Al-Zn-Mg-Cu alloy material for lightweight structural parts and preparation method thereof

By adjusting the composition and heat treatment process of the Al-Zn-Mg-Cu alloy, the problem that the alloy is difficult to possess multiple excellent properties at the same time is solved, and the comprehensive performance improvement of high strength, corrosion resistance and low quenching sensitivity is achieved, which is suitable for aerospace and aerospace applications. Manufacturing of transportation equipment.

CN116179907BActive Publication Date: 2024-10-25UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211433753.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-10-25
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

It is difficult for existing Al-Zn-Mg-Cu alloys to possess the comprehensive properties of high strength and toughness, high corrosion resistance, fatigue resistance, low quenching sensitivity and high electrical conductivity at the same time. The addition of alloy elements and preparation methods cannot work together, especially reducing the Quenching sensitivity affects strength and corrosion resistance.

Method used

By adjusting the content ranges of Zn, Mg and Cu, the chemical equivalent balance of the alloy in the α (Al) phase solid solution zone is ensured, and the Cu content is controlled at a reasonable level to improve fracture toughness and stress corrosion performance, while using heat treatment and deformation processing technology. , such as T6 peak aging, T74 state treatment, combined with solid solution quenching and natural aging processes, to prepare high-performance Al-Zn-Mg-Cu alloy.

Benefits of technology

Developed a high-performance Al-Zn-Mg-Cu alloy with strength equal to or higher than AA7081 aluminum alloy. It has excellent corrosion resistance and low quenching sensitivity. The elongation and fracture toughness are significantly improved. It is suitable for manufacturing lightweight and high-strength Components of aerospace and transportation equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116179907B_ABST
    Figure CN116179907B_ABST
Patent Text Reader

Abstract

The present invention discloses an Al-Zn-Mg-Cu alloy material and a preparation method for lightweight structural parts, belonging to the technical field of Al-Zn-Mg-Cu alloy material and preparation. The components in the alloy material are calculated by mass percentage: Zn: 6.7-8.2, Mg: 2.0-2.5, Cu: 1.8-2.6, Zr: 0.01-0.2, Fe: ≤0.3, Si: ≤0.25, Mn: ≤0.2, Cr: ≤0.2, Ti: ≤0.15, other elements ≤0.05, and the rest are Al. The aluminum alloy material developed by the present invention has the properties of high toughness, high corrosion resistance, fatigue resistance, low quenching sensitivity, high electrical conductivity, etc., and the addition of alloy elements and the preparation method can work well together; it can be used to manufacture plates / profiles of different sizes and specifications to meet the manufacturing and application requirements of lightweight and high-strength components required for aerospace aircraft and transportation equipment manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of Al-Zn-Mg-Cu alloy materials and preparation thereof, and relates to an Al-Zn-Mg-Cu alloy material for lightweight structural parts and a preparation method thereof. Background Art

[0002] Al-Zn-Mg-Cu alloys have low density, high strength and toughness, excellent corrosion resistance and fatigue resistance, and are widely used in the manufacture of key load-bearing components such as aerospace and automobiles. Typical aluminum alloys such as AA7075, AA7050, AA7055, AA7449, and AA7085 are used to manufacture wings, beams, frames, and anti-collision parts. At present, the damage tolerance of some high-strength Al-Zn-Mg-Cu alloys (such as fracture toughness, stress corrosion cracking (SCC) and fatigue performance) is still insufficient, which seriously restricts the long-term, stable and safe service of key load-bearing components. Aluminum alloys such as AA7050, AA7010, and AA7040 (medium and low Zn content) used for the manufacture of thick-gauge components such as wing beams and ribs usually have medium quenching sensitivity, which can ensure uniform performance in the thickness direction within a certain thickness, but their strength level, damage tolerance and corrosion resistance still need to be optimized and improved.

[0003] In the prior art, the low-Zn AA7150 aluminum alloy and the high-Zn AA7055 and AA7449 aluminum alloys have high strength and are mainly used for aircraft wing panels, but their fracture toughness and corrosion resistance are only acceptable under current service conditions. The medium-Zn AA7085 and AA7081 aluminum alloys have low quenching sensitivity and high damage tolerance, and are used to manufacture integral wing beam structures, thereby replacing traditional assembled wing beam structures, which is conducive to reducing structural weight and saving costs, but the relatively low Mg and Cu content makes their strength level not high. It can be seen that based on the composition range of aluminum alloys such as AA7X50, AA7X55, AA7449, AA7085 and AA7081 and their organizational performance characteristics, the development of Al-Zn-Mg-Cu alloy materials with better comprehensive properties such as high strength and toughness, high corrosion resistance and fatigue resistance is a key technical guarantee for the development of ultra-high-speed, high-energy-efficiency, high-safety and reliability aerospace aircraft and transportation equipment.

[0004] In Al-Zn-Mg-Cu alloys, the main alloying elements Zn and Mg can form different forms of metastable MgZn2 strengthening phases and significantly strengthen the alloy matrix. Therefore, high Zn and high Mg content help to obtain higher strength, but will reduce or deteriorate other properties, such as fracture toughness and stress corrosion cracking performance. The addition of Cu elements will affect the precipitation or transformation process of MgZn2 phase and its metastable phase, and then affect the strength, plasticity, toughness and corrosion resistance of Al-Zn-Mg-Cu alloys. At present, high-performance Al-Zn-Mg-Cu alloys show a development trend of high Zn, high Zn:Mg ratio, and medium / high Cu content. The key to obtaining high aging strengthening effect is that the alloying elements can be completely dissolved in the aluminum matrix after solid solution treatment. However, high alloying content usually forms coarse and refractory intermetallic compounds, such as Al7Cu2Fe, S-Al2CuMg, etc., which will consume a certain amount of Mg and Cu alloying elements and affect the aging strengthening effect. Moreover, such intermetallic compound phases are often easy to become the source of loading or corrosion failure.

[0005] Among them: Chinese patent CN113481416A discloses a high-performance Al-Zn-Mg-Cu alloy, in which the Cu content and Mg content in the composition selection are low, the prepared plate is thicker, and the fracture toughness and elongation of the obtained plate cannot be improved synergistically. Other synergistic properties based on this, such as high corrosion resistance, fatigue resistance, low quenching sensitivity, and high electrical conductivity, are not considered.

[0006] Chinese patent CN112981196A discloses an ultra-high strength, high toughness Al-Zn-Mg-Cu aluminum alloy and a preparation method thereof. The high Zn content and low Cu content in the composition selection, combined with the preparation method selection, will result in the failure to synergistically improve the fracture toughness and elongation of the alloy's comprehensive properties. Other synergistic properties based on this, such as high corrosion resistance, fatigue resistance, low quenching sensitivity, and high electrical conductivity, are not considered.

[0007] Therefore, the development of high-performance Al-Zn-Mg-Cu alloys with high strength and toughness and excellent corrosion resistance faces great technical difficulties. In addition, the quenching sensitivity of medium and thick plates / profiles is also an important factor affecting the use of such alloys in the manufacture of large key components, especially products with strict quenching sensitivity requirements often use relatively low alloying levels. Summary of the invention

[0008] The technical problem to be solved by the present invention is how to overcome the problem that the Al-Zn-Mg-Cu alloy in the prior art cannot simultaneously have the properties of high strength and toughness, high corrosion resistance, fatigue resistance, low quenching sensitivity, high conductivity, etc., and the addition of alloy elements and the preparation method cannot work well together. In particular, although the addition of some alloy elements can reduce the quenching sensitivity, it will also reduce the strength and / or corrosion resistance.

[0009] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0010] An Al-Zn-Mg-Cu alloy material for lightweight structural parts, wherein the components of the Al-Zn-Mg-Cu alloy material are as follows by mass percentage: Zn: 6.7-8.2, Mg: 2.0-2.5, Cu: 1.8-2.6, Zr: 0.01-0.2, Fe: ≤0.3, Si: ≤0.25, Mn: ≤0.2, Cr: ≤0.2, Ti: ≤0.15, and other elements ≤0.0 5, and the rest is Al; wherein the total weight of (Zn+Mg+Cu) is 11.0-13.2wt.%, the total weight of (Cu+Mg) is 3.9-4.7wt.%, the weight ratio of Zn:Mg is 2.7-4.1, the weight ratio of (Zn+Cu):Mg is 3.6-5.2, the weight ratio of Cu:Mg is 0.75-1.30, and 1.15+0.37Cu≤Mg≤1.71+0.37Cu is satisfied.

[0011] Preferably, the other elements are Ag, Sc, Er, Hf, Ni, and Co.

[0012] Preferably, the T6 peak aged tensile strength of the hot-rolled Al-Zn-Mg-Cu alloy material plate at a 1 / 4 thickness position along the rolling direction (L direction) is not less than 570 MPa, the yield strength is not less than 490 MPa, and the elongation is not less than 14.0%; the T6 peak aged tensile strength of the hot-rolled Al-Zn-Mg-Cu alloy material plate at a 1 / 4 thickness position perpendicular to the rolling direction (LT) is not less than 560 MPa, the yield strength is not less than 480 MPa, and the elongation is not less than 8.0%.

[0013] Preferably, the T74 tensile strength of the hot-rolled Al-Zn-Mg-Cu alloy material plate along the rolling direction (L direction) at a 1 / 4 thickness position is not less than 500 MPa, the yield strength is not less than 440 MPa, and the elongation is not less than 11.0%; the T74 tensile strength of the hot-rolled Al-Zn-Mg-Cu alloy material plate along the rolling direction (L direction) at a 1 / 4 thickness position is not less than 480 MPa, the yield strength is not less than 430 MPa, and the elongation is not less than 5.4%.

[0014] Preferably, the Al-Zn-Mg-Cu alloy material has a fracture toughness in the LT direction of not less than 37.0 MPa·mm after heat treatment by T74 process. 1 / 2 , fracture toughness in TL direction is not less than 26.5MPa·mm 1 / 2, the exfoliation corrosion grade is not less than EB, and the electrical conductivity is not less than 40.0% IACS; the L-direction elongation, LT-direction fracture toughness and electrical conductivity of the Al-Zn-Mg-Cu alloy material after T74 process heat treatment are greater than those of AA7449, AA7081 and AA7050 aluminum alloys.

[0015] Preferably, the tensile strength of the Al-Zn-Mg-Cu alloy material hot-rolled plate in the natural aging state at 1 / 4 thickness position along the rolling direction (L direction) is not less than 535 MPa, the yield strength is not less than 380 MPa, the elongation is not less than 20.0%, the strain hardening coefficient n value is not less than 0.160, and the plastic strain ratio r value is not less than 0.60; the tensile strength of the Al-Zn-Mg-Cu alloy material hot-rolled plate in the simulated baking paint state at 1 / 4 thickness position along the rolling direction (L direction) is not less than 560 MPa, the yield strength is not less than 500 MPa, and the elongation is not less than 13.0%; and the difference in yield strength between the natural aging state and the simulated baking paint state is equivalent to or better than that of AA7050 and AA6016 aluminum alloys; the calculated strain hardening coefficient n value and plastic strain ratio r value of the Al-Zn-Mg-Cu alloy material in the natural aging state are close to or equivalent to those of AA7075, AA7050 and AA6016 alloys (thin plates).

[0016] The preparation method of the Al-Zn-Mg-Cu alloy material for lightweight structural parts comprises the following steps:

[0017] S1. Weighing the raw materials according to the alloy components of the Al-Zn-Mg-Cu alloy material to obtain weighed raw materials;

[0018] S2, melting the raw materials weighed in step S1, controlling the melt temperature at 730-780°C, stirring the alloy melt after melting to achieve full melting, then adding a refining agent and a refiner, refining, slagging and standing the melt, and casting at 690-725°C to obtain an alloy ingot;

[0019] S3, performing homogenization treatment and surface peeling treatment on the alloy ingot obtained in step S2 to obtain a semi-finished alloy ingot;

[0020] S4, performing hot / warm deformation processing on the semi-finished alloy ingot obtained in step S3 to obtain alloy plates or profiles of required specifications or shapes;

[0021] S5. Performing solid solution treatment, quenching and artificial aging treatment on the alloy plate or profile obtained in step S4 to obtain a high-strength, high-toughness, corrosion-resistant aluminum alloy plate / profile.

[0022] Preferably, in step S3, the homogenization treatment adopts a single-stage, double-stage or three-stage heat treatment system, wherein the single-stage heat treatment process is: 465-480°C insulation for 3-72h, the double-stage heat treatment process is: 400-460°C insulation for 5-96h + 460-490°C insulation for 3-72h, and the three-stage heat treatment process is: 250-420°C insulation for 10-96h + 420-470°C insulation for 3-72h + 470-490°C insulation for 3-72h.

[0023] Preferably, the hot / warm deformation processing in step S4 is: the alloy ingot is kept at 150-460°C for 1-24 hours and then subjected to multiple hot / warm deformations (such as rolling or forging), with a total deformation amount of 50-99% and a deformation amount of 3-30% each time. The hot / warm deformation blank can be further subjected to solution quenching or annealing and heat preservation and then continuously deformed, with a total deformation amount of 50-99% and a deformation amount of 10-50% each time.

[0024] Preferably, the solution treatment system in step S4 is 460-500°C for 0.1-5h, and the transfer time from solution treatment to room temperature water quenching is 0.1-5min; the annealing treatment system is 200-450°C for 0.1-48h, and deformation processing can be performed without cooling after annealing until the final size specification.

[0025] Preferably, in step S5, the solution treatment can adopt a single-stage or multi-stage solution treatment process, wherein the single-stage solution treatment process is 450-496°C insulation for 0.1-15h, the double-stage solution treatment process is: 440-460°C insulation for 1-15h + 460-496°C insulation for 0.1-10h, the three-stage solution treatment process is: 380-430°C insulation for 1-5h + 430-460°C insulation for 1-10h + 460-500°C insulation for 0.1-10h, and the transfer time from solution to room temperature water quenching is 0.5-30min.

[0026] Preferably, in step S5, the artificial aging heat treatment adopts T6 peak aging or T7X over-aging treatment system.

[0027] Preferably, in step S5, the T6 peak aging process is: 115-130°C for 18-30h; the T7X over-aging treatment system includes a two-stage or three-stage treatment process such as T73 (51), T74 (51), T76 (51), T77 (51) or T79 (51), wherein the T73 heat treatment system is 115-128°C / 6-10h+155-168°C / 20-36h, and the T74 heat treatment system is 115-128°C / 3-6h+155- 168℃ / 24~30h, T76 heat treatment system is 115~128℃ / 3~6h+155~168℃ / 12~24h, T77 heat treatment system is 110~128℃ / 12~24h+185~220℃ / 5~60min+110~128℃ / 12~24h, T79 heat treatment system is 115~128℃ / 3~6h+150~168℃ / 12~18h, among which, (51) indicates pre-stretching of 1%~3% before aging.

[0028] Preferably, the preparation method further includes step S6, performing solid solution treatment, pre-aging, natural aging and baking varnish treatment on the plate or profile obtained in step S4 to obtain a high-strength aluminum alloy material with good formability and high baking varnish hardening ability.

[0029] Preferably, in the above step S6, the solution treatment system is 460-500°C for 0.1-3h, and the transfer time from solution treatment to room temperature water quenching is 1-5min; the pre-aging temperature range is 80-130°C, and the pre-aging time is 20-240min; the natural aging treatment system is -10-30°C ambient temperature for 1 day to 6 months; the paint treatment system is 170-200°C for 10-40min.

[0030] The alloy composition of the present invention involves the principle:

[0031] The main technical approaches to ensure that Al-Zn-Mg-Cu alloys have excellent comprehensive properties include: (1) controlling the content of the main alloy components below the solubility limit, which is beneficial to improving the fracture toughness and damage tolerance, and the strength value is relatively high within a certain range of the α (Al) phase solid solution zone near the solid solubility line; (2) a high Zn:Mg ratio is beneficial to improving SCC and quenching sensitivity; (3) maintaining chemical equivalence between different main alloy components, and controlling the Cu content at a reasonable level to improve fracture toughness and SCC performance. The performance of the existing typical Al-Zn-Mg-Cu alloys is analyzed and compared based on the distribution range of Cu and Mg contents of different alloys, the solubility limits obtained by thermodynamic calculation, and the chemical equivalent equilibrium intervals of different components. It is found that the Mg and Cu contents of aluminum alloys such as AA7050, AA7010, and AA7040 (Zn content of 5.7-6.7wt.%) with medium and low Zn contents are quite different, but the strength of the three alloys is equivalent. The difference is that the fracture toughness and damage tolerance of AA7050 aluminum alloy are both low, while those of AA7010 and AA7040 aluminum alloys are higher; the SCC performance of AA7050 aluminum alloy is at a medium level, the SCC performance of AA7010 aluminum alloy is low, and the SCC performance of AA7040 aluminum alloy is high; the Zn content (7.6-8.4wt.%) of AA7055 aluminum alloy is higher than that of AA7050 aluminum alloy, and the Mg content is reduced , while the Cu content remains unchanged, so its strength increases, SCC performance is better, and fracture toughness and damage tolerance are improved; the Zn content of AA7081 and AA7085 aluminum alloys is higher than that of AA7050 aluminum alloy, while the Mg and Cu contents are reduced, so their strength increases, fracture toughness and damage tolerance are also significantly improved, and SCC performance is equivalent (AA7081) or better (AA7085), and the high Zn:Mg ratio and low Cu content make it have lower quenching sensitivity; the Zn, Mg and Cu contents of AA7136 aluminum alloy are higher than those of AA7081 aluminum alloy, resulting in a significant increase in its strength, but a decrease in fracture toughness, damage tolerance and SCC resistance; compared with AA7136 aluminum alloy, the Zn and Cu contents of AA7449 aluminum alloy are reduced, and the Mg content is increased, so its strength is low, but the fracture toughness and damage tolerance are better, and the SCC performance is also better.

[0032] Based on the above analysis and in combination with the typical alloy composition range and the corresponding performance advantages and disadvantages, in order to further improve the mechanical properties of Al-Zn-Mg-Cu alloys, the present invention proposes the following alloy composition design ideas: (1) The Zn content is maintained at a medium level, which is significantly higher than that of AA7050 aluminum alloy and is close to or equivalent to AA7449, AA7055, AA7085 and AA7081 aluminum alloys; (2) The Mg content is at a medium / high level, which is significantly higher than that of AA7085 and AA7081 aluminum alloys and is equivalent to AA7050 aluminum alloy; (3) The Cu content is at a medium / high level, which is significantly higher than that of AA7085 and AA7081 aluminum alloys and is close to or higher than that of AA7050 aluminum alloy.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] In the above scheme, the present invention develops a high-performance Al-Zn-Mg-Cu alloy material with a strength equivalent to or higher than that of commonly used high-strength aluminum alloys, a toughness equivalent to or higher than that of AA7081 aluminum alloy, and excellent corrosion resistance by regulating the contents of Zn, Mg and Cu and combining relevant preparation methods.

[0035] The Al-Zn-Mg-Cu alloy material developed by the present invention has good formability and high paint hardening ability after being treated by solid solution quenching, pre-aging, natural aging and simulated paint baking.

[0036] The Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 573±14.2MPa, a yield strength of not less than 496±9.2MPa, and an elongation of not less than 14.1±0.5% at a 1 / 4 thickness position of a tested hot-rolled plate after T6 peak aging heat treatment, and a tensile strength of not less than 565±2.3MPa, a yield strength of not less than 487±1.1MPa, and an elongation of not less than 8.5±4.5% at a 1 / 4 thickness position of a tested hot-rolled plate after T6 peak aging heat treatment.

[0037] The Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 501±3.2MPa, a yield strength of not less than 443±2.7MPa, and an elongation of not less than 11.0±0.5% at a 1 / 4 thickness position of a tested hot-rolled plate after T74 process heat treatment; the tensile strength of the Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 487±4.8MPa, a yield strength of not less than 432±1.1MPa, and an elongation of not less than 5.4±1.0% at a 1 / 4 thickness position of a tested hot-rolled plate after T74 process heat treatment perpendicular to the rolling direction (LT).

[0038] The Al-Zn-Mg-Cu alloy material developed by the present invention has a fracture toughness in the LT direction of not less than 38.2±1.65MPa·mm after heat treatment by T74 process. 1 / 2 , fracture toughness in TL direction is not less than 29.5±1.48MPa·mm 1 / 2 , the exfoliation corrosion grade is not lower than EB, and the electrical conductivity is not less than 41.5% IACS; the L-direction elongation, LT-direction fracture toughness and electrical conductivity of the Al-Zn-Mg-Cu alloy material after T74 process heat treatment are greater than those of AA7449, AA7081 and AA7050 aluminum alloys.

[0039] The Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 539±3.7MPa, a yield strength of not less than 383±4.0MPa, an elongation of not less than 21.1±0.6%, a strain hardening coefficient n value of not less than 0.167±0.002, and a plastic strain ratio r value of not less than 0.62±0.01 after a test hot-rolled plate of the Al-Zn-Mg-Cu alloy material treated with simulated baking varnish, and a tensile strength of not less than 568±7.2 MPa, the yield strength is not less than 507±8.5MPa, and the elongation is not less than 14.6±1.0%; and the difference in yield strength between the hot-rolled plate tested after natural aging treatment and the hot-rolled plate tested after simulated baking paint treatment is less than the difference in yield strength between the hot-rolled plate tested after natural aging treatment and the hot-rolled plate tested after simulated baking paint treatment of AA7050; the calculated strain hardening coefficient n value and the plastic strain ratio r value of the Al-Zn-Mg-Cu alloy material in the natural aging state are slightly lower than those of AA7075 and AA6016 alloys (thin plates); but are close to or equivalent to those of AA7050 alloy.

[0040] In summary, the high-performance Al-Zn-Mg-Cu alloy material developed by the present invention can simultaneously have the properties of high strength and toughness, high corrosion resistance, fatigue resistance, low quenching sensitivity, high electrical conductivity, etc., and the addition of alloy elements and the preparation method can work well together; it can be used to manufacture plates / profiles of different sizes and specifications to meet the manufacturing and application needs of lightweight and high-strength components required for the manufacture of aerospace vehicles and transportation equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0042] Figure 1 The main alloy element composition distribution of an Al-Zn-Mg-Cu alloy material for a lightweight structural part provided by the present invention and a comparative alloy in the prior art; wherein: FIG a indicates the Zn-Mg composition distribution of the alloy in the present invention and the prior art, FIG b indicates the Zn-Cu composition distribution of the alloy in the present invention and the prior art, and FIG c indicates the Cu-Mg composition distribution of the alloy in the present invention and the comparative alloy;

[0043] Figures a and b simultaneously mark the composition distribution of the current classic high-strength Al-Zn-Mg-Cu alloys (AA7050, AA7055, AA7085, AA7081, AA7449, etc.) and the alloys involved in the relevant patents [US20200232072A1] and [US20080283163A1], as well as the Al-Zn-Mg-Cu alloy material for lightweight structural parts of the present invention and the comparative alloy; Figure c approximates the solubility limit (490°C) corresponding to a Zn content of 6.7wt.% based on the phase diagram calculation;

[0044] Figure 2 The strength-toughness distribution of the Al-Zn-Mg-Cu alloy material for lightweight structural parts of the present invention and the comparative alloy;

[0045] Figure 3 The Al-Zn-Mg-Cu alloy material for lightweight structural parts of the present invention, comparative alloys and the strength-toughness distribution of alloys involved in patents and literatures thereof. DETAILED DESCRIPTION

[0046] The following will describe the technical solutions and technical problems solved in the embodiments of the present invention in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.

[0047] Example 1

[0048] An Al-Zn-Mg-Cu alloy material for lightweight structural parts, wherein the components of the Al-Zn-Mg-Cu alloy material are as follows by mass percentage: Zn: 6.7-8.2, Mg: 2.0-2.5, Cu: 1.8-2.6, Zr: 0.01-0.2, Fe: ≤0.3, Si: ≤0.25, Mn: ≤0.2, Cr: ≤0.2, Ti: ≤0.15, and other elements ≤0.0 5, and the rest is Al; wherein the total weight of (Zn+Mg+Cu) is 11.0-13.2wt.%, the total weight of (Cu+Mg) is 3.9-4.7wt.%, the weight ratio of Zn:Mg is 2.7-4.1, the weight ratio of (Zn+Cu):Mg is 3.6-5.2, the weight ratio of Cu:Mg is 0.75-1.30, and 1.15+0.37Cu≤Mg≤1.71+0.37Cu is satisfied. The alloy materials that meet the composition requirements of the present invention are alloys #1-7 in Table 1, #8 is a high-Zn, high-Cu alloy with (Zn+Mg+Cu)wt.%=13.35, and its Zn content is close to the upper limit of the Zn content of the alloy of the present invention (8.2wt.%), and #9 is a low-Zn, high-Cu alloy with (Zn+Mg+Cu)wt.%=11.54, and its Zn content is lower than the lower limit of the Zn content of the alloy of the present invention (6.7wt.%), and the Cu content of the two alloys exceeds the upper limit of the Cu content of the alloy of the present invention (2.6wt.%).

[0049] The main alloy element composition distribution of the Al-Zn-Mg-Cu alloy material for lightweight structural parts provided by the present invention and the comparative alloy in the prior art is as follows: Figure 1 shown; through Figure 1 Figures a and b clearly show the differences in the distribution of the main alloy elements. Figure c approximates the solubility limit (490°C) corresponding to a Zn content of 6.7wt.% based on the phase diagram.

[0050] Table 1 Composition of alloy of Example 1 (wt.%)

[0051] Alloy No. Is it the alloy of the present invention? Zn Mg Cu Zr Ti Fe Si Al 1 yes 7.20 2.21 1.83 0.09 ≤0.1 ≤0.25 ≤0.2 ≥95.32 2 yes 7.27 2.19 2.05 0.093 ≤0.1 ≤0.25 ≤0.2 ≥95.12 3 yes 7.30 2.32 2.06 0.096 ≤0.1 ≤0.25 ≤0.2 ≥94.97 4 yes 7.20 2.11 2.58 0.098 ≤0.1 ≤0.25 ≤0.2 ≥94.66 5 yes 6.86 2.17 2.07 0.100 ≤0.1 ≤0.25 ≤0.2 ≥95.11 6 yes 7.34 2.37 1.94 0.087 ≤0.1 ≤0.25 ≤0.2 ≥95.15 7 yes 7.68 2.38 2.26 0.082 ≤0.1 ≤0.25 ≤0.2 ≥94.73 8 no 8.15 2.36 2.84 0.089 ≤0.1 ≤0.25 ≤0.2 ≥94.16 9 no 6.50 2.15 2.89 0.100 ≤0.1 ≤0.25 ≤0.2 ≥94.31

[0052] Note 1: Zr content is about 0.01-0.2wt.%;

[0053] The preparation method of Al-Zn-Mg-Cu alloy material comprises the following steps:

[0054] S1. Weigh the raw materials according to the alloy composition of 1-9#Al-Zn-Mg-Cu alloy material as described in Table 1 to obtain weighed raw materials;

[0055] S2, dissolving the raw materials weighed in step S1, controlling the melt temperature at 730-780°C, stirring the alloy melt after dissolution to achieve full melting, then adding a refining agent and a refiner, refining, slagging and standing the melt, and casting at 690-725°C to obtain an alloy ingot;

[0056] S3, performing homogenization annealing treatment on the alloy ingot obtained in step S2, wherein the homogenization annealing may adopt a three-stage heat treatment system, wherein the three-stage heat treatment process is: 420° C. insulation for 10 h + 470° C. insulation for 12 h + 480° C. insulation for 24 h, followed by air cooling, removing the homogenization annealing ingot skin, and obtaining a semi-finished alloy ingot;

[0057] S4, heating the semi-finished alloy ingot obtained in step S3 until the temperature rises to 430° C. and preheating for 3 hours, and then performing multiple hot rolling at 430° C. to obtain a plate with a thickness of about 20 mm;

[0058] S5. The alloy plate or profile obtained in step S4 is subjected to a two-stage solution treatment at 445°C / 2h+475°C / 2h, followed by immediate room temperature water quenching, and then subjected to T6 and T74 artificial aging treatments, respectively, wherein the T6 heat treatment process is 120°C / 24h, and the T74 heat treatment process is 120°C / 6h+163°C / 24h, to obtain a high-strength, high-toughness, corrosion-resistant aluminum alloy plate.

[0059] The tensile properties of the prepared high-strength, high-toughness, corrosion-resistant aluminum alloy plate refer to ASTM E8-2016 to test the room temperature tensile mechanical properties of the rolled plate at 1 / 4 thickness along the rolling direction (L direction) and perpendicular to the rolling direction (LT), including yield strength, tensile strength and elongation; as shown in Table 2:

[0060] Table 2 Tensile properties of alloys in Example (UTS = tensile strength, TYS = yield strength, δ = elongation)

[0061]

[0062] According to ASTM E399-20a standard, compact tensile C (T) specimens were used to test the fracture toughness of T74 alloy in LT and TL directions. Test process: (1) Prefabricate a fatigue crack of a certain length; (2) Open side grooves (10% depth each) along the thickness B of the specimen; (3) Stretch until breaking and obtain the displacement-load curve; (4) According to the formula specified in the standard, calculate the critical stress intensity factor K that directly characterizes the fracture toughness of the material Qsi (5) According to the standard, calculate and verify whether the test meets the validity conditions. If it does, the critical stress intensity factor K Isi =K QsiIf it is not satisfied, the sample size needs to be further adjusted and retested. Isi Different from K which is more sensitive to sample size Ic The value is obtained according to the linear elastic, surface strain fracture toughness calculation method for size insensitivity specified in standard ASTM E399-20a. Isi The value is calculated based on a constant crack extension (0.5 mm apparent crack extension), while K Ic The value is the crack growth based on a percentage of a constant initial crack size. K Isi The calculation process of K Ic The values ​​remain the same, but the validity conditions are different, K Isi The following conditions must be met: Isi / TYS) 2 <12.7mm. The alloys prepared by the present invention all meet the validity condition. For the alloy materials processed in the same batch, K Isi The larger the value, the more difficult it is for the crack to propagate, that is, the higher the fracture toughness. The fracture toughness, exfoliation corrosion grade and electrical conductivity of 1-9#Al-Zn-Mg-Cu alloy sheet are shown in Table 3.

[0063] Table 3 Fracture toughness (K Isi ), exfoliation corrosion grade (EXCO) and electrical conductivity (EC Ave. )

[0064]

[0065] Note: The anti-exfoliation corrosion performance is tested according to ASTM G34-13 standard.

[0066] From the performance test results in Table 2 and Table 3, it can be seen that in the T6 / T74 state, the 1-7# alloys of the present invention have excellent comprehensive properties in different directions, namely high strength, high toughness, and good corrosion resistance. All the invention alloys in the T74 state have a yield strength in the L direction of >440MPa, an elongation of ≥11%, and a fracture toughness in the LT direction of ≥38.2MPa·mm 1 / 2 . Both are higher than the minimum strength and fracture toughness of AA7050-T74 specified in AMS4050J (441MPa and 32MPa·mm 1 / 2 ). In this embodiment, all alloys are subjected to the same deformation processing and heat treatment process, and the main difference lies in the different contents of Zn, Mg and Cu elements.

[0067] It can be found from this embodiment that the strength of the alloy increases with the increase of Mg content, while the fracture toughness tends to decrease, that is, the Mg content significantly affects the strength and fracture toughness of the alloy. For example, the Mg content of 3# alloy, 6# alloy, 7# alloy and 8# alloy is higher than 2.3wt.%, and its T74 state yield strength (>465MPa) is higher than that of 1# alloy, 2# alloy, 4# alloy and 5# alloy (Mg<2.2wt.%), and the strength of the alloy tends to increase with the increase of Mg content. When the Mg and Cu contents are close, the higher the Zn content, the higher the strength. For example, the Zn content of 2# alloy is higher, and its strength is slightly higher than that of 5# alloy. Adding Cu can accelerate aging precipitation, that is, promote the nucleation and formation of nanoscale aging precipitation phase, which is beneficial to increase the content of aging precipitation phase. At the same time, adding a certain amount of Cu can also play a solid solution strengthening effect. However, high Cu content will lead to more coarse and refractory intermetallic compound phases, such as S-Al2CuMg phase, remaining in the alloy, which will consume part of Mg and Cu solute atoms, resulting in a decrease in the content of effective precipitation strengthening phase and a weakening of the total strengthening effect. In addition, the residual coarse S-Al2CuMg phase is prone to cause stress concentration, which is unfavorable to the strength, plasticity and toughness of the alloy. For example, the Zn and Mg contents of alloy 1#, alloy 2# and alloy 4# are similar, and the Cu content increases successively, but the strength of the three decreases successively. However, the strength, elongation, fracture toughness, corrosion resistance and stress corrosion cracking resistance of alloy 8# are relatively well matched. On the one hand, the alloy has relatively high Mg and Zn contents, which is conducive to obtaining a higher content of effective precipitation strengthening phase. On the other hand, although its Cu content is very high, the higher Zn and Mg contents will consume part of the Cu atoms when forming an effective precipitation strengthening phase (such as Mg(ZnAlCu)2 precipitation phase), and at the same time, part of the Cu atoms will be dissolved in the matrix (solid solution strengthening), thereby reducing the residual coarse Cu-rich phase. Calculations show that the main alloying elements Zn, Mg and Cu of the 8# alloy are basically balanced in stoichiometric numbers, so the fracture toughness of the 8# alloy is at a relatively high level. However, the equilibrium phase diagram calculation shows that the 8# alloy is in the (α+S) two-phase region, which is higher than the solubility limit. Therefore, compared with the medium / low Cu alloys with the same Zn and Mg content (such as the 10# alloy in Example 2), the strength, plasticity and fracture toughness of the 8# alloy are reduced. Considering the cost of high alloying (especially high Cu content), the alloy does not have practical application advantages. The Mg content of the 9# alloy is at a medium level, the Zn content is low, and the Cu content is high. Its precipitated phase content is low, and the more residual coarse Cu-rich phases cause its strength and toughness to decrease.

[0068] In this embodiment, alloy 1# has the lowest Cu content. Under appropriate heat treatment process, the coarse S-Al2CuMg phase can be completely dissolved back into the aluminum matrix, and the Zn and Mg contents are at a medium level, so the fracture toughness of the alloy is the highest. The composition and fracture properties of alloy 6# are similar to those of alloy 1#; the Cu content in alloy 5# is moderate, and there are a few coarse S-Al2CuMg phases, but the Zn content is low, and the Mg content is close to that of other alloys, and the fracture toughness of the alloy remains at a high level; the Zn and Cu contents of alloy 7# are increased to varying degrees, the microstructure and properties are well balanced, and the strength and toughness are maintained well; compared with alloy 1#, the Cu and / or Mg contents in alloys 2#, 3# and 4# are increased, while the Zn content remains unchanged, resulting in more coarse S-Al2CuMg phases remaining in the alloys, and thus the fracture toughness is reduced. The elongation, fracture toughness, corrosion resistance and stress corrosion cracking resistance of 4# alloy are acceptable, but due to its high Cu content and slightly reduced Mg content, more coarse S-Al2CuMg phase and a small amount of θ-Al2Cu phase remain, and the strength level is reduced, but still acceptable, and the overall performance remains basically balanced.

[0069] From the examples, the fracture toughness is obviously affected by the changes in the content of the main alloy components (Zn, Mg and Cu). When the Zn content is at a medium and low level and the Cu and Mg contents are high, the residual coarse S-Al2CuMg phase is not conducive to fracture toughness; when the Cu content is at a medium and low level and the Mg and Zn contents are high, the volume fraction, size and distribution state of the precipitated phases at the grain boundary and in the grain are the main influencing factors of fracture toughness; when the Zn, Mg and Cu contents are all high, multiple mechanisms jointly dominate the fracture process of the alloy. In addition, the grain structure (grain size and degree of recrystallization) also affects the fracture toughness of the alloy.

[0070] In this example, the difference in fracture toughness in the LT direction of alloys with different compositions is not significant, but the toughness in the TL direction of some alloys is still significantly different. This is because the coarse second phase particles in the hot-rolled plate are distributed in a band-like manner at the grain boundary along the rolling direction, which is extremely unfavorable to the fracture toughness of the alloy, resulting in some alloys showing obvious performance anisotropy.

[0071] From the examples, the alloys of the present invention can be divided into three categories: (1) when the Zn content is medium, the Mg content is high and the Cu content is low, the alloy strength and toughness (especially toughness) are better (such as 1# alloy and 6# alloy); (2) when the Cu content is high and the Zn and Mg contents are at medium levels, the alloy strength remains unchanged or increases, the toughness decreases, but the strength and toughness match is still good (such as 2# alloy, 3# alloy and 5# alloy); (3) when the Cu content is high and the Zn and Mg contents are at medium levels or both increase, the alloy strength is acceptable or increases, and the toughness decreases slightly (such as 4# alloy). As a comparative alloy, the strength, corrosion resistance and stress corrosion cracking resistance of alloy 9# are acceptable, but its Cu and Mg contents are both high (especially Cu content), and its Zn content is low, resulting in a significant decrease in its elongation and fracture toughness.

[0072] To ensure that the alloy has excellent toughness, especially for low Zn alloys, high Cu and Mg contents should be avoided, wherein the Cu content does not exceed 2.6wt.%, and preferably does not exceed 2.4wt.%, and the more preferred upper limit is 2.2wt.%; the Mg content does not exceed 2.5wt.%. The contents of Cu and Mg components must be carefully designed or reasonably matched, and preferably both are at the same low level, or the Mg content is moderate and the Cu content is low.

[0073] Example 2

[0074] The performance differences between the alloy of the present invention and the commercial high-strength and high-toughness Al-Zn-Mg-Cu alloy were compared. Taking the 1# alloy, 6# alloy and 10# alloy of the present invention as examples, alloy plates with the components listed in Table 4 were prepared using the process consistent with Comparative Example 1.

[0075] In Table 4, the compositions of alloys 1#, 6# and 10# are within the range of the alloy compositions of the present invention, alloy 11# is AA7449 aluminum alloy, alloy 12# is AA7081 aluminum alloy, and alloy 13# is AA7050 aluminum alloy specified in AMS 4050J. The mechanical properties of the above alloys are shown in Table 5, wherein alloy 13# gives the corresponding minimum mechanical property values. As can be seen from Table 5, compared with AA7081 (12# alloy) and AA7050 (13# alloy) aluminum alloys, the composition of alloy 1# is close to that of alloy 12#, and its Zn content is higher than that of AA7050, its Mg content is comparable, and its Cu content is lower. The fracture toughness obtained is improved relative to that of alloy 12#, which is much higher than the minimum value of AA7050 aluminum alloy (13# alloy). The Zn, Mg and Cu contents of 6# alloy are all increased compared with 1# alloy. Its strength is slightly higher than 1# alloy and lower than AA7449 aluminum alloy (11# alloy), but its fracture toughness is improved to a certain extent (compared with 11# alloy, 12# alloy and 13# alloy). Compared with AA7050 (13# alloy), the Zn content increases and the Cu content decreases. The strength is higher than AA7050, and the toughness is also significantly improved. The strength of 10# alloy is slightly lower than AA7449 (11# alloy), but higher than AA7081 (12# alloy) and AA7050 (13# alloy). Its strength, toughness and elongation are better. Although the Cu content of AA7449 aluminum alloy (11# alloy) is low, its Zn and Mg contents are high, so its strength is the highest, resulting in relatively low elongation and fracture toughness. In summary, the higher the Mg content, the higher the alloy strength, but too high Mg content will significantly reduce the elongation and fracture toughness; the fracture toughness of low Cu and medium / low Mg alloys is generally better. Generally, when the content of Zn is high, Cu is low and Mg content is above medium, the alloy has better comprehensive properties. In addition, compared with the strength and toughness of AA7050-T74 aluminum alloy in the literature, it is found that Figure 2 and 3 As shown, the invented alloy has a better combination of strength and toughness: the strength or fracture toughness is equivalent to or higher than that of the existing alloy (AA7081), and the fracture toughness is higher than that of AA7050 and AA7449 alloys; the comprehensive performance is better than that of AA7081 alloy (12# alloy), and has better performance balance.

[0076] The alloy of the present invention further enriches the composition range of Al-Zn-Mg-Cu alloys, and can improve the single or comprehensive properties (strength, toughness and elongation) of the alloys to varying degrees. The matching design of strength, toughness and elongation of the alloy of the present invention can meet the performance requirements of high strength, high toughness or high strength and toughness and excellent elongation, providing more possibilities for the selection of lightweight key structural parts.

[0077] Table 4 Composition of Example Alloys (wt.%)

[0078]

[0079] Table 5 Performance of Example Alloy T74

[0080]

[0081] Note: Alloy 13# is AA7050 aluminum alloy, corresponding to the minimum values ​​of various properties of T74 state specified by AMS 4050J in Table 5.

[0082] In addition, the exfoliation corrosion ratings of the alloys of the present invention are all at EB level or above, and the electrical conductivity that can characterize the alloy's stress corrosion resistance is also relatively high (all greater than 40% IACS), indicating that the alloys of the present invention have excellent corrosion resistance.

[0083] In summary, the alloy of the present invention has excellent comprehensive properties of high strength, high toughness and corrosion resistance.

[0084] Example 3

[0085] In order to broaden the application possibilities of the Al-Zn-Mg-Cu alloy of the present invention, three Al-Zn-Mg-Cu alloys 1#, 7# and 10# were selected, and the alloy thin plates with a thickness of 2.5 mm were prepared by combining the method described in the patents [ZL 201410223778.9, CN 111705274 A]. The specific preparation process is as follows:

[0086] Step 1, casting three kinds of Al-Zn-Mg-Cu alloy ingots 1#, 7# and 10# of the present invention. The ingot is homogenized at 420°C for 10 hours, then heated to 470°C and kept warm for 12 hours, then heated to 480°C and kept warm for 24 hours, and then air-cooled. After homogenization, the ingot is descaled and heated to 430°C and kept warm for about 3 hours, and then hot-rolled at 430°C through multiple passes to a thickness of about 20 mm. Then, the 20 mm thick hot-rolled plate is solution treated at 475°C / 2h and then water-quenched, then cold-rolled to ~10 mm (deformation is ~50%), immediately heated to 380°C and kept warm for 30 to 40 minutes, then taken out of the furnace without cooling and immediately continuously rolled to a final thickness of ~2.5 mm (the plate is not returned to the furnace for heating during this process).

[0087] Step 2, subjecting the thin plate obtained in step 1 to a solution treatment at 475±3°C / 30min in a salt bath furnace, followed by immediate water quenching at room temperature;

[0088] Step 3, immediately subjecting the plate obtained in step 2 to a pre-aging treatment at 100±1°C / 30min;

[0089] Step 4, isothermally treating the thin plate obtained in step 3 at room temperature for 14 days (i.e., natural aging treatment);

[0090] Step 5, subjecting the plate obtained in step 4 to a simulated paint baking treatment at 180±1°C / 30min.

[0091] The room temperature tensile properties of the alloy plates in the natural aging state (100℃ / 30min+14 days of room temperature natural aging), simulated baking paint state (100℃ / 30min+14 days of room temperature natural aging+180℃ / 30min) and T6 state were tested (including tensile strength (σ b ), yield strength (σ s ), elongation (δ), and the strain hardening coefficient n and plastic strain ratio r were calculated at the same time. The results are listed in Table 6.

[0092] Table 6 Tensile properties of example alloys under different heat treatment conditions

[0093]

[0094]

[0095] Note: [1] CN 111705274 A—A processing method for Al-Zn-Mg-(Cu) alloy material

[0096] Table 6 shows that the room temperature tensile elongation of the three invented aluminum alloy sheets after natural aging is greater than 21.0%, which is higher than the naturally aged AA7050 aluminum alloy (18.4%), close to AA7075 (22.9%) and AA6111 aluminum alloy (~22.0%), but its strength is higher than the comparative alloys (AA7075, AA7050 and AA6111). After the simulated baking paint treatment, the yield strength increment of the three invented aluminum alloys reaches ~120MPa, which is better than the baking paint increment of the car body aluminum plates such as AA6016 and AA6111 (about 70~80MPa), and is equivalent to the comparative alloys AA7075 (121MPa) and AA7050 (127MPa). The tensile data shows that the yield strength of the simulated baking paint state of alloy 1# (522MPa) is close to the T6 state (545MPa), and the elongation is equivalent. In addition, the calculated strain hardening coefficient n value and plastic strain ratio r value of the three aluminum alloy materials of the present invention after pretreatment and natural aging treatment are slightly lower than those of AA7075 and AA6016 alloys (thin plates); but are close to or equivalent to those of AA7050 alloy.

[0097] It can be seen that the formability of the alloy sheet of the present invention is slightly lower than that of the naturally aged AA6016 and AA7075 alloys, and is equivalent to that of the AA7050 alloy. After natural aging treatment, it has good plastic deformation or forming ability and better paint hardening ability, and is suitable for manufacturing high-strength vehicle structural parts (such as anti-collision parts) that require baking treatment.

[0098] In the above scheme, the present invention develops a high-performance Al-Zn-Mg-Cu alloy material with a strength equivalent to or higher than that of commonly used high-strength aluminum alloys, a toughness equivalent to or higher than that of AA7081 aluminum alloy, and excellent corrosion resistance by regulating the contents of Zn, Mg and Cu and combining relevant preparation methods.

[0099] The Al-Zn-Mg-Cu alloy material developed by the present invention has good formability and high paint hardening ability after being treated by solid solution quenching, pre-aging, natural aging and simulated paint baking.

[0100] The Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 573±14.2MPa, a yield strength of not less than 496±9.2MPa, and an elongation of not less than 14.1±0.5% at a 1 / 4 thickness position of a tested hot-rolled plate after T6 peak aging heat treatment, and a tensile strength of not less than 565±2.3MPa, a yield strength of not less than 487±1.1MPa, and an elongation of not less than 8.5±4.5% at a 1 / 4 thickness position of a tested hot-rolled plate after T6 peak aging heat treatment.

[0101] The Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 501±3.2MPa, a yield strength of not less than 443±2.7MPa, and an elongation of not less than 11.0±0.5% at a 1 / 4 thickness position of a tested hot-rolled plate after T74 process heat treatment; the tensile strength of the Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 487±4.8MPa, a yield strength of not less than 432±1.1MPa, and an elongation of not less than 5.4±1.0% at a 1 / 4 thickness position of a tested hot-rolled plate after T74 process heat treatment perpendicular to the rolling direction (LT).

[0102] The Al-Zn-Mg-Cu alloy material developed by the present invention has a fracture toughness in the LT direction of not less than 38.2±1.65MPa·mm after heat treatment by T74 process. 1 / 2 , fracture toughness in TL direction is not less than 29.5±1.48MPa·mm 1 / 2 , the exfoliation corrosion grade is not lower than EB, and the electrical conductivity is not less than 41.5% IACS; the L-direction elongation, LT-direction fracture toughness and electrical conductivity of the Al-Zn-Mg-Cu alloy material after T74 process heat treatment are greater than those of AA7449, AA7081 and AA7050 aluminum alloys.

[0103] The Al-Zn-Mg-Cu alloy material developed by the present invention has a tensile strength of not less than 539±3.7MPa, a yield strength of not less than 383±4.0MPa, an elongation of not less than 21.1±0.6%, a strain hardening coefficient n value of not less than 0.167±0.002, and a plastic strain ratio r value of not less than 0.62±0.01 after a test hot-rolled plate of the Al-Zn-Mg-Cu alloy material treated with simulated baking varnish, and a tensile strength of not less than 568±7.2 MPa, the yield strength is not less than 507±8.5MPa, and the elongation is not less than 14.6±1.0%; and the difference in yield strength between the hot-rolled plate tested after natural aging treatment and the hot-rolled plate tested after simulated baking paint treatment is less than the difference in yield strength between the hot-rolled plate tested after natural aging treatment and the hot-rolled plate tested after simulated baking paint treatment of AA7050; the calculated strain hardening coefficient n value and the plastic strain ratio r value of the Al-Zn-Mg-Cu alloy material in the natural aging state are slightly lower than those of AA7075 and AA6016 alloys (thin plates); but are close to or equivalent to those of AA7050 alloy.

[0104] In summary, the high-performance Al-Zn-Mg-Cu alloy material developed by the present invention can simultaneously have the properties of high strength and toughness, high corrosion resistance, fatigue resistance, low quenching sensitivity, high electrical conductivity, etc., and the addition of alloy elements and the preparation method can work well together; it can be used to manufacture plates / profiles of different sizes and specifications to meet the manufacturing and application needs of lightweight and high-strength components required for the manufacture of aerospace vehicles and transportation equipment.

[0105] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An Al-Zn-Mg-Cu alloy material for lightweight structural parts, characterized in that: The components of the Al-Zn-Mg-Cu alloy material are as follows by mass percentage: Zn: 6.7-8.2, Mg: 2.11-2.5, Cu: 1.8-2.6, Zr: 0.01-0.2, Fe: ≤0.3, Si: ≤0.25, Mn: ≤0.2, Cr: ≤0.2, Ti: ≤0.15, other elements ≤0.05, and the rest is Al; wherein (Zn+Mg+Cu ) total weight is 11.0-13.2wt.%, (Cu+Mg) total weight is 3.9-4.7wt.%, Zn:Mg weight ratio is 2.7-(7.20 / 2.11), (Zn+Cu):Mg weight ratio is 3.6-(9.78 / 2.11), Cu:Mg weight ratio is 0.75-1.30, and satisfies 1.15+0.37Cu≤Mg≤1.71+0.37Cu; The other elements are Ag, Sc, Er, Hf, Ni, and Co; The Al-Zn-Mg-Cu alloy hot-rolled plate has a T6 peak aging state tensile strength at a 1 / 4 thickness position along the rolling direction (L direction) of not less than 570 MPa, a yield strength of not less than 490 MPa, and an elongation of not less than 14.0%; the Al-Zn-Mg-Cu alloy hot-rolled plate has a T6 peak aging state tensile strength at a 1 / 4 thickness position perpendicular to the rolling direction (LT) of not less than 560 MPa, a yield strength of not less than 480 MPa, and an elongation of not less than 8.0%; The method for preparing the Al-Zn-Mg-Cu alloy material for lightweight structural parts comprises the following steps: S1. Weighing the raw materials according to the alloy components of the Al-Zn-Mg-Cu alloy material to obtain weighed raw materials; S2, melting the raw materials weighed in step S1, controlling the melt temperature at 730-780°C, stirring the alloy melt after melting to achieve full melting, then adding a refining agent and a refiner, refining, slagging and standing the melt, and casting at 690-725°C to obtain an alloy ingot; S3, performing homogenization treatment and surface peeling treatment on the alloy ingot obtained in step S2 to obtain a semi-finished alloy ingot; S4, performing hot / warm deformation processing on the semi-finished alloy ingot obtained in step S3 to obtain alloy plates or profiles of required specifications or shapes; S5, performing solid solution treatment, quenching and artificial aging treatment on the alloy plate or profile obtained in step S4 to obtain a high-strength, high-toughness, corrosion-resistant aluminum alloy plate / profile; In step S3, the homogenization treatment adopts a single-stage, double-stage or three-stage heat treatment system, wherein the single-stage heat treatment process is: 465-480°C insulation for 3-72h, the double-stage heat treatment process is: 400-460°C insulation for 5-96h + 460-490°C insulation for 3-72h, and the three-stage heat treatment process is: 250-420°C insulation for 10-96h + 420-470°C insulation for 3-72h + 470-490°C insulation for 3-72h; The hot / warm deformation processing in step S4 is as follows: the alloy ingot is kept at 150-460°C for 1-24 hours and then subjected to multiple hot / warm deformations, wherein the multiple hot / warm deformations are rolling or forging, with a total deformation amount of 50-99% and a deformation amount of 3-30% each time; the hot / warm deformation blank is subjected to solution quenching or annealing and then continuously deformed, with a total deformation amount of 50-99% and a deformation amount of 10-50% each time; The solution treatment system in step S4 is 460-500°C for 0.1-5h, and the transfer time from solution treatment to room temperature water quenching is 0.1-5min; the annealing treatment system is 200-450°C for 0.1-48h, and deformation processing can be performed without cooling after annealing until the final size specification.

2. The Al-Zn-Mg-Cu alloy material for lightweight structural parts according to claim 1, characterized in that: The Al-Zn-Mg-Cu alloy hot-rolled plate has a T74 tensile strength of not less than 500 MPa, a yield strength of not less than 440 MPa, and an elongation of not less than 11.0% at a 1 / 4 thickness position along the rolling direction (L direction).

3. The Al-Zn-Mg-Cu alloy material for lightweight structural parts according to claim 1, characterized in that: The Al-Zn-Mg-Cu alloy material has a fracture toughness in the LT direction of not less than 37.0 MPa·mm after heat treatment by T74 process. 1 / 2 , fracture toughness in TL direction is not less than 26.5MPa·mm 1 / 2 , the exfoliation corrosion grade is not less than EB, and the electrical conductivity is not less than 40.0% IACS; the L-direction elongation, LT-direction fracture toughness and electrical conductivity of the Al-Zn-Mg-Cu alloy material after T74 process heat treatment are greater than those of AA7449, AA7081 and AA7050 aluminum alloys.

4. The Al-Zn-Mg-Cu alloy material for lightweight structural parts according to claim 1, characterized in that: The tensile strength of the Al-Zn-Mg-Cu alloy material hot-rolled plate in the natural aging state at a 1 / 4 thickness position along the rolling direction (L direction) is not less than 535 MPa, the yield strength is not less than 380 MPa, the elongation is not less than 20.0%, the strain hardening coefficient n value is not less than 0.160, and the plastic strain ratio r value is not less than 0.60; the tensile strength of the Al-Zn-Mg-Cu alloy material hot-rolled plate in the simulated baking paint state at a 1 / 4 thickness position along the rolling direction (L direction) is not less than 560 MPa, the yield strength is not less than 500 MPa, and the elongation is not less than 13.0%; and the difference in yield strength between the natural aging state and the simulated baking paint state is equivalent to or better than that of AA7050 and AA6016 aluminum alloys; the calculated strain hardening coefficient n value and plastic strain ratio r value of the Al-Zn-Mg-Cu alloy material in the natural aging state are close to or equivalent to those of AA7075, AA7050 and AA6016 alloy sheets.