A HIPS material, preparation method thereof, appearance part and air conditioner

By blending polystyrene and polypropylene and adding inorganic rigid particles and styrene-butadiene copolymer, the problem of HIPS materials losing gloss when improving impact resistance is solved, achieving high gloss, toughness and strength. Improved, cost lower than ABS, suitable for air conditioner appearance parts.

CN116178872BActive Publication Date: 2024-10-29HISENSE (SHANDONG) AIR CONDITIONING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310154250.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-10-29
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Existing HIPS materials lose gloss while improving impact resistance. They cannot improve toughness and strength while maintaining gloss. They are also costly and difficult to apply to high-gloss air conditioner exterior parts.

Method used

Polystyrene and polypropylene are blended, and inorganic rigid particles and styrene-butadiene copolymer are added as tougheners, together with compatibilizers such as polypropylene grafted maleic anhydride, through high-speed mixing and twin-screw melt extrusion. HIPS materials are prepared using advanced technology to improve the toughness and strength of the material while maintaining gloss.

Benefits of technology

It is possible to improve the toughness and strength of HIPS materials while maintaining gloss. The cost is lower than ABS, and the processing performance does not decrease, and can match ABS.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116178872B_ABST
    Figure CN116178872B_ABST
Patent Text Reader

Abstract

The present invention discloses a HIPS material, a preparation method thereof, an appearance part and an air conditioner, and belongs to the technical field of polymer materials. The HIPS material includes polystyrene, polypropylene, a toughening agent, and a compatibilizer; the toughening agent includes inorganic rigid particles and styrene-butadiene copolymer, and the weight ratio of the inorganic rigid particles to the styrene-butadiene copolymer is any value of 1:2-2:1; the compatibilizer is selected from at least one of polypropylene grafted maleic anhydride, silane coupling agent, aluminate coupling agent and titanate coupling agent. The present invention is applied to the appearance parts of air conditioners, solves the problem that the existing HIPS material cannot take into account both impact resistance and glossiness and cannot be applied to the appearance parts of air conditioners, and can improve the toughness, strength and rigidity of the substrate while maintaining the glossiness of the material, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a HIPS material, a preparation method thereof, an appearance part and an air conditioner. Background Art

[0002] As people's living standards improve, household appliances with high-gloss shells are becoming more and more popular. For example, air conditioners mainly use high-gloss ABS materials for the manufacture of exterior parts. ABS has excellent comprehensive performance, but the price is relatively high and is affected by market fluctuations. HIPS is relatively cheap, but its impact resistance and glossiness are far lower than ABS, and its usage scenarios are limited. The high-gloss HIPS materials currently on the market have a much lower impact strength than ABS, and their glossiness cannot be on par with ABS.

[0003] The classic method of producing HIPS is bulk polymerization, that is, dissolving rubber in styrene monomer, and polymerizing by heat or initiator to form a graft copolymer of styrene and rubber to improve the toughness of the product. However, while the introduction of rubber improves the toughness of the material, it also makes the material lose its transparency, and also has a certain impact on the heat resistance and gloss of the material. It can be seen that the impact resistance and gloss of HIPS are a pair of relatively contradictory indicators, and adding rubber to toughen it will reduce the gloss of HIPS. Summary of the invention

[0004] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is to overcome the problem that the existing HIPS material cannot take into account both impact resistance and glossiness and cannot be applied to air-conditioning appearance parts. A low-cost HIPS material, a preparation method thereof, an appearance part and an air-conditioner are proposed, which can improve the toughness, strength and rigidity of the substrate while maintaining the glossiness of the material.

[0005] In order to solve the technical problem, the technical solution adopted by the present invention is:

[0006] On one hand, the present invention provides a HIPS material, comprising polystyrene, polypropylene, a toughening agent, and a compatibilizer; in parts by weight, the polystyrene is selected from any value in the range of 60-80 parts, the polypropylene is selected from any value in the range of 20-40 parts, the toughening agent is selected from any value in the range of 5-20 parts, and the compatibilizer is selected from any value in the range of 0.5-3 parts; the toughening agent comprises inorganic rigid particles and styrene-butadiene copolymer, and the weight ratio of the inorganic rigid particles to the styrene-butadiene copolymer is any value in the range of 1:2-2:1; the compatibilizer is selected from at least one of polypropylene grafted maleic anhydride, a silane coupling agent, an aluminate coupling agent, and a titanate coupling agent.

[0007] Preferably, the inorganic rigid particles are surface modified by the following method, including: drying the unmodified inorganic rigid particles, weighing the dried inorganic rigid particles into a high-speed universal grinder, quickly introducing stearic acid dissolved in ethanol into the high-speed universal grinder, stirring for 3-8 minutes, taking out and drying at 60-100°C, sampling and storing to obtain the inorganic rigid particles; the mass ratio of the stearic acid to the ethanol is any value between 1:8 and 1:12.

[0008] Preferably, the melt flow rate of the polystyrene is 2-25 g / 10 min, and the weight average molecular weight is 5×104-15×104; the polypropylene is medium melt index polypropylene, the melt flow rate is 10-20 g / 10 min, and the Izod notched impact strength is ≥20 kJ / ㎡.

[0009] Preferably, the compatibilizer is polypropylene grafted with maleic anhydride.

[0010] Preferably, it also includes an antioxidant, a lubricant, and a UV absorber; in parts by weight, the antioxidant is selected from any value in the range of 0.1-2.5 parts, the lubricant is selected from any value in the range of 0.1-0.5 parts, and the UV absorber is selected from any value in the range of 0-2.5 parts.

[0011] Preferably, the antioxidant is one or more of diphenylamine and its derivatives, p-phenylenediamine and its derivatives, 2,6-tert-butyl-4-methylphenol, bis(3,5-tert-butyl-4-hydroxyphenyl)sulfide or phosphite; the lubricant is one or more of silicone oil, white mineral oil, barium stearate, magnesium stearate, paraffin, and ethylenebisstearamide; the UV absorber is a mixture of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0012] The present invention also provides a method for preparing the HIPS material described in any of the above technical solutions, comprising a raw material mixing step and a HIPS material preparation step.

[0013] Preferably, the raw material mixing step adopts high-speed mixing, the rotation speed of the high-speed mixing and stirring is 700-1200r / min, and the mixing time is 5-10min; the HIPS material preparation step adopts twin-screw melt extrusion, cooling, drying and pelletizing to obtain the HIPS material, the extrusion temperature of the twin-screw melt extrusion is 180-210°C, the screw speed is 300-600r / min, the drying temperature is 65-115°C, and the drying time is 1-3h.

[0014] Another aspect of the present invention provides an appearance part, which is prepared from the HIPS material described in any of the above technical solutions.

[0015] The present invention also provides an air conditioner, comprising the appearance part described in the above technical solution.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The invention provides a HIPS material, which adopts polystyrene resin and polypropylene resin to blend, and can improve the toughness, strength and rigidity of a base material while maintaining the glossiness; inorganic rigid particles and SBS are compounded as a toughening agent, and can improve the strength and rigidity of the material while improving the toughness, and there is no disadvantage of reduced processing performance; the glossiness and toughness of the material can be equal to those of ABS, and the cost is lower than ABS. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a flow chart of the preparation process of the HIPS material provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0019] The technical scheme in the specific embodiment of the present invention will be described in detail and completely in conjunction with the accompanying drawings. Obviously, the described embodiments are only some specific implementation methods of the overall technical scheme of the present invention, rather than all implementation methods. Based on the overall concept of the present invention, all other embodiments obtained by ordinary technicians in this field fall within the scope of protection of the present invention.

[0020] On one hand, the present invention provides a HIPS material, comprising polystyrene, polypropylene, a toughening agent, and a compatibilizer; in parts by weight, the polystyrene is selected from any value in the range of 60-80 parts, the polypropylene is selected from any value in the range of 20-40 parts, the toughening agent is selected from any value in the range of 5-20 parts, and the compatibilizer is selected from any value in the range of 0.5-3 parts; the toughening agent comprises inorganic rigid particles and styrene-butadiene copolymer, and the weight ratio of the inorganic rigid particles to the styrene-butadiene copolymer is any value in the range of 1:2-2:1; the compatibilizer is selected from at least one of polypropylene grafted maleic anhydride, a silane coupling agent, an aluminate coupling agent, and a titanate coupling agent. The present invention specifically defines the dosage of polystyrene, polypropylene, toughening agent, and compatibilizer. It is understood that the dosage of polystyrene can also be 65, 70, 75 parts and any value within the range, the dosage of polypropylene can also be 25, 30, 35 parts and any value within the range, the dosage of toughening agent can also be 10, 15 parts and any value within the range, and the dosage of compatibilizer can also be 1, 1.5, 2, 2.5 parts and any value within the range. Optionally, the particle size of the inorganic rigid particles (RIF) is between 0.05 μm and 5 μm.

[0021] The present invention provides a HIPS material, which can achieve high gloss, high impact resistance and low cost through the types and proportions of polystyrene, polypropylene, toughening agent and compatibilizer, so as to replace the existing ABS material for air conditioner appearance parts. By blending polystyrene resin and polypropylene resin, the toughness, strength and rigidity of the substrate can be improved while maintaining the gloss; by compounding inorganic rigid particles with SBS as a toughening agent, the strength and rigidity of the material can be improved while improving the toughness, and there is no disadvantage of reduced processing performance; the gloss and toughness of the material can be the same as ABS, while the cost is lower than ABS. Specifically, polypropylene (PP) has the advantages of light weight, low price, chemical resistance, good heat resistance and stability, and is widely used in the fields of household appliances, transportation, electric tools, etc., but PP also has many disadvantages, such as large molding shrinkage, low hardness, poor printing performance, etc., which limit its wider application. Compared with PP, polystyrene (PS) has poor environmental stress cracking resistance, toughness and chemical resistance, but PS has higher modulus, higher surface hardness, low shrinkage and excellent printing performance, and is widely used in home appliances, office equipment, household products and other industries. As the continuous phase of polystyrene and the dispersed phase of polypropylene, there is a great difference in Young's modulus and Poisson's ratio, which generates a high static pressure around the interface of the two phases. Under the action of this high static pressure, the dispersed phase of polypropylene is prone to yield and produce cold stretching, and a brittle-tough transition occurs, thereby absorbing a large amount of impact energy to achieve the purpose of toughening. The use of polypropylene and polystyrene blends can improve the strength and rigidity of the material while improving the toughness, and there is no deficiency of gloss reduction. In addition, the traditional toughening method is very simple and easy to implement, which can significantly improve the toughening of the resin. Generally, a small amount of rubber elastomer is added to the resin as a toughening agent. However, due to the low modulus and poor strength of the rubber phase added to the material, the rigidity, processing performance and tensile strength of the material are often reduced to varying degrees while the impact strength of the entire composite material is improved. During deformation, the presence of inorganic rigid particles (RIGID Inorganic Filler, RIF for short) produces a stress concentration effect, which triggers the yield of the resin matrix around the particles (cavitation, silver streaks, shear bands). The yield of this matrix will absorb a large amount of deformation work, thereby producing toughness. At the same time, the presence of inorganic rigid particles can hinder the expansion of cracks or passivate and terminate cracks. The reason for hindering crack expansion is the pinning effect, which increases the resistance to crack expansion and consumes deformation work. The reason for particle passivation or crack termination is that the partial debonding of the two-phase interface forms cavitation, which passivates the cracks and prevents them from developing into destructive cracks. The use of RIF can improve the strength and rigidity of the material while improving toughness, without the disadvantage of reduced processing performance. This means that it is possible to obtain a low-cost composite material with good molding and processing performance from cheap raw materials.The toughening agent of the present invention adopts inorganic rigid particles and styrene-butadiene copolymer. The high molar content of butadiene in the styrene-butadiene copolymer (SBS) can better maintain or improve the impact strength of the system. In addition, a certain content of styrene can make SBS more compatible with PS, thereby enhancing the stability of the system.

[0022] In a preferred embodiment, the inorganic rigid particles are surface modified by the following method, including: drying the unmodified inorganic rigid particles, weighing the inorganic rigid particles after drying to a high-speed universal pulverizer, quickly introducing stearic acid dissolved in ethanol into the high-speed universal pulverizer, stirring for 3-8min, taking out 60-100°C for drying, sampling and saving to obtain the inorganic rigid particles; the mass ratio of stearic acid to the ethanol is 1:8-1:12. Specifically including, the inorganic rigid particles (RIF) are placed in an oven, dried at 100-120°C for 15-25h, weighing 40-60g to a high-speed universal pulverizer, weighing 0.2-2g stearic acid, dissolving it in ethanol with a mass ratio of stearic acid to ethanol of 1:8-1:12, dissolving it by ultrasonic at 40-60°C, quickly introducing it into a high-speed universal pulverizer, stirring for 3-8min, taking out 60-100°C for drying, and sampling and saving. This embodiment specifically defines the surface modification method of inorganic rigid particles because the organic layer coated on the surface of the inorganic rigid particles can enhance the wetting effect of the polymer melt on the rigid particles during the compounding process, reducing the tendency of the particles to aggregate. More importantly, stearic acid, as a surface modifier, can reduce the surface energy of the inorganic rigid particles, making the rigid particles better dispersed in the polymer matrix, reducing the interfacial adhesion between the dispersed phase and the polymer, thereby affecting the tensile and impact properties of the composite material.

[0023] In a preferred embodiment, the melt flow rate of the polystyrene is 2-25 g / 10 min, and the weight average molecular weight is 5×104-15×104; the polypropylene is a medium melt index polypropylene, with a melt flow rate of 10-20 g / 10 min and a notched cantilever beam impact strength of ≥20 kJ / ㎡. This embodiment specifically defines the properties of polystyrene and polypropylene because the medium melt index PP has good toughness, which can ensure the impact resistance, rigidity and fluidity of the composition.

[0024] In a preferred embodiment, the compatibilizer is polypropylene grafted maleic anhydride. This embodiment specifically limits the compatibilizer to polypropylene grafted maleic anhydride because polypropylene grafted maleic anhydride can utilize its polypropylene part to improve the compatibility of the compatibilizer and the polypropylene substrate, and utilize the part of maleic anhydride to reduce the surface tension between the components to improve the compatibility of the components.

[0025] In a preferred embodiment, an antioxidant, a lubricant, and a UV absorber are also included; by weight, the antioxidant is selected from any value in the range of 0.1-2.5 parts, the lubricant is selected from any value in the range of 0.1-0.5 parts, and the UV absorber is selected from any value in the range of 0-2.5 parts. This embodiment specifically defines the dosage of the antioxidant, lubricant, and UV absorber. It can be understood that the dosage of the antioxidant can also be 0.5, 1.0, 1.5, 2.0 parts and any point value within the range, the dosage of the lubricant can also be 0.2, 0.3, 0.4 parts and any point value within the range, and the dosage of the UV absorber can also be 0.5, 1.0, 1.5, 2.0 parts and any point value within the range.

[0026] In a preferred embodiment, the antioxidant is one or more of diphenylamine and its derivatives, p-phenylenediamine and its derivatives, 2,6-tert-butyl-4-methylphenol, bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide or phosphite; the lubricant is one or more of silicone oil, white mineral oil, barium stearate, magnesium stearate, paraffin, and ethylene bisstearamide; the UV absorber is a mixture of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0027] The present invention also provides a method for preparing the HIPS material described in any of the above technical solutions, comprising a raw material mixing step and a HIPS material preparation step. Figure 1 As shown, the HIPS material preparation step includes mixing the materials in a high-speed mixer, a twin-screw extruder, cooling, drying, and pelletizing. In a preferred embodiment, the raw material mixing step adopts high-speed mixing, the speed of the high-speed mixing and stirring is 700-1200r / min, and the mixing time is 5-10min; the HIPS material preparation step adopts twin-screw melt extrusion, cooling, drying and pelletizing to obtain the HIPS material, the extrusion temperature of the twin-screw melt extrusion is 180-210℃, the screw speed is 300-600r / min, the drying temperature is 65-115℃, and the drying time is 1-3h.

[0028] Another aspect of the present invention provides an appearance part, which is prepared from the HIPS material described in any of the above technical solutions. The appearance part not only meets the requirements of air conditioner appearance parts for toughness, strength and rigidity, but also has high glossiness and is lower in cost than ABS.

[0029] The present invention also provides an air conditioner, comprising the appearance part described in the above technical solution.

[0030] In order to more clearly and in detail introduce the HIPS material, preparation method, appearance part and air conditioner provided by the embodiments of the present invention, they will be described in combination with specific embodiments below.

[0031] Example 1

[0032] 1. Formula composition

[0033] By weight, it includes 70 parts of PS, 30 parts of PP, 5 parts of inorganic rigid particles, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted with maleic anhydride), 1 part of antioxidant (diphenylamine and its derivatives), 0.3 parts of lubricant (silicone oil), and 0.7 parts of UV absorber;

[0034] Among them, the inorganic rigid particles are surface modified by the following method, including: placing the inorganic rigid particles (RIF) in an oven, drying at 110°C for 20 hours, weighing 50g into a high-speed universal grinder, weighing 1g of stearic acid, dissolving it in ethanol with a mass ratio of stearic acid to ethanol of 1:10, dissolving it with ultrasound at 50°C, quickly introducing it into the high-speed universal grinder, stirring for 5 minutes, taking out and drying at 80°C, and sampling and storing.

[0035] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0036] 2. Preparation method

[0037] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0038] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0039] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0040] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0041] Example 2

[0042] 1. Formula composition

[0043] By weight, it includes 70 parts of PS, 40 parts of PP, 5 parts of inorganic rigid particles, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted with maleic anhydride), 1 part of antioxidant (p-phenylenediamine and its derivatives), 0.3 parts of lubricant (white mineral oil), and 0.7 parts of UV absorber;

[0044] Among them, the inorganic rigid particles are surface modified by the following method, including: placing the inorganic rigid particles (RIF) in an oven, drying at 110°C for 20 hours, weighing 50g into a high-speed universal grinder, weighing 0.2-2g of stearic acid, dissolving it in ethanol at a mass ratio of stearic acid to ethanol of 1:10, dissolving it by ultrasonic at 50°C, quickly introducing it into a high-speed universal grinder, stirring for 5 minutes, taking out and drying at 80°C, and sampling and storing.

[0045] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0046] 2. Preparation method

[0047] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0048] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0049] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0050] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0051] Example 3

[0052] 1. Formula composition

[0053] By weight, it includes 70 parts of PS, 20 parts of PP, 5 parts of inorganic rigid particles, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted maleic anhydride), 1 part of antioxidant (2,6-tert-butyl-4-methylphenol), 0.3 parts of lubricant (barium stearate), and 0.7 parts of UV absorber;

[0054] Among them, the inorganic rigid particles are surface modified by the following method, including: placing the inorganic rigid particles (RIF) in an oven, drying at 110°C for 20 hours, weighing 50g into a high-speed universal grinder, weighing 1g of stearic acid, dissolving it in ethanol with a mass ratio of stearic acid to ethanol of 1:10, dissolving it with ultrasound at 50°C, quickly introducing it into the high-speed universal grinder, stirring for 5 minutes, taking out and drying at 80°C, and sampling and storing.

[0055] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0056] 2. Preparation method

[0057] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0058] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0059] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0060] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0061] Example 4

[0062] 1. Formula composition

[0063] By weight, it includes 70 parts of PS, 30 parts of PP, 10 parts of inorganic rigid particles, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted maleic anhydride), 1 part of antioxidant (bis (3,5-tert-butyl-4-hydroxyphenyl) sulfide), 0.3 parts of lubricant (magnesium stearate), and 0.7 parts of UV absorber;

[0064] Among them, the inorganic rigid particles are surface modified by the following method, including: placing the inorganic rigid particles (RIF) in an oven, drying at 110°C for 20 hours, weighing 50g into a high-speed universal grinder, weighing 1g of stearic acid, dissolving it in ethanol with a mass ratio of stearic acid to ethanol of 1:10, dissolving it with ultrasound at 50°C, quickly introducing it into the high-speed universal grinder, stirring for 5 minutes, taking out and drying at 80°C, and sampling and storing.

[0065] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0066] 2. Preparation method

[0067] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0068] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0069] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0070] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0071] Example 5

[0072] 1. Formula composition

[0073] By weight, it includes 70 parts of PS, 30 parts of PP, 15 parts of inorganic rigid particles, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted maleic anhydride), 1 part of antioxidant (phosphite), 0.3 parts of lubricant (paraffin), and 0.7 parts of UV absorber;

[0074] Among them, the inorganic rigid particles are surface modified by the following method, including: placing the inorganic rigid particles (RIF) in an oven, drying at 110°C for 20 hours, weighing 50g into a high-speed universal grinder, weighing 1g of stearic acid, dissolving it in ethanol with a mass ratio of stearic acid to ethanol of 1:10, dissolving it with ultrasound at 50°C, quickly introducing it into the high-speed universal grinder, stirring for 5 minutes, taking out and drying at 80°C, and sampling and storing.

[0075] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0076] 2. Preparation method

[0077] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0078] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0079] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0080] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 5min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0081] Comparative Example 1

[0082] 1. Formula composition

[0083] By weight, it includes 70 parts of PS, 5 parts of inorganic rigid particles, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted with maleic anhydride), 1 part of antioxidant (diphenylamine and its derivatives), 0.3 parts of lubricant (ethylene bis stearamide), and 0.7 parts of UV absorber;

[0084] Among them, the inorganic rigid particles are surface modified by the following method, including: placing the inorganic rigid particles (RIF) in an oven, drying at 110°C for 20 hours, weighing 50g into a high-speed universal grinder, weighing 1g of stearic acid, dissolving it in ethanol with a mass ratio of stearic acid to ethanol of 1:10, dissolving it with ultrasound at 50°C, quickly introducing it into the high-speed universal grinder, stirring for 5 minutes, taking out and drying at 80°C, and sampling and storing.

[0085] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0086] 2. Preparation method

[0087] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0088] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0089] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0090] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0091] Comparative Example 2

[0092] 1. Formula composition

[0093] By weight, it includes 70 parts of PS, 30 parts of PP, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted maleic anhydride), 1 part of antioxidant (p-phenylenediamine and its derivatives), 0.3 parts of lubricant (silicone oil), and 0.7 parts of UV absorber;

[0094] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0095] 2. Preparation method

[0096] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0097] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0098] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0099] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0100] Comparative Example 3

[0101] 1. Formula composition

[0102] By weight, it includes 70 parts of PS, 30 parts of PP, 5 parts of inorganic rigid particles, 2 parts of compatibilizer (polypropylene grafted with maleic anhydride), 1 part of antioxidant (2,6-tert-butyl-4-methylphenol), 0.3 parts of lubricant (white mineral oil), and 0.7 parts of UV absorber;

[0103] Among them, the inorganic rigid particles are surface modified by the following method, including: placing the inorganic rigid particles (RIF) in an oven, drying at 110°C for 20 hours, weighing 50g into a high-speed universal grinder, weighing 1g of stearic acid, dissolving it in ethanol with a mass ratio of stearic acid to ethanol of 1:10, dissolving it with ultrasound at 50°C, quickly introducing it into the high-speed universal grinder, stirring for 5 minutes, taking out and drying at 80°C, and sampling and storing.

[0104] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0105] 2. Preparation method

[0106] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0107] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0108] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0109] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0110] Comparative Example 4

[0111] 1. Formula composition

[0112] By weight, it includes 70 parts of PS, 30 parts of PP, 5 parts of inorganic rigid particles without surface modification, 10 parts of SBS, 2 parts of compatibilizer (polypropylene grafted with maleic anhydride), 1 part of antioxidant (diphenylamine and its derivatives), 0.3 parts of lubricant (silicone oil), and 0.7 parts of UV absorber;

[0113] The UV absorber is a compound of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:1.

[0114] 2. Preparation method

[0115] A. Weigh and set aside according to the weight of PS resin, PP resin, toughening agent, compatibilizer, antioxidant, lubricant and UV absorber;

[0116] B. Mixing the components weighed in step A at high speed to obtain a mixture;

[0117] C. The mixture obtained in step B is subjected to twin-screw melt extrusion, cooling, drying and pelletizing to obtain a composite material.

[0118] In the above steps, in step B, the rotation speed of the high-speed mixing and stirring is 1000r / min, and the mixing time is 8min; in step C, the extrusion temperature of the twin-screw melt extrusion is 200°C, the screw speed is 500r / min, the drying temperature is 85°C, and the drying time is 2h.

[0119] Performance Testing

[0120] The test methods and standards are shown in Table 1, and the results are shown in Table 2.

[0121] Table 1 Test methods and standards

[0122] project Izod beam notched impact strength / kJ / ㎡ Tensile strength / MPa Flexural modulus / MPa Glossiness Test Standards GB / T 1843 GB / T1040.1 / 2 GB / T 9341 GB / T 8807 Test conditions Notch type A, impact energy 2.75J Tensile rate 50mm / min Bending rate 2mm / min 60° angle

[0123] Table 2 Examples and comparative test results

[0124] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Impact strength kJ / ㎡ 22 26 20 22 25 10 13 14 18 Tensile strength / MPa 26 31 23 28 29 28 24 22 25 Flexural modulus / MPa 2030 2240 1960 2050 2120 1800 1850 1750 1940 Glossiness 90 86 95 88 82 101 93 98 87

Claims

1. A HIPS material, characterized in that: including polystyrene, polypropylene, toughening agent, and compatibilizer; In parts by weight, the polystyrene is selected from any value in the range of 60-80 parts, the polypropylene is selected from any value in the range of 25-40 parts, the toughening agent is selected from any value in the range of 5-20 parts, and the compatibilizer is selected from any value in the range of 0.5-3 parts; The toughening agent comprises inorganic rigid particles and styrene-butadiene copolymer, and the weight ratio of the inorganic rigid particles to the styrene-butadiene copolymer is any value in the range of 1:2-2:1; The compatibilizer is selected from at least one of polypropylene grafted maleic anhydride, a silane coupling agent, an aluminate coupling agent and a titanate coupling agent; The inorganic rigid particles are surface modified by the following method, including: The unmodified inorganic rigid particles are dried, weighed and put into a high-speed universal grinder, stearic acid dissolved in ethanol is quickly introduced into the high-speed universal grinder, stirred for 3-8 minutes, taken out and dried at 60-100° C., and sampled and stored to obtain the inorganic rigid particles; the mass ratio of the stearic acid to the ethanol is any value in the range of 1:8-1:

12.

2. The HIPS material according to claim 1, characterized in that: The melt flow rate of the polystyrene is 2-25 g / 10 min, and the weight average molecular weight is 5×10 4 -15×10 4 ; The polypropylene is a medium melt index polypropylene with a melt flow rate of 10-20 g / 10 min and an Izod notched impact strength of ≥20 kJ / ㎡.

3. The HIPS material according to claim 1, characterized in that: The compatibilizer is polypropylene grafted with maleic anhydride.

4. The HIPS material according to claim 1, characterized in that: It also includes an antioxidant, a lubricant, and a UV absorber; in parts by weight, the antioxidant is selected from any value in the range of 0.1-2.5 parts, the lubricant is selected from any value in the range of 0.1-0.5 parts, and the UV absorber is selected from any value in the range of 0-2.5 parts.

5. The HIPS material according to claim 4, characterized in that: The antioxidant is one or more of diphenylamine and its derivatives, p-phenylenediamine and its derivatives, 2,6-tert-butyl-4-methylphenol, bis(3,5-tert-butyl-4-hydroxyphenyl)sulfide or phosphite; the lubricant is one or more of silicone oil, white mineral oil, barium stearate, magnesium stearate, paraffin, and ethylenebisstearamide; the UV absorber is a mixture of a benzotriazole UV absorber and a hindered amine light stabilizer, and the weight ratio of the benzotriazole UV absorber to the hindered amine light stabilizer is 1:

1.

6. The method for preparing the HIPS material according to any one of claims 1 to 5, characterized in that: The method comprises a raw material mixing step and a HIPS material preparation step.

7. The method for preparing the HIPS material according to claim 6, characterized in that: The raw material mixing step adopts high-speed mixing, the rotation speed of the high-speed mixing and stirring is 700-1200r / min, and the mixing time is 5-10min; the HIPS material preparation step adopts twin-screw melt extrusion, cooling, drying and pelletizing to obtain the HIPS material, the extrusion temperature of the twin-screw melt extrusion is 180-210°C, the screw speed is 300-600r / min, the drying temperature is 65-115°C, and the drying time is 1-3h.

8. An appearance part, characterized in that: The invention is prepared from the HIPS material according to any one of claims 1 to 5.

9. An air conditioner, characterized in that: The invention comprises the appearance part as claimed in claim 8.

Citation Information

Patent Citations

  • HIPS / PP (high impact polystyrene / polypropylene) alloy plastic with high gloss and excellent oil resistance and preparation method thereof

    CN106633455A