A solid waste-based building template and preparation method thereof

By using solid waste-based building templates prepared with composite tailings powder, rice husk ash and resin polymers, the existing building templates have solved the shortcomings in cost, performance and turnover rate, and efficient utilization of solid waste resources is achieved. It is a building formwork with high strength, high stiffness and strong durability, suitable for mass production.

CN116177929BActive Publication Date: 2024-11-05THE THIRD CONSTR OF CHINA CONSTR EIGHTH ENG BUREAU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310204903.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-06
Publication Date
2024-11-05
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

The existing building formwork has shortcomings in terms of cost, performance and turnover, especially the low turnover rate of bamboo and wood formwork, inflexible processing of aluminum alloy formwork, poor thermal stability of plastic formwork, and ineffective utilization of solid waste resources.

Method used

A new type of building formwork is prepared using composite tailings powder, rice husk ash and resin polymers. The composite material with high fineness is formed through drying, grinding, screening and mixing processes, and combined with silane coupling agent and lubricant , flame retardant and other ingredients to prepare solid waste-based building formwork with low cost, strong thermal stability and excellent mechanical properties, and design it as hollow plates or reinforced ribbed plates.

Benefits of technology

It realizes the efficient utilization of solid waste resources, provides construction formwork with low cost, stable performance and high turnover rate, meets the safety, practicality and economic requirements of the construction industry, and has high strength, high stiffness, strong durability and ability Advantages of multiple recycles and utilization, suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a solid waste-based building template, which is mainly prepared from the following raw materials: 15-25 parts of composite tailings powder, 5-12 parts of rice husk ash, 56-89 parts of resin polymer, 0.6-1.2 parts of silane coupling agent, 0.8-2 parts of lubricant, 1.8-2.5 parts of defoaming masterbatch, 0.5-0.9 parts of flame retardant, 0.4-0.8 parts of stabilizer and 0.2-0.4 parts of antioxidant, in parts by weight; the composite tailings powder is formed by compounding molybdenum tailings and red mud in a mass ratio of 1:1, with a fineness of 1000-1200 mesh and a moisture content of less than 0.1%. The present invention also discloses a preparation method of such a solid waste-based building template. The composite tailings powder used in the present invention is formed by compounding molybdenum tailings and red mud, and the two can be put into use only after drying and grinding, so there is no need to consider the influence of raw material components on product quality and performance. This utilization method significantly improves the resource utilization level of tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a building template, in particular to a building template with solid waste as main material and a preparation method thereof. Background Art

[0002] The large amount of tailings not only occupies land and threatens the local ecological environment, but also poses a major safety hazard in the local area. It is necessary to explore how to efficiently utilize tailings sand to serve economic development.

[0003] Building formwork is one of the commonly used turnover materials in the engineering field, and enterprises purchase a huge amount of it every year. Currently, bamboo-wood system, aluminum alloy system and plastic system formwork are used more. Among them, bamboo wood board has a low turnover rate and wastes a lot of forest resources every year; aluminum alloy plate has high strength and rigidity, but requires stereotyped processing and cannot be flexibly cut; plastic formwork has low cost and high turnover rate, but the material has poor thermal stability and is easy to deform. In order to cater to the development trend of the construction industry, it is of great significance to develop a new type of building formwork with low cost, stable performance, high turnover rate and free processing. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to address the deficiencies of the prior art, make rational use of solid waste resources, and provide a solid waste-based building formwork with low cost, strong thermal stability, high turnover rate and excellent mechanical properties.

[0005] Another object of the present invention is to provide a method for preparing the solid waste-based building template.

[0006] Technical solution: The solid waste-based building template described in the present invention is mainly prepared from the following raw materials: 15-25 parts of composite tailings powder, 5-12 parts of rice husk ash, 56-89 parts of resin polymer, 0.6-1.2 parts of silane coupling agent, 0.8-2 parts of lubricant, 1.8-2.5 parts of defoaming masterbatch, 0.5-0.9 parts of flame retardant, 0.4-0.8 parts of stabilizer and 0.2-0.4 parts of antioxidant, calculated in parts by weight; the composite tailings powder is formed by compounding molybdenum tailings and red mud in a mass ratio of 1:1, and is dried, ground and screened to form a fineness of 1000-1200 mesh and a moisture content of less than 0.1%. The main components are shown in Table 1.

[0007] Table 1 Main components of composite tailings powder

[0008]

[0009] Preferably, the rice husk ash is in the form of white-grey powder, has a fineness of 400-600 mesh after high grinding, a moisture content of less than 0.1%, and a main component of SiO2.

[0010] Preferably, the resin polymer comprises a density of 0.91 to 0.92 g / cm3 Block copolymer polypropylene 38-55 parts, density 0.88-0.90 g / cm 3 5-10 parts of low-density polyethylene, density 0.92-0.93 g / cm 3 3-6 parts of maleic anhydride grafted modified polypropylene, density 0.87-0.89 g / cm 3 10 to 18 parts of EPDM rubber, by weight.

[0011] Preferably, the silane coupling agent is one or more of epoxy type or amino type.

[0012] Preferably, the lubricant includes an internal lubricant and an external lubricant, which are one or more of fatty acid amide or organosilicon compound, the internal lubricant is used in an amount of 0.3 to 0.8 parts, and the external lubricant is used in an amount of 0.5 to 1.2 parts.

[0013] Preferably, the density of the defoaming masterbatch is 1.4-1.45 g / cm 3 , the melt flow rate is 15.5-23.2 (g / 10min); the flame retardant is one or more of CAS1309-42-8 and CAS21645-51-2; the stabilizer is one or more of ultraviolet absorber or hydroperoxide decomposer, and the antioxidant is one or more of 1010, 168 and 1024.

[0014] Preferably, the template is a lightweight hollow plate or a reinforced ribbed plate;

[0015] The standard length of the lightweight hollow board is 1830-2440 mm, the width is 915-1220 mm, the thickness of the lightweight hollow board is 15-25 mm, and the bulk density is 0.55-0.60 t / m 3 The solid part on both sides of the facade is 10-15mm thick, the internal hole shape is circular, rectangular, X-shaped or triangular, and the opening direction is arranged along the longitudinal direction;

[0016] The standard plate length of the reinforced ribbed plate is 1830-2440mm, and the width is 915-1220mm. Other sizes can also be customized according to project needs; the plate rib height is 2-3cm; the reinforced ribbed plate is provided with transverse ribs and longitudinal ribs, and the standard spacing is 0.46-0.60m, which can also be adjusted according to site needs; the rib thickness is consistent with the plate thickness, which is 2-3mm; the reinforced ribbed plate is provided with special tension screw holes, and the hole diameter and position are standardized according to the diameter of the tension screw and the needs of the cast component.

[0017] The method for preparing the solid waste-based building template comprises the following steps:

[0018] (1) drying the molybdenum tailings and red mud at 180-200° C., compounding them in a mass ratio of 1:1, and grinding them to form composite tailings powder with a fineness of 1000-1200 meshes;

[0019] (2) mixing the silane coupling agent and the composite tailings powder of step (1) uniformly and placing the mixture in a high-temperature mixer, and mixing the mixture at 105-115° C. for 4-6 minutes to form a mixture 1;

[0020] (3) drying and grinding the rice husk ash from the power plant, and then sieving to form a powder of 400-600 mesh;

[0021] (4) placing the rice husk ash and the resin polymer in step (3) in a high-temperature mixer and stirring at 105-115° C. for 4-6 minutes, and sieving through a vibrating screen to form a mixture 2 with a fineness of less than 50 mesh;

[0022] (5) placing the mixture 2 of step (4), the mixture 1 of step (2), an internal lubricant, an external lubricant, a defoamer, a flame retardant, a stabilizer and an antioxidant in a high temperature refrigerator, and then stirring for 8 to 10 minutes to form a mixture 3;

[0023] (6) putting the mixture 3 formed in step (5) into an internal mixer, heating, mixing and plasticizing for 15 to 20 minutes, and stopping stirring in the internal mixer when the mixture becomes a lump-like material;

[0024] (7) pouring the agglomerated material of step (6) into a conical double feeding system, and using a single screw granulation system to extrude particles of 1 to 3 mm in length to obtain a new solid waste-based composite substrate;

[0025] (8) Mix the granules obtained in step (7) with the masterbatch in proportion, dry them at 70 to 90° C., pour them into a blender and stir for 5 to 10 minutes, and then let them stand for 12 to 24 hours;

[0026] (9) The particles of step (8) are put into a construction formwork production line to form a new solid waste-based construction formwork through melting, adsorption, shaping, cutting and other steps.

[0027] Preferably, the parameters of the cone double feeding system in step (7) are set as follows: feeding speed 150-170 r / min, extrusion temperature 175-205° C., screw speed 350-450 r / min, pelletizing speed 15-25 r / min;

[0028] The parameters of the template production line in step (9) are set as follows: processing temperature 200-230°C, screw speed 150-200r / min, extrusion die temperature 190-205°C, pulling speed of the extrudate 0.8-2.3m / min, and the extrudate is formed by the template equipment after extrusion.

[0029] Beneficial effects: (1) The composite tailings powder used in the present invention is formed by the composite of molybdenum tailings and red mud. The two can be put into use only after drying and grinding, so there is no need to consider the influence of raw material components on product quality and performance. This utilization method significantly improves the resource utilization level of tailings; the new composite material prepared by using raw materials such as ultrafine tailings powder, rice husk ash and polymer resin has high overall strength, high rigidity and strong thermal stability, and the comprehensive cost is significantly lower than that of pure polymer materials; the composite material is used to prepare a new building formwork, which meets the requirements of safety, practicality and economy, has the advantages of high strength, high rigidity, strong durability, high turnover rate and multiple recycling, and is suitable for mass production. (2) From the perspective of structural design, the present invention designs the formwork into a hollow plate with an aperture of 15 to 25 mm, which is light in weight and easy to process, and is suitable for beams, plates and other components that bear less lateral pressure of concrete; after being designed as a reinforced ribbed plate, the overall rigidity and stability of the formwork are greatly improved, and it is more suitable for use in vertical walls, large spans or high hydration heat concrete components. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is described in detail below, but the protection scope of the present invention is not limited to the embodiments.

[0031] Example 1

[0032] Molybdenum tailings and red mud are dried at 180-200° C. and compounded in a mass ratio of 1:1, and ground to obtain composite tailings powder, the fineness of which is controlled at 1000-1200 meshes, the moisture content is ≤0.1%, and the dosage is 20 parts; 1.2 parts of silane coupling agent are evenly mixed with the composite tailings powder and placed in a high-temperature mixer, and mixed at 105-115° C. for 5 minutes to form a mixture 1; 8 parts of rice husk ash are taken, dried and ground, and sieved to form a powder of 400-600 meshes, which is placed in a high-temperature mixer with a resin polymer and stirred at 105-115° C. for 5 minutes, and sieved through a vibrating screen to form a mixture 2 with a fineness of less than 50 meshes; the resin polymer is selected from block copolymer polypropylene, low-density polyethylene, maleic anhydride grafted modified polypropylene and ethylene propylene diene monomer rubber, and the dosages are 45 parts, 7.5 parts, 4.5 parts and 14 parts respectively. Mixture 1, mixture 2, 0.8 parts of internal lubricant, 1.2 parts of external lubricant, 2.5 parts of defoamer, 0.9 parts of flame retardant, 0.8 parts of stabilizer and 0.4 parts of antioxidant are placed in a high-temperature refrigerator, and then stirred for 8 to 10 minutes to form mixture 3. Mixture 3 is put into an internal mixer, heated, mixed and plasticized for 15 to 20 minutes. When the mixture becomes a mass material, the internal mixer stops stirring, and the mass material is poured into a cone double feeding system, and a single screw granulation system is used to extrude particles with a length of 1 to 3 mm to obtain a new type of solid waste-based composite substrate; the particles are mixed with masterbatches in proportion, dried at 70 to 90°C, poured into a mixer and stirred for 5 to 10 minutes, and then left to stand for 20 hours, and then put into the template production line, and after melting, adsorption, shaping, cutting and other steps, a bulk density of 0.57t / m 3 , a hollow template with a thickness of 15 mm. According to the standard GB / T-1043.1, the water absorption rate, dimensional change rate after heating, microcal softening point, surface hardness, unnotched impact strength, bending strength and bending elastic modulus of the template were measured. The measurement results are shown in Table 2.

[0033] Example 2

[0034] The method and the amount of raw materials used are the same as in Example 1, and the bulk density is 1.13-1.35 t / m 3 According to the standard GB / T-1043.1, the water absorption rate, dimensional change rate after heating, microcal softening point, surface hardness, unnotched impact strength, bending strength and bending elastic modulus of the template were measured. The measurement results are shown in Table 2.

[0035] Example 3

[0036] The method and the amount of raw materials used are the same as in Example 1, the amount of composite tailings powder is adjusted to 25 parts, the amount of rice husk ash is 12 parts, and the amounts of other materials and methods remain unchanged. According to standard GB / T-1043.1, the water absorption rate, dimensional change rate after heating, microcal softening point, surface hardness, unnotched impact strength, flexural strength and flexural elastic modulus of the template are determined, and the measurement results are shown in Table 2.

[0037] Example 4

[0038] The method and the amount of raw materials used are the same as in Example 3, and the bulk density is 1.13-1.35 t / m 3 According to the standard GB / T-1043.1, the water absorption rate, dimensional change rate after heating, microcal softening point, surface hardness, unnotched impact strength, bending strength and bending elastic modulus of the template were measured. The measurement results are shown in Table 2.

[0039] Table 2 Main data statistics of each embodiment

[0040]

[0041] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.

Claims

1. A solid waste-based building template, characterized in that: It is mainly prepared from the following raw materials: 25 parts of composite tailings powder, 12 parts of rice husk ash, 45 parts of block copolymer polypropylene, 7.5 parts of low-density polyethylene, 4.5 parts of maleic anhydride grafted modified polypropylene, 14 parts of EPDM rubber, 1.2 parts of silane coupling agent, 0.8 parts of internal lubricant, 1.2 parts of external lubricant, 2.5 parts of defoaming masterbatch, 0.9 parts of flame retardant, 0.8 parts of stabilizer and 0.4 parts of antioxidant, calculated in parts by weight; the composite tailings powder is formed by compounding molybdenum tailings and red mud in a mass ratio of 1:1, with a fineness of 1000-1200 mesh and a moisture content of less than 0.1%.

2. The solid waste-based building template according to claim 1, characterized in that: The rice husk ash has a fineness of 400-600 meshes and a moisture content of less than 0.1%.

3. The solid waste-based building template according to claim 1, characterized in that: Including density of 0.91~0.92g / cm 3 Block copolymer polypropylene 45 parts, density 0.88~0.90g / cm 3 7.5 parts of low-density polyethylene, with a density of 0.92-0.93 g / cm 3 4.5 parts of maleic anhydride grafted modified polypropylene, density 0.87~0.89g / cm 3 14 parts of EPDM rubber, by weight.

4. The solid waste-based building template according to claim 1, characterized in that: The silane coupling agent is one or more of epoxy type or amino type.

5. The solid waste-based building template according to claim 1, characterized in that: The internal lubricant and the external lubricant are one or more of fatty acid amide or organic silicon compound.

6. The solid waste-based building template according to claim 1, characterized in that: The density of the defoaming masterbatch is 1.4-1.45 g / cm3, and the melt flow rate is 15.5-23.2 (g / 10 min); the flame retardant is one or more of CAS1309-42-8 and CAS21645-51-2; the stabilizer is one or more of ultraviolet absorber or hydroperoxide decomposer, and the antioxidant is one or more of 1010, 168 and 1024.

7. The solid waste-based building template according to claim 1, characterized in that: The formwork is a lightweight hollow board or a reinforced ribbed board; the standard length of the lightweight hollow board is 1830-2440mm, the width is 915-1220mm, the thickness of the lightweight hollow board is 15-25mm, the bulk density is 0.55-0.60t / m³, the solid part on both sides of the facade is 10-15mm thick, the internal hole type is circular, rectangular, X-shaped or triangular, and the opening direction is arranged longitudinally; the standard board length of the reinforced ribbed board is 1830-2440mm, the width is 915-1220mm, and the board rib height is 2-3cm; the reinforced ribbed board is provided with transverse ribs and longitudinal ribs, the standard spacing is 0.46-0.60m, and the rib thickness is consistent with the board thickness, which is 2-3mm; the reinforced ribbed board is provided with special tension screw holes, and the hole diameter and position are set according to the diameter of the tension screw and the needs of the cast component.

8. The method for preparing a solid waste-based building template according to any one of claims 1 to 7, characterized in that The invention comprises the following steps: (1) drying molybdenum tailings and red mud at 180-200° C. and compounding them in a mass ratio of 1:1, grinding and processing to form a composite tailings powder with a fineness of 1000-1200 mesh; (2) mixing a silane coupling agent and the composite tailings powder of step (1) uniformly and placing them in a high-temperature mixer, mixing them at 105-115° C. for 4-6 minutes to form a mixture 1; (3) drying and grinding rice husk ash from a power plant, and sieving and forming a powder with a mesh of 400-600 mesh; (4) placing the rice husk ash of step (3) and a resin polymer in a high-temperature mixer, stirring them at 105-115° C. for 4-6 minutes, and sieving them through a vibrating screen to form a mixture 2 with a fineness of less than 50 mesh; (5) mixing the mixture 2 of step (4), the mixture 1 of step (2), an internal lubricant, an external lubricant, and a defoaming agent; The agent, flame retardant, stabilizer and antioxidant are placed together in a high-temperature cooling machine, and then stirred for 8 to 10 minutes to form a mixture 3; (6) The mixture 3 formed in step (5) is put into an internal mixer, and heated, mixed and plasticized for 15 to 20 minutes. When the mixture becomes a mass material, the internal mixer stops stirring; (7) The mass material of step (6) is poured into a conical double feeding system, and a single screw granulation system is used to extrude particles with a length of 1 to 3 mm to obtain a solid waste-based new composite substrate; (8) The particles of step (7) are mixed with masterbatches in proportion, dried at 70 to 90°C, poured into a mixer and stirred for 5 to 10 minutes, and then left to stand for 12 to 24 hours; (9) The particles of step (8) are put into a building template production line, and a solid waste-based new building template is formed through melting, adsorption, shaping and cutting.

9. The method for preparing a solid waste-based building formwork according to claim 8, characterized in that: The parameters of the conical double feeding system in step (7) are set as follows: feeding speed 150-170 r / min, extrusion temperature 175-205°C, screw speed 350-450 r / min, and pelletizing speed 15-25 r / min; the parameters of the template production line in step (9) are set as follows: processing temperature 200-230°C, screw speed 150-200 r / min, extrusion die temperature 190-205°C, and pulling speed of the extrudate 0.8-2.3 m / min, and the extrudate is formed by the template equipment after extrusion.