A high-fluidity and high-shape-retention PE material and its preparation method and application
The PE resin is swelled by terpene resin and liquid paraffin, and reacted with ferrocene under magnetic field and temperature to generate high-flow and high-type retention PE material, which solves the poor extrusion and form retention of PE raw materials in the production of hollow wound tubes. The problem of this achieves efficient production and low-cost hollow winding pipe manufacturing.
Patent Information
- Application Number
- CN202211712174.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The existing PE raw materials are not suitable for square tube extrusion when preparing hollow winding pipes and have poor pattern retention, resulting in low production efficiency, high scrap rate and increased cost.
The PE resin is swelled by terpene resin and liquid paraffin, and react with the ferrocene catalyst at a magnetic field and a specific temperature to form a plasticized PE resin in EVA to improve the fluidity and pattern retention of the material.
The prepared high-flow and high-type retention PE material has good thermal stability, small wall thickness deviation, high tensile yield strength and low impact test breakage rate of the lower hammer, and is suitable for the production of hollow winding tubes.
Smart Images

Figure GDA0004205461730000071 
Figure GDA0004205461730000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of material technology, and more specifically, to a high-fluidity and high-shape-retaining PE material and a preparation method and application thereof. Background Art
[0002] PE hollow winding tube is made of high-density polyethylene (HDPE) and is formed by winding and welding. Due to its unique molding process, PE hollow winding tube with a diameter of up to 3 meters can be produced. At present, the production process of PE hollow winding tube is a two-step molding process: the first extruder extrude the round tube, which is shaped into a square tube by a shaping and cooling machine, and then enters the winding molding machine. At the same time, the second extruder extrude the molten rubber strip to bond the square tube in the form of a spiral line. Since the existing PE raw materials have poor shape retention, when a square tube mold is used for extrusion, it is easy to deform, so the square tube extrusion process cannot be used. At present, the industry mainly uses round tube extrusion and then square tube shaping. This process is not only inefficient, but also has a high scrap rate, resulting in increased product costs.
[0003] The Chinese patent entitled HDPE Hollow Flat Wall Wrapping Tube Material provides a hollow flat wall wrapping tube material, which mainly focuses on the mechanical properties of the material and does not focus on the shape retention of the material.
[0004] Therefore, it is necessary to study a PE material that is suitable for the extrusion of square tubes and has a good shape-retaining effect. Summary of the invention
[0005] The primary purpose of the present invention is to overcome the problem that the above-mentioned existing PE raw materials are not suitable for extrusion of square tubes and have poor shape retention when preparing hollow winding tubes, and to provide a method for preparing a high-fluidity and high-shape retention PE material. The high-fluidity and high-shape retention PE material prepared by the preparation method has high thermal stability and thus has good fluidity; the hollow winding tube made of the high-fluidity and high-shape retention PE material as a raw material has a small wall thickness deviation and good shape retention. In addition, the high-fluidity and high-shape retention PE material also has good tensile yield strength and a low drop weight impact test breakage rate.
[0006] A further object of the present invention is to provide a PE material with high fluidity and high shape retention.
[0007] A further object of the present invention is to provide the use of the above-mentioned high-fluidity and high-shape-retaining PE material in the preparation of a hollow winding pipe.
[0008] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0009] A method for preparing a high-fluidity and high-shape-retaining PE material comprises the following steps:
[0010] S1. The terpene resin and liquid paraffin are mixed, heated, and then PE resin is added to obtain a first mixed solution for standby use; the EVA resin is heated, and then a ferrocene catalyst is added to react to obtain a second mixed solution for standby use;
[0011] S2. The first mixed liquid and the second mixed liquid are mixed, reacted, and then plasticized under the conditions of a magnetic field strength of 1 to 1.5 T and a temperature of 30 to 60° C. to obtain the high-fluidity and high-shape-retention PE material.
[0012] The inventor of the present invention has found through many studies that terpene resin and liquid paraffin are used as solvents to swell PE resin so that it has a certain viscoelasticity, and a PE resin with terminal group activity, i.e., the first mixed solution, is obtained; at the same time, a ferrocene catalyst is added to the EVA resin to react to generate a terminal ferrocene EVA resin, i.e., the second mixed solution; then the first mixed solution and the second mixed solution are mixed, and first react to generate an EVA internal plasticized PE resin, and then plasticize in a magnetic field and a specific temperature to make the EVA internal plasticized PE resin molecule arrangement oriented, thereby obtaining a high-fluidity and high-shape-retaining PE material. The high-fluidity and high-shape-retaining PE material has high thermal stability and thus has good fluidity; the wall thickness deviation of the hollow winding tube made of it as a raw material is small and the shape retention is good. In addition, the high-fluidity and high-shape-retaining PE material also has good tensile yield strength and a low drop hammer impact test breakage rate.
[0013] Preferably, in step S1, the mass ratio of the terpene resin to the liquid paraffin is 1:(0.5-2).
[0014] More preferably, in step S1, the mass ratio of the terpene resin to the liquid paraffin is 1:(0.6-1.6).
[0015] The mass ratio of terpene resin to liquid paraffin is controlled within this range, and the PE hollow winding tube made of the high-fluidity and high-shape-retaining PE material finally obtained has smaller wall thickness deviation and better shape-retaining property.
[0016] Preferably, in step S1, after the terpene resin and the liquid paraffin are mixed, the heating temperature before the PE resin is added is 90-120°C.
[0017] Preferably, in step S1, the mass percentage of the PE resin in the first mixed solution is 80-90%.
[0018] More preferably, in step S1, the mass percentage of PE resin in the first mixed solution is 84-88%.
[0019] When the PE resin is controlled within this range, the resulting high-fluidity and high-shape-retention PE material will have better thermal stability.
[0020] Preferably, the weight average molecular weight of the EVA resin in step S1 is 10,000 to 50,000.
[0021] Preferably, before adding the ferrocene catalyst in step S1, the EVA resin is heated to 90-100°C.
[0022] Preferably, after the EVA resin is heated in step S1, the viscosity of the EVA resin is 10000-12000 cps.
[0023] Preferably, before adding the ferrocene catalyst in step S1, the process further comprises adding a diluent into the EVA resin.
[0024] More preferably, the diluent is cyclohexane.
[0025] Preferably, the reaction temperature of the reaction in step S1 is 90-120°C.
[0026] More preferably, the reaction temperature of the reaction in step S1 is 100-115°C.
[0027] By controlling the reaction of EVA resin and ferrocene within this range, the obtained high-fluidity and high-shape-retention PE material not only has better fluidity and shape-retention, but also has higher tensile yield strength and lower breakage rate in drop weight impact test.
[0028] Preferably, in step S1, the mass ratio of the EVA resin to the ferrocene catalyst is 1:(0.005-0.02).
[0029] More preferably, in step S1, the mass ratio of the EVA resin to the ferrocene catalyst is 1:(0.01-0.018).
[0030] By controlling the mass ratio of EVA resin to ferrocene catalyst within this range, the obtained high-fluidity and high-shape-retention PE material not only has better fluidity and shape-retention, but also has higher tensile yield strength and lower breakage rate in drop weight impact test.
[0031] Preferably, in step S2, the mass ratio of the first mixed liquid to the second mixed liquid is 1:(0.05-2).
[0032] More preferably, in step S2, the mass ratio of the first mixed liquid to the second mixed liquid is 1:(0.5-2).
[0033] Preferably, the reaction temperature of the reaction in step S2 is 100-120° C., and the reaction time is 30-90 min.
[0034] A high-fluidity and high-shape-retaining PE material is prepared by the above preparation method.
[0035] The application of the above-mentioned high-fluidity and high-shape-retaining PE material in the preparation of hollow winding pipes is also within the protection scope of the present invention.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] The high-fluidity and high-shape-retaining PE material of the present invention has high thermal stability and good fluidity; the hollow winding tube made of the high-fluidity and high-shape-retaining PE material has small wall thickness deviation and good shape retention. In addition, the high-fluidity and high-shape-retaining PE material has good tensile yield strength and low drop weight impact test breakage rate. DETAILED DESCRIPTION
[0038] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.
[0039] Example 1
[0040] The present embodiment provides a method for preparing a high-fluidity and high-shape-retaining PE material, comprising the following steps:
[0041] 1. Mix terpene resin and liquid paraffin in a mass ratio of 1:2, heat at 90°C until the terpene resin and liquid paraffin are evenly mixed, then add PE resin (weight average molecular weight of 3000000, the same below), stir until homogeneous to obtain a first mixed solution for standby use; heat EVA resin (weight average molecular weight of 10000, the same below) to 90°C, test its viscosity using a rotary viscometer, add an appropriate amount of inactive diluent cyclohexane, adjust the viscosity to 10000cps, then add ferrocene catalyst, react at 90°C for 1 hour, and obtain a second mixed solution. Among them, the mass fraction of PE resin in the first mixed solution is 80%; the mass fraction of ferrocene catalyst in the EVA resin is 0.5%.
[0042] 2. The first mixed liquid and the second mixed liquid were mixed at a mass ratio of 1:0.5 at 100°C and reacted for 30 minutes; then plasticized under the conditions of a magnetic field intensity of 1T and a temperature of 30°C to obtain a high-fluidity and high-shape-retention PE material.
[0043] Example 2
[0044] The present embodiment provides a method for preparing a high-fluidity and high-shape-retaining PE material, comprising the following steps:
[0045] 1. Mix terpene resin and liquid paraffin in a mass ratio of 1:1.6, heat at 90°C until the terpene resin and liquid paraffin are evenly mixed, then add PE resin, stir until homogeneous to obtain a first mixed solution for standby use; heat EVA resin to 90°C, test its viscosity using a rotary viscometer, add an appropriate amount of inactive diluent cyclohexane, adjust the viscosity to 10000cps, then add ferrocene catalyst, react at 90°C for 0.5 hours, and obtain a second mixed solution. Among them, the mass fraction of PE resin in the first mixed solution is 82%; the mass fraction of ferrocene catalyst in EVA resin is 0.8%.
[0046] 2. The first mixed liquid and the second mixed liquid were mixed at a mass ratio of 1:0.75 at 100°C and reacted for 30 minutes; then plasticized under the conditions of a magnetic field strength of 1.1T and a temperature of 35°C to obtain a high-fluidity and high-shape-retention PE material.
[0047] Example 3
[0048] The present embodiment provides a method for preparing a high-fluidity and high-shape-retaining PE material, comprising the following steps:
[0049] 1. Mix terpene resin and liquid paraffin in a mass ratio of 1:1.2, heat at 90°C until the terpene resin and liquid paraffin are evenly mixed, then add PE resin, stir until homogeneous to obtain a first mixed solution for standby use; heat EVA resin to 90°C, test its viscosity using a rotary viscometer, add an appropriate amount of inactive diluent cyclohexane, adjust the viscosity to 10000cps, add ferrocene catalyst, react at 100°C for 1 hour, and obtain a second mixed solution. Among them, the mass fraction of PE resin in the first mixed solution is 84%; the mass fraction of ferrocene catalyst in EVA resin is 1%.
[0050] 2. The first mixed liquid and the second mixed liquid were mixed at a mass ratio of 1:1 at 100°C and reacted for 30 minutes; then plasticized under the conditions of a magnetic field intensity of 1.2T and a temperature of 40°C to obtain a high-fluidity and high-shape-retention PE material.
[0051] Example 4
[0052] The present embodiment provides a method for preparing a high-fluidity and high-shape-retaining PE material, comprising the following steps:
[0053] 1. Mix terpene resin and liquid paraffin in a mass ratio of 1:1, heat at 90°C until the terpene resin and liquid paraffin are evenly mixed, then add PE resin, stir until homogeneous to obtain a first mixed solution for standby use; heat EVA resin to 90°C, test its viscosity using a rotary viscometer, add an appropriate amount of inactive diluent cyclohexane, adjust the viscosity to 10000cps, then add ferrocene catalyst, react at 110°C for 1.2 hours, and obtain a second mixed solution. Among them, the mass fraction of PE resin in the first mixed solution is 85%; the mass fraction of ferrocene catalyst in EVA resin is 1.2%.
[0054] 2. The first mixed liquid and the second mixed liquid were mixed at a mass ratio of 1:1.5 at 100°C and reacted for 30 minutes; then plasticized under the conditions of a magnetic field strength of 1.25T and a temperature of 45°C to obtain a high-fluidity and high-shape-retention PE material.
[0055] Example 5
[0056] The present embodiment provides a method for preparing a high-fluidity and high-shape-retaining PE material, comprising the following steps:
[0057] 1. Mix terpene resin and liquid paraffin in a mass ratio of 1:0.8, heat at 90°C until the terpene resin and liquid paraffin are evenly mixed, then add PE resin, stir until homogeneous to obtain a first mixed solution for standby use; heat EVA resin to 90°C, test its viscosity using a rotary viscometer, add an appropriate amount of inactive diluent cyclohexane, adjust the viscosity to 10000cps, then add ferrocene catalyst, react at 110°C for 1.1 hours, and obtain a second mixed solution. Among them, the mass fraction of PE resin in the first mixed solution is 86%; the mass fraction of ferrocene catalyst in EVA resin is 1.5%.
[0058] 2. The first mixed liquid and the second mixed liquid were mixed at a mass ratio of 1:1.75 at 100°C and reacted for 30 minutes; then plasticized under the conditions of a magnetic field strength of 1.3T and a temperature of 50°C to obtain a high-fluidity and high-shape-retention PE material.
[0059] Example 6
[0060] The present embodiment provides a method for preparing a high-fluidity and high-shape-retaining PE material, comprising the following steps:
[0061] 1. Mix terpene resin and liquid paraffin in a mass ratio of 1:0.6, heat at 90°C until the terpene resin and liquid paraffin are evenly mixed, then add PE resin, stir until homogeneous to obtain a first mixed solution for standby use; heat EVA resin to 90°C, test its viscosity using a rotary viscometer, add an appropriate amount of inactive diluent cyclohexane, adjust the viscosity to 10000cps, then add ferrocene catalyst, react at 115°C for 1.3 hours, and obtain a second mixed solution. Among them, the mass fraction of PE resin in the first mixed solution is 88%; the mass fraction of ferrocene catalyst in EVA resin is 1.8%.
[0062] 2. The first mixed liquid and the second mixed liquid were mixed at a mass ratio of 1:1.8 at 100°C and reacted for 30 minutes; then plasticized under the conditions of a magnetic field strength of 1.4T and a temperature of 55°C to obtain a high-fluidity and high-shape-retention PE material.
[0063] Example 7
[0064] The present embodiment provides a method for preparing a high-fluidity and high-shape-retaining PE material, comprising the following steps:
[0065] 1. Mix terpene resin and liquid paraffin in a mass ratio of 1:0.5, heat at 90°C until the terpene resin and liquid paraffin are evenly mixed, then add PE resin, stir until homogeneous to obtain a first mixed solution for standby use; heat EVA resin to 90°C, test its viscosity using a rotary viscometer, add an appropriate amount of inactive diluent cyclohexane, adjust the viscosity to 10000cps, then add ferrocene catalyst, react at 120°C for 1.5 hours, and obtain a second mixed solution. Among them, the mass fraction of PE resin in the first mixed solution is 90%; the mass fraction of ferrocene catalyst in EVA resin is 2%.
[0066] 2. The first mixed liquid and the second mixed liquid were mixed at a mass ratio of 1:2 at 100°C and reacted for 30 minutes; then plasticized under the conditions of a magnetic field strength of 1.5T and a temperature of 60°C to obtain a high-fluidity and high-shape-retention PE material.
[0067] Comparative Example 1
[0068] This comparative example provides a method for preparing a PE material, which is different from Example 1 in that: in the first step, no ferrocene catalyst is added, that is, the EVA resin is heated to 90°C, and then an appropriate amount of inactive diluent cyclohexane is added and adjusted to a viscosity of 10,000 cps to obtain a second mixed liquid.
[0069] Comparative Example 2
[0070] This comparative example provides a method for preparing a PE material. Except that the step of obtaining the first mixed solution is the same as that in Example 1, the other steps are as follows: no ferrocene catalyst is added to the EVA resin, that is, the EVA resin and the ferrocene catalyst are not reacted at 90°C for 1 hour, but the EVA resin and the ferrocene catalyst are directly added to the first mixed solution at the same time, mixed at 100°C, and reacted for 30 minutes; and then plasticized under the conditions of a magnetic field intensity of 1.5T and a temperature of 60°C to obtain the PE material.
[0071] Comparative Example 3
[0072] This comparative example provides a method for preparing a PE material, which is different from Example 1 in that no terpene resin is added.
[0073] Comparative Example 4
[0074] This comparative example provides a method for preparing a PE material, which is different from Example 1 in that liquid paraffin is not added.
[0075] Performance Testing
[0076] The high-fluidity and high-shape-retaining PE materials obtained in Examples 1 to 7 and the PE materials obtained in Comparative Examples 1 to 5 were taken and their properties were measured according to the following test methods or test standards.
[0077] Thermal stability: The PE materials of the embodiments and comparative examples were subjected to dynamic thermal stability tests using a torque rheometer. The test process was as follows: sampling was performed every 3 minutes for color testing until the color changed. The length of the thermal stability time characterizes the thermal stability of the material system. The slower the color change and the longer the thermal stability time, the better the thermal stability of the material. The faster the color change and the shorter the thermal stability time, the worse the thermal stability of the material.
[0078] Tensile yield strength: The test method is determined in accordance with GB / T8804.2-2003;
[0079] Breakage rate of drop weight impact test: The test method is determined in accordance with GB / T14152-2001, breakage rate = (number of broken samples / total number of samples) × 100%.
[0080] The high-fluidity and high-shape-retention PE materials obtained in Examples 1 to 7 and the PE materials obtained in Comparative Examples 1 to 5 were used as raw materials to make PE hollow winding tubes and test the wall thickness deviation of the PE hollow winding tubes. The test method is as follows:
[0081] Wall thickness deviation: Wall thickness deviation = [(maximum wall thickness - minimum wall thickness) / nominal wall thickness] × 100%, the nominal wall thickness refers to GB / T10002.1-2006, the maximum wall thickness and the minimum wall thickness are measured at 20 points along the circumference of the pipe wall, and the maximum and minimum values are taken as the maximum wall thickness and the minimum wall thickness respectively.
[0082] The test results of various properties are shown in Table 1 below.
[0083] Table 1 Performance test results of various embodiments and comparative examples
[0084]
[0085]
[0086] From Table 1, we can see that;
[0087] The thermal stability time of the high-fluidity and high-shape-retaining PE materials of Examples 1 to 7 is greater than 39 minutes, indicating that the high-fluidity and high-shape-retaining PE materials prepared by the preparation method of the present invention have high thermal stability and thus have good fluidity; the wall thickness deviation of the prepared PE hollow winding tube is less than 1.5%, indicating that the high-fluidity and high-shape-retaining PE materials prepared by the preparation method of the present invention have good shape retention. In addition, the tensile yield strength of the high-fluidity and high-shape-retaining PE materials of Examples 1 to 7 is greater than 40.2MPa, and the drop weight impact test breakage rate is less than 5%, indicating that the high-fluidity and high-shape-retaining PE materials prepared by the preparation method of the present invention also have good tensile yield strength and low drop weight impact test breakage rate.
[0088] In Comparative Example 1, no ferrocene catalyst is added, and the obtained high-fluidity and high-shape-retention PE material has low thermal stability, low tensile yield strength, high drop weight impact test breakage rate, and poor shape retention of the material; in Comparative Example 2, EVA resin and ferrocene catalyst are directly added to the first mixed liquid without reacting, and the obtained high-fluidity and high-shape-retention PE material has low thermal stability, low tensile yield strength, high drop weight impact test breakage rate, and poor shape retention of the material; Comparative Examples 3 and 4 do not add terpene resin and liquid paraffin respectively, and the obtained high-fluidity and high-shape-retention PE materials have poor thermal stability, tensile yield strength and drop weight impact test breakage rate, and the material has poor shape retention.
[0089] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a high-fluidity and high-shape-retaining PE material, characterized in that: The steps include: S1. The terpene resin and liquid paraffin are mixed, heated, and then PE resin is added to obtain a first mixed solution for standby use; the EVA resin is heated, and then a ferrocene catalyst is added to react to obtain a second mixed solution for standby use; S2. The first mixed solution and the second mixed solution are mixed, reacted, and then plasticized under a magnetic field strength of 1 to 1.5T and a temperature of 30 to 60°C to obtain the high fluidity and high shape retention PE material; The reaction temperature of the reaction in step S1 is 90-120°C; The mass ratio of the EVA resin to the ferrocene catalyst in step S1 is 1:(0.005-0.02); Before adding the ferrocene catalyst in step S1, the process further includes adding a diluent into the EVA resin, wherein the diluent is cyclohexane.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the terpene resin to the liquid paraffin in step S1 is 1:(0.5-2).
3. The preparation method according to claim 1, characterized in that: In step S1, after the terpene resin and the liquid paraffin are mixed, the heating temperature before the PE resin is added is 90-120°C.
4. The preparation method according to claim 1, characterized in that: In step S1, the mass percentage of PE resin in the first mixed solution is 80-90%.
5. The preparation method according to claim 1, characterized in that: The weight average molecular weight of the EVA resin in step S1 is 10,000 to 50,000.
6. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of the first mixed liquid to the second mixed liquid is 1:(0.05-2).
7. The preparation method according to claim 1, characterized in that: The reaction temperature of the reaction in step S2 is 90-120° C., and the reaction time is 30-90 min.
8. A high-fluidity and high-shape-retention PE material, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the high-fluidity and high-shape-retaining PE material according to claim 8 in the preparation of hollow wall winding pipes.