A bio-based polishing particle and its preparation process
By optimizing the preparation process, using walnut shells as raw material and mixing them with polyethylene oxide (PEO), and allowing the mixture to stand and the temperature controlled, the problem of insufficient strength and wear resistance of bio-based polishing particles was solved, thus improving the particle strength and wear resistance.
Patent Information
- Application Number
- CN202211581365.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-12-09
AI Technical Summary
Existing bio-based polishing particles have low strength, are easily broken, and lack wear resistance, which affects their service life.
Walnut shells were used as a bio-based material. Wood chips were prepared by grinding, and then mixed with polyethylene oxide (PEO) and water. The mixture was left to stand and stirred at high speed. The water volume and temperature were controlled and then granulated to form bio-based polishing particles.
It improves the strength and wear resistance of bio-based polishing particles, reduces the breakage rate by 30%, enhances wear resistance and oil absorption by 10%, and reduces the formation of pores.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a bio-based polishing particle and its preparation process. Background Technology
[0002] Currently, with the increasing demand for various materials and environmental protection, bio-based materials have received significant attention. Bio-based materials are an abundant renewable resource, widely found in various plants. Due to their advantages such as renewability, short cycle time, wide availability of raw materials, low cost, good biodegradability, and non-toxicity, their applications are becoming increasingly widespread. One method involves utilizing the gelatinization of cellulose in wood chips to increase their viscosity, and then adding corundum as a wear-resistant material. After mixing wood powder, water, and corundum, the mixture is granulated to obtain polishing particles. These polishing particles exhibit good wear resistance, do not damage the workpiece surface, and have excellent oil absorption, leading to their widespread use, particularly for polishing aluminum automotive parts. However, the polishing particles prepared by this method have low strength and are prone to breakage during use, reducing their lifespan. Therefore, there is a need to develop high-strength bio-based polishing particles. Summary of the Invention
[0003] To address the shortcomings of the existing technology, the present invention provides a bio-based polishing particle with high strength and good wear resistance, as well as its preparation process.
[0004] To solve the above problems, the technical solution adopted by the present invention is as follows:
[0005] A process for preparing bio-based polishing particles, comprising the following steps:
[0006] S1. Preparation of wood powder: Grind the bio-based material to obtain bio-based powder;
[0007] S2. Pre-mixing: 40-60 parts of bio-based powder and 5-10 parts of water are fed into a mixer for mixing to achieve impregnation treatment;
[0008] S3. Secondary mixing: Let the water-based mixture from step S2 stand for 7 to 10 hours, then add 40 to 60 parts of bio-based powder, 10 to 20 parts of polyethylene oxide (PEO), and 8 to 12 parts of water, and continue to mix at high speed to obtain a mixed slurry.
[0009] S4. Granulation: The mixed slurry from step S3 is fed into a granulator for extrusion granulation to obtain bio-based polished particles.
[0010] Furthermore, the bio-based material in step S1 is walnut shell; the walnut shell is ground into wood powder and passed through a 100-mesh sieve.
[0011] Furthermore, in step S2, 50 parts of the bio-based powder and 8 parts of water are fed into a mixer for mixing.
[0012] Furthermore, in step S3, 50 parts of bio-based powder, 15 parts of polyethylene oxide (PEO), and 10 parts of water are added to the settled water mixture and stirred.
[0013] Furthermore, the stirring rate in step S2 is 200-300 r / min.
[0014] Furthermore, the granulation temperature in step S4 is 85 to 95°C.
[0015] The bio-based polishing particles prepared by the process of this invention.
[0016] The beneficial effects of this invention are as follows:
[0017] 1. The polyethylene oxide (PEO) used in this invention has strong adhesive properties, which can better bond the various component particles together, improving the strength of the prepared particles. Simultaneously, the amide bonds in the PEO component give the material higher mechanical properties and wear resistance. Furthermore, the PEO molecular chain contains urethane and ether bonds, which can form hydrogen bonds with the hydroxyl groups in the cellulose molecular chain of the bio-based powder, exhibiting a certain degree of miscibility. This enhances the intermolecular forces, increases the overall system strength, and makes it less prone to breakage. The optimized particles show a significant improvement in strength, with a 30% reduction in breakage rate; the product's wear resistance and oil absorption properties are improved by 10%.
[0018] 2. In this invention, bio-based powder is pre-mixed with a small amount of water to impregnate the bio-based powder. The mixture is then left to stand for 7-10 hours to allow the water to evaporate naturally while the bio-based powder is impregnated. Finally, 40-60 parts of bio-based powder, 10-20 parts of polyethylene oxide (PEO), and 8-12 parts of water are added and stirred together to achieve rapid mixing and granulation. This invention strictly controls the amount of water used, which greatly reduces the drawbacks of water vapor generating bubbles during the preparation process and reduces the porosity of the bio-based polishing particles, thus further improving the strength of the product.
[0019] 3. This invention controls the granulation temperature to between 85 and 95°C, thereby extending the extrusion time, resulting in more uniform components and better product performance. Detailed Implementation
[0020] The present invention will now be described in further detail.
[0021] Example 1
[0022] A process for preparing bio-based polishing particles, comprising the following steps:
[0023] S1. Preparation of wood chips: The bio-based material is ground to obtain bio-based powder; the bio-based material is walnut shell; the walnut shell is ground into wood chips and passed through a 100-mesh sieve.
[0024] S2. Pre-mixing: 40 parts of bio-based powder and 5 parts of water are fed into a mixer for mixing to achieve impregnation treatment; the mixing speed is 200 r / min.
[0025] S3. Secondary mixing: Let the water-based mixture from step S2 stand for 7 hours, then add 40 parts of bio-based powder, 10 parts of polyethylene oxide (PEO), and 8 parts of water, and continue to mix at high speed to obtain a mixed slurry.
[0026] S4. Granulation: The mixed slurry from step S3 is fed into a granulator for extrusion granulation at a granulation temperature of 85°C to obtain bio-based polished particles.
[0027] Example 2
[0028] A process for preparing bio-based polishing particles, comprising the following steps:
[0029] S1. Preparation of wood chips: The bio-based material is ground to obtain bio-based powder; the bio-based material is walnut shell; the walnut shell is ground into wood chips and passed through a 100-mesh sieve.
[0030] S2. Pre-mixing: 50 parts of bio-based powder and 8 parts of water are fed into a mixer for mixing to achieve impregnation treatment; the mixing speed is 250 r / min.
[0031] S3. Secondary mixing: Let the water mixture from step S2 stand for 8 hours, then add 50 parts of bio-based powder, 15 parts of polyethylene oxide (PEO), and 10 parts of water, and continue to mix at high speed to obtain a mixed slurry.
[0032] S4. Granulation: The mixed slurry from step S3 is fed into a granulator for extrusion granulation at a granulation temperature of 90°C to obtain bio-based polished particles.
[0033] Example 3
[0034] A process for preparing bio-based polishing particles, comprising the following steps:
[0035] S1. Preparation of wood chips: The bio-based material is ground to obtain bio-based powder; the bio-based material is walnut shell; the walnut shell is ground into wood chips and passed through a 100-mesh sieve.
[0036] S2. Pre-mixing: 60 parts of bio-based powder and 10 parts of water are fed into a mixer for mixing to achieve impregnation treatment; the mixing speed is 300 r / min.
[0037] S3. Secondary mixing: Let the water-based mixture from step S2 stand for 10 hours, then add 60 parts of bio-based powder, 20 parts of polyethylene oxide (PEO), and 12 parts of water, and continue high-speed mixing to obtain a mixed slurry.
[0038] S4. Granulation: The mixed slurry from step S3 is fed into a granulator for extrusion granulation at a granulation temperature of 95°C to obtain bio-based polished particles.
[0039] Example 4
[0040] A process for preparing bio-based polishing particles, comprising the following steps:
[0041] S1. Preparation of wood chips: The bio-based material is ground to obtain bio-based powder; the bio-based material is walnut shell; the walnut shell is ground into wood chips and passed through a 100-mesh sieve.
[0042] S2. Pre-mixing: 45 parts of bio-based powder and 8 parts of water are fed into a mixer for mixing to achieve impregnation treatment; the mixing speed is 280 r / min.
[0043] S3. Secondary mixing: Let the water mixture from step S2 stand for 9 hours, then add 45 parts of bio-based powder, 11 parts of polyethylene oxide (PEO), and 11 parts of water, and continue to mix at high speed to obtain a mixed slurry.
[0044] S4. Granulation: The mixed slurry from step S3 is fed into a granulator for extrusion granulation at a granulation temperature of 88°C to obtain bio-based polished particles.
[0045] Comparative Example 1
[0046] Walnut shells are ground into powder and sieved through a 100-mesh sieve to obtain wood dust. 40-60 parts of wood dust are mixed with 30-40 parts of water and 40-50 parts of corundum, and then added to a Changzhou Yirui GHJ-350 high-speed mixer for stirring to obtain a mixed material. The mixture is then granulated at 110℃ using a Shandong Tony TYJ551-Ⅱ pellet mill to obtain bio-based polishing particles.
[0047] Breakage rate test
[0048] Take 500g of each of the bio-based polishing particles from each embodiment, and use the bio-based polishing particles from each embodiment to polish the same automotive aluminum parts. After polishing, sieve and test the weight of the remaining particles (the percentage of the weight after polishing to the original weight), as shown in the figure below.
[0049]
[0050] The polyethylene oxide (PEO) used in this invention has strong adhesive properties, which can better bond the various component particles together and improve the strength of the prepared particles. At the same time, the amide bonds contained in the PEO component give the material higher mechanical properties and wear resistance. In addition, the PEO molecular chain contains urethane and ether bonds, which can form hydrogen bonds with the hydroxyl groups in the cellulose molecular chain of the bio-based powder and have a certain degree of miscibility. This can improve the intermolecular forces, increase the strength of the entire system, and make it less prone to breakage.
[0051] This invention involves pre-mixing and stirring bio-based powder with a small amount of water to impregnate the bio-based powder. The mixture is then left to stand for 7-10 hours to allow the water to evaporate naturally while the bio-based powder is properly impregnated. Finally, 40-60 parts of the bio-based powder, 10-20 parts of polyethylene oxide (PEO), and 8-12 parts of water are added and stirred together to achieve rapid mixing and granulation. This invention strictly controls the amount of water used, which greatly reduces the drawbacks of water vapor generating bubbles during the preparation process and reduces the porosity of the bio-based polishing particles, thus further improving the strength of the product.
[0052] This invention controls the granulation temperature to between 85 and 95°C, thereby extending the extrusion time, resulting in more uniform components and better product performance.
[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A process for the preparation of biobased polishing particles, characterized in that, The steps are as follows: S1. Preparation of wood chip powder: Grind the bio-based material to obtain bio-based powder; the bio-based material is walnut shell; the walnut shell is ground into wood chip powder and passed through a 100-mesh sieve; S2. Pre-mixing: 40-60 parts of bio-based powder and 5-10 parts of water are fed into a mixer for mixing to achieve impregnation treatment; S3. Secondary mixing: Let the water-based mixture from step S2 stand for 7 to 10 hours, then add 40 to 60 parts of bio-based powder, 10 to 20 parts of polyethylene oxide (PEO), and 8 to 12 parts of water, and continue to mix at high speed to obtain a mixed slurry. S4. Granulation: The mixed slurry from step S3 is fed into a granulator for extrusion granulation at a granulation temperature of 85 to 95°C to obtain bio-based polished particles.
2. The process for the preparation of biobased polishing particles according to claim 1, characterized in that, In step S2, 50 parts of bio-based powder and 8 parts of water are fed into a mixer for mixing.
3. The process for the preparation of biobased polishing particles according to claim 1, characterized in that, In step S3, 50 parts of bio-based powder, 15 parts of polyethylene oxide (PEO), and 10 parts of water are added to a settled water mixture and stirred.
4. The process for the preparation of biobased polishing particles according to claim 1, characterized in that, The stirring rate in step S2 is 200-300 r / min.
5. A bio-based polishing particle prepared according to the preparation process described in claim 1.
Citation Information
Patent Citations
Plant fiber polishing powder and production method thereof
CN101885948A
Regenerated cellulose nano-particles and preparation method thereof
CN104558639A
Thermoplastic abrasive for polishing hard alloy and manufacture method thereof
CN107674304A