technical problem that needs to be urgently solved in this field. This is of great significance for promoting arc additive manufacturing technology and the engineering application of high-entropy alloys. Summary of the invention

[0007] The purpose of the present invention is to provide a flux-cored filler wire and a process method for double-wire arc additive manufacturing of high-entropy alloys. The use of double-core filler wire materials and double-wire arc additive manufacturing of high-entropy alloys can produce high-entropy alloys with high efficiency, high quality and low cost.

[0008] The technical solution of the present invention is: a flux-cored filling wire and a process method for double-wire arc additive manufacturing of high-entropy alloys, including a special flux-cored filling wire for double-wire arc additive manufacturing of high-entropy alloys and a process method for double-wire arc additive manufacturing of high-entropy alloys.

[0009] The first technical solution adopted by the present invention is to manufacture a special flux core filling wire for high entropy alloy by double-wire arc additive manufacturing, including a flux core filling wire 1 and a flux core filling wire 2. Both the flux core filling wire 1 and the flux core filling wire 2 are composed of an outer skin and a core powder.

[0010] The outer skin of the cored wire 1 is made of 304 stainless steel, and the mass percentage of each element of the core powder is as follows: the mass percentage of metal cobalt powder is 40% to 80%, and the mass percentage of metal aluminum powder is 20% to 60%.

[0011] The outer sheath of the core filling wire 2 is nickel-based 625, and the mass percentage of each element of the core powder is: the mass percentage of metal copper powder is 0-100%, and the mass percentage of metal manganese powder is 0-100%, preferably copper and manganese are not 0.

[0012] The core powder filling rate of the core-filled wire 1 is 40 wt.% to 50 wt.%, and the core powder filling rate of the core-filled wire 2 is 20 wt.% to 30 wt.%.

[0013] The particle size of the powder in the core-filled wire 1 is 400-600 meshes, and the particle size of the powder in the core-filled wire 2 is 100-200 meshes.

[0014] The second technical solution adopted by the present invention is a double-wire arc additive manufacturing process for high entropy alloys.

[0015] The described twin-wire arc additive manufacturing high-entropy alloy process method comprises a system consisting of a workbench for fixing equipment, a three-dimensional motion mechanism, a welding structure, a wire feeding structure, a motion control structure, and a shielding gas structure; the workbench is fixed on the plane where the XY axis of the three-dimensional motion mechanism is located, and the workbench includes a clamp for fixing the substrate to ensure the thermal stability of the substrate during the working process.

[0016] In the three-dimensional motion mechanism, the X-axis, Y-axis and Z-axis are perpendicular to each other. The Z-axis is connected to the welding gun of the welding structure and can control the movement of the welding gun in the Z-axis direction. The X-axis and Y-axis are fixed under the workbench and can carry the workbench to move in the XY-axis plane. The ends of the three axes are all connected to the motion control structure to receive signals from the control center.

[0017] The welding structure is composed of a welding gun, a welding machine and several connecting wires. The welding gun is fixed on the Z axis and moves with the Z axis. The welding gun is connected to the welding machine to receive a signal for heating the welding wire with an arc as a heat source. The welding machine is used to control arc starting and arc extinguishing and current, and the control current range is 150A to 200A.

[0018] The wire feeding mechanism is composed of a wire feeding tube, a wire feeding machine and a plurality of welding wires. The wire feeding tube is fixed on the Z axis and moves with the Z axis. The end thereof is 3 to 5 mm opposite to the bottom of the tungsten electrode of the welding gun. The wire feeding tube is 20 to 40 degrees with the plane where the XZ axis is located, and 15 to 30 degrees with the plane where the XY axis is located. The two wire feeding tubes correspond to the core filling wire 1 and the core filling wire 2 respectively and are symmetrically distributed relative to the plane where the XZ axis is located. The molten pool is formed by the simultaneous melting of the heating ends of the core filling wire 1 and the core filling wire 2. The wire feeding machine is used to control the wire feeding speed and wire feeding mode. The uniform wire feeding speeds of the core filling wire 1 and the core filling wire 2 are both 1.1 m / min to 2.5 m / min, and both groups of wire feeding adopt an oscillating wire feeding mode.

[0019] The motion control mechanism is composed of a programmable controller and several connecting wires. The controller is connected to the three-dimensional motion platform, the wire feeding mechanism and the welding structure. The controller can control the motion trajectory of the three-dimensional motion platform, the arc starting of the welding gun and the wire feeding of the wire feeding mechanism through programming. The controller sets the welding speed to 120mm / min to 180mm / min.

[0020] The shielding gas mechanism is composed of a gas tank and an injection system. The gas tank is used to store argon inert gas. The injection system is connected to the welding machine, which is then connected to the end of the welding gun. The gas flow rate can be set to 10-15L / min through a pressure gauge for local cooling and air isolation.

[0021] Also included is a method for making a high entropy alloy based on the above-mentioned equipment, wherein the welding wire includes a 304 stainless steel flux-cored welding wire and a nickel-based 625 flux-cored welding wire, and the welding gun uses an electric arc as a heat source for additive manufacturing.

[0022] As a further configuration of the above scheme, the built-in program of the wire feeding mechanism can adjust the conveying speed and wire feeding mode of each conveying component for the welding wire by setting.

[0023] As a further configuration of the above scheme, the combination composition of the high entropy alloy can be quickly adjusted by changing the core composition to change the overall composition of the combined wire or by changing the wire feeding speed between the 304 stainless steel cored welding wire and the nickel-based 625 cored welding wire.

[0024] As a further configuration of the above scheme, the substrate is a Q235 steel plate, and the arc is tungsten inert gas welding (TIG) welding.

[0025] As a further configuration of the above solution, the arc additive manufacturing comprises the following steps:

[0026] 1) Grind the surface of the substrate to remove the oxide layer and clean the surface with alcohol;

[0027] 2) After cleaning, use a clamp to fix the substrate on the workbench;

[0028] 3) The prefabricated double wires are respectively loaded into the wire feeding mechanism, and the parameters of each mechanism of the built-in program control of the equipment are set through preliminary experiments and calculations. The parameters include the running speed of the three-dimensional motion platform, the wire feeding speed, the welding current and the shielding gas flow rate;

[0029] 4) After the parameter setting is completed, adjust the front end of the welding gun tungsten electrode to 3-5 mm away from the substrate, and import the welding gun path program into the three-dimensional motion platform controller, and the three-axis motion is controlled by the three-dimensional motion controller according to the preset running speed;

[0030] 5) After the setting is completed, start the protective gas system, and determine through testing that the protective gas system outputs the protective gas evenly and the output parameters meet the set parameters;

[0031] 6) After all parameters and program preparations are completed, run the program, start the equipment preheating, and start printing after the equipment preheating is completed;

[0032] 7) The welding mechanism, the double wire feeding mechanism and the shielding gas system are linked to move the welding gun horizontally on the substrate to manufacture the first layer. After one layer is manufactured, the welding mechanism and the wire feeding mechanism are removed, and the angle grinding mechanism is started to grind the workpiece to remove the oxide layer;

[0033] 8) After polishing is completed, the second layer is manufactured again and the cycle continues;

[0034] 9) After waiting for the printed part to cool down, remove the printed part to obtain a high entropy alloy part.

[0035] In the process of preparing the powder and selecting the outer skin of the present invention, the reasons for limiting the composition and content of each chemical element are described as follows:

[0036] Aluminum improves the strength and hardness of high-entropy alloys through solid solution strengthening and improves the bearing capacity of the matrix. The increase in aluminum content can increase the content of body-centered cubic phase and reduce the face-centered cubic phase in the high-entropy alloy. Controlling the aluminum content can make the high-entropy alloy in a specific dual-phase structure, thus having higher strength and maximum elongation at fracture, and the best comprehensive mechanical properties.

[0037] Nickel can be infinitely dissolved in iron and can also be miscible with aluminum, cobalt, chromium, etc. It can improve the compatibility of the weld and the base material, inhibit the formation of intermetallic compounds, and improve the comprehensive performance of the high-entropy alloy.

[0038] Copper has poor solubility with most elements, so copper usually concentrates between dendrites, which reduces the strength and hardness of high-entropy alloys and increases plasticity and toughness.

[0039] Beneficial effects of high entropy alloy production equipment and heterogeneous double flux-cored welding wire:

[0040] (1) Compared with other welding wires, the composition of the flux-cored wire of the present invention is more flexible, the welding wire production cycle is short, and the manufacturing difficulty and cost are low.

[0041] (2) Compared with other high entropy alloy additive methods, the welding wire used in the present invention can make the content of each component of the high entropy alloy additive part roughly the same, ensure that the alloy phase is composed of face-centered cubic and body-centered cubic, effectively inhibit the generation of intermetallic compounds, and enhance the comprehensive performance of the material.

[0042] (3) Compared with other additive process methods, the present invention adopts dual-wire coordinated additive manufacturing and three-dimensional motion platform mode, and simultaneously connects the welding structure, wire feeding structure, and three-dimensional motion platform to the control center, making the operation very simple and easy, and the programming code is easy to understand. The three-axis motion control additive manufacturing is more accurate than the robot arm.

[0043] (4) The present invention makes the printing cost of high entropy alloy additive parts lower and more efficient. Some large parts and small parts that are not particularly precise can be printed quickly. The process is simple, and the double-wire composition and process can be controlled, so that the high entropy alloy additive parts have good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 A model diagram of a method for additively manufacturing a high entropy alloy by a twin-wire TIG arc in an embodiment;

[0045] Figure 2 It is a structural schematic diagram of a wire feeding structure and a welding structure in a high entropy alloy additive manufacturing device according to an embodiment of the present invention;

[0046] In the figure, 1. Wire feeder for flux-cored filler wire 1; 2. Wire feeder for flux-cored filler wire 2; 3. Conductive nozzle 1; 4. Conductive nozzle 2; 5. High-entropy alloy additive layer; 6. TIG welding power supply; 7. Workbench; 8. Welding gun. DETAILED DESCRIPTION

[0047] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0048] The following combination Figure 1 and Figure 2 And specific embodiments are provided to specifically introduce the present invention.

[0049] Embodiment 1:

[0050] This embodiment uses Q235 steel plate as the metal substrate, and uses 304 stainless steel flux-cored welding wire with a filling rate of 40%, a filling mass fraction of 25% aluminum powder and 75% cobalt powder as the flux-cored filling wire 1. A nickel-based 625 flux-cored welding wire with a filling rate of 20%, a filling mass fraction of 40% copper powder and 60% manganese powder is used as the flux-cored filling wire 2. Double-wire TIG welding is used for additive manufacturing, and the steps are as follows:

[0051] 1) Grind the surface of the substrate to remove the oxide layer and clean the surface with alcohol;

[0052] 2) After the surface is cleaned, use a clamp to fix the substrate on the workbench;

[0053] 3) Load the two welding wires into the conveying assembly of the wire feeding mechanism respectively, set the wire feeding speed of the welding gun to 5.5m / min, set the welding current to 150A, and the shielding gas flow rate to 10L / min;

[0054] 4) Adjust the front end of the welding gun tungsten electrode to 3-5 mm away from the substrate, and import the welding gun path program into the three-dimensional motion platform controller, and the three-axis motion is controlled by the three-dimensional motion controller according to the preset running speed;

[0055] 5) Run the program and start printing;

[0056] 6) Between each printing layer, adjust the wire feeding angle and speed of the two welding wires by observing the weld formation, and use an angle grinder to grind the workpiece surface to remove the oxide layer;

[0057] 7) After waiting for the printed part to cool down, remove the printed part to obtain a high entropy alloy material part.

[0058] Table of the main element contents of weld metal measured after welding (atomic percentage\at%)

[0059] element Fe Ni Cr Mo Mn Cu Al Co content 22.46% 25.76% 15.08% 2.1% 4.69% 5.29% 10.38% 14.25%

[0060] According to the entropy formula Enthalpy formula Atomic radius difference formula Average valence electron concentration formula The alloy entropy is calculated to be 1.86R = 15.49 J·mol ~1 K ~1 (1.86R>1.5R), mixing enthalpy is ~6.89KJ·mol ~1 (~15KJ·mol ~1<~6.89KJ·mol ~1 <5 kJ·mol ~1 ), the atomic radius difference is 4.42% (4.42% < 6%), and the average valence electron concentration is 7.91 (6.5 < 7.91 < 8). After theoretical calculation and actual testing, it is known that the additive parts have reached high entropy. After grinding and cutting the additive parts, the hardness of the samples was tested according to the GBT_7997-2014 cemented carbide Vickers hardness test method, and the average hardness of the samples was 270HV; after grinding and cutting the additive parts, the mechanical properties of the samples were tested according to the GB / T2651-2008 welded joint tensile test method, and the tensile strength was 823MPa.

[0061] Embodiment 2:

[0062] This embodiment uses Q235 steel plate as the metal substrate, and uses 304 stainless steel flux-cored welding wire with a filling rate of 40%, a filling mass fraction of 30% aluminum powder and 70% cobalt powder as the flux-cored filling wire 1. A nickel-based 625 flux-cored welding wire with a filling rate of 20%, a filling mass fraction of 45% copper powder and 55% manganese powder is used as the flux-cored filling wire 2. Double-wire TIG welding is used for additive manufacturing, and the steps are as follows:

[0063] 1) Grind the surface of the substrate to remove the oxide layer and clean the surface with alcohol;

[0064] 2) After the surface is cleaned, use a clamp to fix the substrate on the workbench;

[0065] 3) Load the two welding wires into the conveying assembly of the wire feeding mechanism respectively, set the wire feeding speed of the welding gun to 5.5m / min, set the welding current to 150A, and the shielding gas flow rate to 10L / min;

[0066] 4) Adjust the front end of the welding gun tungsten electrode to 3-5 mm away from the substrate, and import the welding gun path program into the three-dimensional motion platform controller, and the three-axis motion is controlled by the three-dimensional motion controller according to the preset running speed;

[0067] 5) Run the program and start printing;

[0068] 6) Between each printing layer, adjust the wire feeding angle and speed of the two welding wires by observing the weld formation, and use an angle grinder to grind the workpiece surface to remove the oxide layer;

[0069] 7) After waiting for the printed part to cool down, remove the printed part to obtain a high entropy alloy material part.

[0070] Table of the main element contents of weld metal measured after welding (atomic percentage\at%)

[0071] element Fe Ni Cr Mo Mn Cu Al Co content 22.19% 25.45% 14.9% 2.08% 5.14% 4.79% 12.3% 13.15%

[0072] According to the entropy formula Enthalpy formula Atomic radius difference formula Average valence electron concentration formula The alloy entropy is calculated to be 1.87R = 15.55 J·mol ~1 K ~1 (1.87R>1.5R), mixing enthalpy is ~7.90KJ·mol ~1 (~15KJ·mol ~1 <~7.90KJ·mol ~1 <5 kJ·mol ~1 ), the atomic radius difference is 4.67% (4.67% < 6%), and the average valence electron concentration is 7.78 (6.5 < 7.78 < 8). After theoretical calculation and actual testing, it is known that the additive parts have reached high entropy. After grinding and cutting the additive parts, the hardness test of the samples was carried out according to the GBT_7997-2014 cemented carbide Vickers hardness test method, and the average hardness of the samples was 280HV; after grinding and cutting the additive parts, the mechanical properties of the samples were tested according to the GB / T2651-2008 welded joint tensile test method, and the tensile strength was 850MPa.

[0073] Embodiment 3:

[0074] This embodiment uses Q235 steel plate as the metal substrate, and uses 304 stainless steel flux-cored welding wire with a filling rate of 40%, a filling mass fraction of 35% aluminum powder and 65% cobalt powder as the flux-cored filling wire 1. A nickel-based 625 flux-cored welding wire with a filling rate of 20%, a filling mass fraction of 50% copper powder and 50% manganese powder is used as the flux-cored filling wire 2. Double-wire TIG welding is used for additive manufacturing, and the steps are as follows:

[0075] 1) Grind the surface of the substrate to remove the oxide layer and clean the surface with alcohol;

[0076] 2) After the surface is cleaned, use a clamp to fix the substrate on the workbench;

[0077] 3) Load the two welding wires into the conveying assembly of the wire feeding mechanism respectively, set the wire feeding speed of the welding gun to 5.5m / min, set the welding current to 150A, and the shielding gas flow rate to 10L / min;

[0078] 4) Adjust the front end of the welding gun tungsten electrode to 3-5 mm away from the substrate, and import the welding gun path program into the three-dimensional motion platform controller, and the three-axis motion is controlled by the three-dimensional motion controller according to the preset running speed;

[0079] 5) Run the program and start printing;

[0080] 6) Between each printing layer, adjust the wire feeding angle and speed of the two welding wires by observing the weld formation, and use an angle grinder to grind the workpiece surface to remove the oxide layer;

[0081] 7) After waiting for the printed part to cool down, remove the printed part to obtain a high entropy alloy material part.

[0082] Table of the main element contents of weld metal measured after welding (atomic percentage\at%)

[0083] element Fe Ni Cr Mo Mn Cu Al Co content 21.94% 25.16% 14.73% 2.05% 5.57% 4.3% 14.19% 12.06%

[0084] According to the entropy formula Enthalpy formula Atomic radius difference formula Average valence electron concentration formula The alloy entropy is calculated to be 1.87R = 15.55 J·mol ~1 K ~1 (1.87R>1.5R), mixing enthalpy is ~8.86KJ·mol ~1 (~15KJ·mol ~1 <~8.86KJ·mol ~1 <5 kJ·mol ~1 ), the atomic radius difference is 4.88% (4.88% < 6%), and the average valence electron concentration is 7.65 (6.5 < 7.65 < 8). After theoretical calculation and actual testing, it is known that the additive parts have reached high entropy. After grinding and cutting the additive parts, the hardness of the samples was tested according to the GBT_7997-2014 cemented carbide Vickers hardness test method, and the average hardness of the samples was 292HV; after grinding and cutting the additive parts, the mechanical properties of the samples were tested according to the GB / T2651-2008 welded joint tensile test method, and the tensile strength was 862MPa.

[0085] Embodiment 4:

[0086] This embodiment uses Q235 steel plate as the metal substrate, and uses 304 stainless steel flux-cored welding wire with a filling rate of 40%, a filling mass fraction of 40% aluminum powder and 60% cobalt powder as the flux-cored filling wire 1. A nickel-based 625 flux-cored welding wire with a filling rate of 20%, a filling mass fraction of 55% copper powder and 45% manganese powder is used as the flux-cored filling wire 2. Double-wire TIG welding is used for additive manufacturing, and the steps are as follows:

[0087] 1) Grind the surface of the substrate to remove the oxide layer and clean the surface with alcohol;

[0088] 2) After the surface is cleaned, use a clamp to fix the substrate on the workbench;

[0089] 3) Load the two welding wires into the conveying assembly of the wire feeding mechanism respectively, set the wire feeding speed of the welding gun to 5.5m / min, set the welding current to 150A, and the shielding gas flow rate to 10L / min;

[0090] 4) Adjust the front end of the welding gun tungsten electrode to 3-5 mm away from the substrate, and import the welding gun path program into the three-dimensional motion platform controller, and the three-axis motion is controlled by the three-dimensional motion controller according to the preset running speed;

[0091] 5) Run the program and start printing;

[0092] 6) Between each printing layer, adjust the wire feeding angle and speed of the two welding wires by observing the weld formation, and use an angle grinder to grind the workpiece surface to remove the oxide layer;

[0093] 7) After waiting for the printed part to cool down, remove the printed part to obtain a high entropy alloy material part.

[0094] Table of the main element contents of weld metal measured after welding (atomic percentage\at%)

[0095] element Fe Ni Cr Mo Mn Cu Al Co content 21.68% 24.87% 14.56% 2.03% 6% 3.83% 16.03% 11.01%

[0096] According to the entropy formula Enthalpy formula Atomic radius difference formula Average valence electron concentration formula The alloy entropy is calculated to be 1.87R = 15.52 J·mol ~1 K ~1 (1.87R>1.5R), mixing enthalpy is ~9.74KJ·mol ~1 (~15KJ·mol ~1 <~9.74KJ·mol ~1 <5 kJ·mol ~1 ), the atomic radius difference is 5.07% (5.07% < 6%), and the average valence electron concentration is 7.53 (6.5 < 7.53 < 8). After theoretical calculation and actual testing, it is known that the additive parts have reached high entropy. After grinding and cutting the additive parts, the hardness of the samples was tested according to the GBT_7997-2014 cemented carbide Vickers hardness test method, and the average hardness of the samples was 305HV; after grinding and cutting the additive parts, the mechanical properties of the samples were tested according to the GB / T2651-2008 welded joint tensile test method, and the tensile strength was 885MPa.

[0097] The high entropy alloy manufacturing equipment and welding wire of the present invention are simple in design and scientific in structure. The principle is mainly aimed at the production of high entropy alloy welding wire and program-controlled production of high entropy alloy. Double flux-cored welding wire is used as raw material. The additive composition is changed by controlling the composition of the flux-cored welding wire and the parameters of the wire feeding mechanism. It can be used for the design of high entropy alloy additives. Moreover, the invention has relatively small requirements on the site and equipment. The present invention can reduce the cost of printing high entropy alloy materials and increase production efficiency. It can also print large components. The process is simple, and due to the rapid cooling effect, the material has good mechanical properties.

[0098] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0099] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A process for arc additive manufacturing of high entropy alloys using a flux-cored filler wire, characterized in that: The following steps are involved: 1) Grind the surface of the substrate to remove the oxide layer and clean the surface with alcohol; 2) After cleaning, use a clamp to fix the substrate on the workbench; 3) The prefabricated double wires are respectively loaded into the wire feeding mechanism, and the parameters of each mechanism of the built-in program control of the equipment are set through preliminary experiments and calculations. The parameters include the running speed of the three-dimensional motion platform, the wire feeding speed, the welding current and the shielding gas flow rate; wherein the welding current is 150A~200A, the wire feeding speed is 1.1m / min~2.5m / min, and the shielding gas flow rate is 10~15L / min; 4) After the parameter setting is completed, adjust the front end of the welding gun tungsten electrode to 3-5 mm away from the substrate, and import the welding gun path program into the three-dimensional motion platform controller, which controls the three-axis motion according to the preset running speed; 5) After the setting is completed, start the protective gas system, and determine through testing that the protective gas system outputs the protective gas evenly and the output parameters meet the set parameters; 6) After all parameters and program preparations are completed, run the program, start the equipment preheating, and start printing after the equipment preheating is completed; 7) The welding mechanism, wire feeding mechanism and shielding gas system are linked to move the welding gun horizontally on the substrate to manufacture the first layer. After one layer is manufactured, the welding mechanism and wire feeding mechanism are removed, and the angle grinding mechanism is started to grind the workpiece to remove the oxide layer; 8) After polishing is completed, the second layer is manufactured again and the cycle continues; 9) After the printed part is cooled, remove the printed part to obtain a high entropy alloy part; The drug core filling wire comprises a drug core filling wire 1 and a drug core filling wire 2; the drug core filling wire 1 and the drug core filling wire 2 are both composed of an outer skin and a core drug powder; The outer skin of the core filling wire 1 is made of 304 stainless steel, and the mass percentage of each element of the core powder is as follows: the mass percentage of metal cobalt powder is 40% to 80%, and the mass percentage of metal aluminum powder is 20% to 60%; The outer sheath of the core filling wire 2 is a nickel-based 625 outer sheath, and the mass percentage of each element of the core powder is: the mass percentage of metal copper powder is 55%, and the mass percentage of metal manganese powder is 45%; The core powder filling rate of the core-filled wire 1 is 40 wt.%, and the core powder filling rate of the core-filled wire 2 is 20 wt.%.

2. The process according to claim 1, characterized in that: The particle size of the powder in the core-filled wire 1 is 400-600 meshes, and the particle size of the powder in the core-filled wire 2 is 100-200 meshes.

3. The process according to claim 1, characterized in that: The adopted system consists of a workbench for fixing equipment, a three-dimensional motion platform, a welding mechanism, a wire feeding mechanism, a three-dimensional motion platform controller, and a protective gas system; the workbench is fixed on the plane where the XY axis of the three-dimensional motion platform is located, and the workbench includes a fixture for fixing the substrate to ensure the thermal stability of the substrate during the working process; The three axes of X, Y and Z in the three-dimensional motion platform are perpendicular to each other. The Z axis is connected to the welding gun of the welding mechanism and can control the welding gun to move in the Z axis direction. The X axis and Y axis are fixed under the workbench and can carry the workbench to move in the XY axis plane. The ends of the three axes are all connected to the three-dimensional motion platform controller. The welding mechanism is composed of a welding gun, a welding machine and a plurality of connecting wires; the welding gun is fixed on the Z axis and moves with the Z axis, the welding gun is connected to the welding machine for receiving a signal for heating the welding wire with an electric arc as a heat source, and the welding machine is used to control arc starting and arc extinction and current; The wire feeding mechanism is composed of a wire feeding tube, a wire feeding machine and a plurality of welding wires; the wire feeding tube is fixed on the Z axis and moves with the Z axis, and its end is 3 to 5 mm opposite to the bottom of the tungsten electrode of the welding gun, the wire feeding tube is 20 to 40 degrees with the plane where the XZ axis is located, and 15 to 30 degrees with the plane where the XY axis is located, the two wire feeding tubes correspond to the core filling wire 1 and the core filling wire 2 respectively and are symmetrically distributed relative to the plane where the XZ axis is located, and the molten pool is formed by the heating ends of the core filling wire 1 and the core filling wire 2 melting together and at the same time; the wire feeding mechanism is used to control the wire feeding speed and wire feeding mode, and both groups of wire feeding adopt the oscillating wire feeding mode; The three-dimensional motion platform controller sets the welding speed to 120mm / min~180mm / min.

4. The method according to claim 3, characterized in that The shielding gas system consists of a gas tank and an injection system. The gas tank is used to store argon inert gas. The injection system is connected to the welding machine, which is then connected to the end of the welding gun for local cooling and air isolation.

5. The method according to claim 3, characterized in that The substrate is a Q235 steel plate, and the electric arc adopts tungsten inert gas welding (TIG) welding.