A method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity
By doping La element and using lithium stearate, the preparation process of titanium-based lithium adsorbent is improved, which solves the problems of manganese element dissolution and insufficient adsorbent performance in the existing technology, and achieves high specific surface area and high adsorption capacity. The titanium-based lithium adsorbent improves the migration rate and adsorption performance of lithium ions, simplifies the process and is suitable for industrial applications.
Patent Information
- Application Number
- CN202310055634.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-20
AI Technical Summary
Existing titanium-based lithium adsorbents suffer from manganese element price changes during the adsorption cycle, resulting in dissolution loss, complicated processes, and the specific surface area and particle size issues of the adsorbents have not been effectively improved, resulting in slow lithium ion adsorption and desorption rates, affecting applications.
By dryly mixing the lithium source, lanthanum salt and titanium source, pouring them into the polyvinyl alcohol aqueous solution, stirring, beating and drying, and performing two-stage heating and calcination. The La element is doped to expand the lattice spacing and generate vacancies. Lithium stearate is used. Used as a lithium source to inhibit grain agglomeration and form a lithium metatitanate adsorbent with high specific surface area, small size and high adsorption capacity.
It improves the adsorption capacity and adsorption performance of the titanium-based lithium adsorbent, increases the migration rate of lithium ions, simplifies the preparation process, increases the specific surface area and yield of the product, is easy to industrialize, and is environmentally friendly.
Smart Images

Figure CN116199256B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity, belonging to the technical field of lithium adsorbent preparation. Background Art
[0002] Lithium resources mainly exist in seawater, salt lake brine and granite pegmatite deposits, of which 80% exist mainly in the form of liquid lithium resources, distributed in large salt lake brines around the world.
[0003] In recent years, metallic lithium and its compounds have been widely used in defense, energy, batteries, glass, metallurgy and other fields due to their excellent physical and chemical properties. Faced with the rapid growth of lithium demand, it is particularly necessary to seek an efficient and stable method for extracting lithium. So far, the methods and technologies for extracting lithium from lithium ore have been quite mature, but at the same time, this method also has many shortcomings, such as high cost, complex process, high energy consumption, etc., so salt lake brine and seawater are selected as the source of Li element. The reserves of liquid lithium resources are far greater than the lithium resources consumed by human life and development every year. The impact of obtaining lithium resources from seawater or salt lake brine on global liquid lithium resources is minimal. In short, seawater and salt lake brine can become an inexhaustible treasure trove of lithium resources.
[0004] The ion exchange method is a method of obtaining lithium ions from brine using ion exchange adsorbents. It has the advantages of low energy consumption, economy, and environmental protection. This method is considered to be one of the most promising methods for extracting lithium from brine. Among them, lithium ion sieve adsorbents are the key in the ion exchange method and are also a research hotspot for recovering lithium from salt lake brines. For lithium ion sieve adsorbents, the two most studied so far are manganese lithium oxide ion sieves and titanium lithium oxide ion sieves. Manganese-based ion sieves have the advantages of abundant raw materials, low price, high lithium selectivity, and large adsorption capacity. However, during the adsorption cycle, due to the change in the valence of the manganese element, Mn is produced. 2+ , and Mn 2+ It is easily soluble in acid, resulting in excessive manganese loss.
[0005] CN110215935A discloses a method for preparing a powder-type high-capacity titanium-based lithium ion exchanger. The adsorbent precursor synthesis process is not doped with metal elements, and thus exhibits a good adsorption capacity. However, the raw material processing stage has many processes, complicated operations, and needs to be processed with different solutions. The adsorbent precursor obtained in the end does not significantly improve the specific surface area and particle size problems. CN109174068A discloses a metatitanate-type lithium adsorbent and a method for preparing the same, which does not improve the specific surface area of the adsorbent and the adsorbent fails to fully function.
[0006] Titanium-based lithium ion sieves are mainly divided into spinel structure H4T i5O 12There are two types of H2TiO3: H2TiO3 and layered structure. The layered structure H2TiO3 ion sieve has a higher theoretical lithium ion adsorption capacity. However, the mass transfer channels of H2TiO3 are narrow, and the migration rate of lithium ions inside the adsorbent is slow, resulting in slow lithium ion adsorption and desorption rates, which greatly affects its application. Summary of the invention
[0007] In order to overcome the deficiencies of the prior art, the present invention provides a method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity.
[0008] A method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity comprises the following steps: dry-mixing a lithium source, a lanthanum salt and a titanium source, pouring them into a polyvinyl alcohol aqueous solution, stirring, slurrying and drying, entering a first stage of heating and calcining, and then entering a second stage of heating and calcining to obtain a precursor for acidification to obtain an adsorbent.
[0009] A method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity is achieved through the following principle: lithium metatitanate with high specific surface area, small size and high adsorption capacity is prepared by doping La elements into the Li2TiO3 lattice to replace part of the Ti element, and has a large radius and low-valent metal ion doping to increase the interplanar spacing and generate vacancies, which is beneficial to expand the internal diffusion channel and increase the internal and external diffusion rate of the adsorbent, thereby improving the adsorption performance of the adsorbent.
[0010] The La element replaces the Ti position, which can effectively inhibit the agglomeration phenomenon that occurs during the crystal growth process, which is beneficial to improve the microporous structure of the adsorbent, reduce the particle size and increase the specific surface area, thereby improving the Li + migration rate.
[0011] By using lithium stearate as a lithium source, because it is an organic salt, it can also play a role in inhibiting grain agglomeration during the preparation process, and the combustion and decomposition of organic matter can form pores, so that the layered lithium titanate has a larger specific surface area.
[0012] By dispersing the raw materials in a polyvinyl alcohol solution, the gel formed after drying can play the role of pore formation and inhibit agglomeration during the crystallization process, further increase its specific surface area, reduce the particle size, thereby opening channels and increasing mass transfer rate, which is beneficial to the Li + adsorption and desorption.
[0013] The advantage of the present invention is that the adsorption capacity of the titanium-based lithium adsorbent is improved. Since the actual adsorption capacity of the titanium-based lithium adsorbent prepared by the prior art is far less than its theoretical value, the lithium source is replaced with lithium stearate, and the lithium adsorbent precursor is prepared into a product with high specific surface area, small size and high adsorption capacity by other means.
[0014] The present invention proposes an adsorption material Li2Lax T i (1-x) O3, doping La in lithium metatitanate is beneficial to expand the internal diffusion channel, increase the internal and external diffusion rate of the adsorbent, and thus improve the adsorption performance of the adsorbent. By using lithium stearate as a lithium source, because it is an organic salt, it can also inhibit the agglomeration of grains during the preparation process, and the combustion and decomposition of organic matter can form pores, so that the layered lithium metatitanate has a larger specific surface area. The raw materials are dispersed in a polyvinyl alcohol solution, and the gel formed after drying can also serve the purpose of forming pores and inhibiting agglomeration during the crystallization process, further increasing its specific surface area and reducing the particle size, thereby opening the channel and increasing the mass transfer rate, which is beneficial to Li + adsorption and desorption.
[0015] The synthesis process of the lithium titanate adsorbent with high specific surface area, small size and high adsorption capacity proposed by the present invention is simple to operate, easy to control, high in yield, environmentally friendly, and easy to recycle, and easy to realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] When considered in conjunction with the accompanying drawings, the present invention can be more completely and better understood and many of the accompanying advantages can be easily known by referring to the detailed description below, but the drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention, as shown in the figure:
[0017] Figure 1 It is a flow chart of the present invention.
[0018] Figure 2 is the Li2La of the present invention 0.01 T i 0.99 XRD pattern of O3.
[0019] Figure 3a is the Li2La of the present invention 0.01 T i 0.99 O3 SEM image.
[0020] Figure 3b is the Li2La of the present invention 0.01 T i 0.99 O3 mapping diagram.
[0021] Figure 3c is the Li2La of the present invention 0.01 T i 0.99 O3 energy spectrum.
[0022] Figure 4 H2La of the present invention 0.01 T i 0.99Trend graph of adsorption capacity of O3.
[0023] Figure 5 is the Li2La of the present invention 0.05 T i 0.95 XRD pattern of O3.
[0024] Figure 6a is the Li2La of the present invention 0.05 T i 0.95 SEM image of O3.
[0025] Figure 6b is the Li2La of the present invention 0.05 T i 0.95 O3’s mapping diagram.
[0026] Figure 6c is the Li2La of the present invention 0.05 T i 0.95 Energy spectrum of O3.
[0027] Figure 7 H2La of the present invention 0.05 T i 0.95 Trend graph of adsorption capacity of O3.
[0028] Figure 8 is the Li2La of the present invention 0.08 T i 0.92 XRD pattern of O3.
[0029] Figure 9a is the Li2La of the present invention 0.08 T i 0.92 O3 SEM image.
[0030] Figure 9b is the Li2La of the present invention 0.08 T i 0.92 O3 mapping diagram.
[0031] Fig.9c is the Li2La of the present invention 0.08 T i 0.92 O3 energy spectrum.
[0032] Fig.10 H2La of the present invention 0.08 T i 0.92 Trend graph of adsorption capacity of O3.
[0033] Fig.11 is the Li2La of the present invention 0.1 T i 0.9 XRD pattern of O3.
[0034] Fig.12a Li2La of the present invention 0.1 T i 0.9 SEM image of O3.
[0035] Figure 12b Li2La of the present invention 0.1 T i 0.9 Mapping diagram of O3.
[0036] Fig.12c Li2La of the present invention 0.1 T i 0.9 Energy spectrum of O3.
[0037] Fig.13 H2La of the present invention 0.1 T i 0.99 Trend graph of adsorption capacity of O3. DETAILED DESCRIPTION
[0038] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0039] Obviously, many modifications and changes made by those skilled in the art based on the purpose of the present invention belong to the protection scope of the present invention.
[0040] It will be understood by those skilled in the art that, unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art.
[0041] To facilitate understanding of the embodiments, further explanations will be given below, and each embodiment does not constitute a limitation on the embodiments.
[0042] Example 1: Figure 1 , Figure 2 , Figure 3a , Figure 3b , Figure 3c , Figure 4 , Figure 5 , Figure 6a , Figure 6b , Figure 6c , Figure 7 , Figure 8 , Figure 9a , Figure 9b , Fig.9c , Fig.10 , Fig.11 , Fig.12a , Figure 12b , Fig.12c and Fig.13As shown, a method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity is used to open the diffusion channel of the adsorbent so as to increase its adsorption capacity in brine. The precursor Li2La is formed by doping La in the Li2TiO3 lattice. x Ti (1-x) O3, where the value of x ranges from 0.01 to 0.1.
[0043] A method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity comprises the following steps: dry-mixing a lithium source, a lanthanum salt and a titanium source using a pulverizer or a ball mill, pouring them into a polyvinyl alcohol aqueous solution, stirring, slurrying and drying, entering a first stage of heating and calcining, and then entering a second stage of heating and calcining to obtain a precursor for acidification to obtain an adsorbent.
[0044] The specific steps include:
[0045] First, a lithium source, a lanthanum salt for doping, and a titanium source are dry-mixed in a molar ratio of Li:La:Ti=2.1-2.5:0.01-0.1:0.99-0.9 for 1-2 hours, wherein the lithium source is lithium stearate (Li C 18 H 35 O2), the lanthanum salt is lanthanum carbonate (La2(CO3)3·8H2O), and the titanium source is metatitanic acid (H2T i O3).
[0046] The dry mixing method is a pulverizer mixing or a ball mill mixing or a combination of the two.
[0047] Then pour the mixed material into polyvinyl alcohol aqueous solution (5%-10%) and stir for 3-6 hours to obtain sol, with a solid-liquid content of 1 kg solid to 1-2 kg liquid. Then use a drying device to dry at 185-200°C for 6-10 hours to obtain a gel.
[0048] The gel was transferred into a muffle furnace for the first stage of heating and calcination at a rate of 2-10°C / min to 550-650°C for 4-8h, and then the second stage of heating was increased to 700-900°C for 4-8h to obtain Li2La with high specific surface area, small size and high adsorption capacity. x T i (1-x) O3 precursor.
[0049] Soak it in 0.01-0.1 mol acid solution for 10-20 hours to acidify the Li + Replaced to obtain lithium adsorbent H2La x T i (1-x) O3, wherein the acid solution is hydrochloric acid or sulfuric acid.
[0050] The obtained lithium adsorbent was then subjected to an adsorption capacity test. The test brine parameters were: 1L of ultrapure water containing lithium carbonate (1.60g), sodium bicarbonate (7.61g), anhydrous sodium sulfate (10.58g), anhydrous sodium carbonate (11.86g), and sodium chloride (78.31g). The feed ratio during the test was 10g / L.
[0051] Example 2: Figure 1 , Figure 2 , Figure 3a , Figure 3b , Figure 3c , Figure 4 , Figure 5 , Figure 6a , Figure 6b , Figure 6c , Figure 7 , Figure 8 , Figure 9a , Figure 9b , Fig.9c , Fig.10 , Fig.11 , Fig.12a , Figure 12b , Fig.12c and Fig.13 As shown, a method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity includes the following steps for preparing a lithium metatitanate adsorbent:
[0052] The lithium source, lanthanum salt and titanium source were mixed in a molar ratio of 2.1:0.01:0.99, that is, 304.93g of lithium stearate (analytical grade), 3.01g of La2(CO3)3·8H2O (analytical grade) and 48.45g (chemically pure) of titanic acid were dry mixed with a high-speed grinder for 1h, poured into 356.39g of an aqueous solution with a polyvinyl alcohol content of 5% at a solid-liquid ratio of 1:1, and then stirred with a stirrer for 3h to obtain a sol, and then dried in an oven at 185°C for 6h to obtain a gel, and then the gel was transferred to a muffle furnace for programmed temperature calcination at a heating rate of 2°C / min. First, it was heated to 550°C and calcined for 4h, then heated to 700°C and calcined for 4h, cooled, and ground to obtain the adsorbent precursor Li2La 0.01 T i 0.99 O3. Then use 0.01mol HCl to acidify it, add 100g of adsorbent precursor into 4L of acid solution, and when the pH value rises, continue to add hydrochloric acid to ensure that its concentration is 0.01mol, then change the acid solution twice, and finally the pH does not change, the acidification is completed, a total of 20h, and wash to obtain H2La 0.01 T i 0.99 O3.Li2La 0.01 T i 0.99 XRD of O3 Figure 2Its microstructure and element distribution are shown in Figure 3. Table 1 Li2La 0.01 Ti 0.99 Atomic content ratio of each element in O3.
[0053] Table 1 Li2La 0.01 T i 0.99 Atomic content of O3
[0054] element Atomic Percent O 81.49 Ti 18.23 La 0.28 Total 100
[0055] Contains material adsorption test steps:
[0056] The H2La obtained above 0.01 T i 0.99 10g of O3 adsorbent was added to the test brine. The adsorbent had an effect on Li + The changes in adsorption capacity are as follows Figure 4 As shown in Table 2, the adsorption capacity after 3 hours is 20.32 mg / g, and the adsorption capacity after 96 hours is 65.19 mg / g. From the adsorption trend, it can be observed that the adsorption rate is high in the first 3 hours, and after 24 hours, the adsorption rate tends to be flat. After 7 cycles of adsorption, as shown in Table 2, the adsorption capacity after 96 hours in the 7th cycle is 61.85 mg / g, and the adsorption performance is still good.
[0057] Table 2H2La 0.01 T i 0.99 Adsorption performance of O3 after 7 cycles
[0058]
[0059] Example 3: Figure 1 , Figure 2 , Figure 3a , Figure 3b , Figure 3c , Figure 4 , Figure 5 , Figure 6a , Figure 6b , Figure 6c , Figure 7 , Figure 8 , Figure 9a , Figure 9b , Fig.9c , Fig.10 , Fig.11 , Fig.12a , Figure 12b , Fig.12c and Fig.13 As shown, a method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity includes the following steps for preparing a lithium metatitanate adsorbent:
[0060] The lithium source, lanthanum salt and titanium source were mixed in a molar ratio of 2.2:0.05:0.95, that is, 511.12g of lithium stearate (analytical grade), 24.08g of La2(CO3)3·8H2O (analytical grade) and 74.39g (chemically pure) of titanic acid were dry mixed with a high-speed grinder for 1.5h, poured into 914.39g of an aqueous solution with a polyvinyl alcohol content of 7% at a solid-liquid ratio of 1:1.5, and then stirred with a stirrer for 4h to obtain a sol, and then dried in an oven at 190°C for 8h to obtain a gel, and then the gel was transferred to a muffle furnace for programmed temperature calcination at a heating rate of 5°C / min. First, it was raised to 550°C and calcined for 6h, then raised to 800°C and calcined for 6h, cooled, and ground to obtain the adsorbent precursor Li2La 0.05 T i 0.95 O3. Then use 0.05mol HCl to acidify it, add 100g of adsorbent precursor into 4L of acid solution, and when the pH value rises, continue to add hydrochloric acid to ensure that its concentration is 0.05mol, then change the acid solution twice, and finally the pH does not change, the acidification is completed, a total of 15h, and wash to obtain H2La 0.05 Ti 0.95 O3.Li2La 0.05 T i 0.95 XRD of O3 Figure 5 Its microstructure and element distribution are shown in Figure 6. Table 3 Li2La 0.05 T i 0.95 Atomic content ratio of each element in O3.
[0061] Table 3 Li2La 0.05 T i 0.95 Atomic content of O3
[0062] element Atomic Percent O 83.66 Ti 15.53 La 0.82 Total 100
[0063] The H2La obtained above 0.05 T i 0.95 10g of O3 adsorbent was added to the test brine. The adsorbent had an effect on Li + The changes in adsorption capacity are as follows Figure 7 As shown in Table 4, the adsorption capacity after 3 hours is 21.33 mg / g, and the adsorption capacity after 96 hours is 65.57 mg / g. From the adsorption trend, it can be observed that the adsorption rate is high in the first 3 hours, and after 24 hours, the adsorption rate tends to be flat. After 7 cycles of adsorption, as shown in Table 4, the adsorption capacity after 96 hours in the 7th cycle is 62.07 mg / g, and the adsorption performance is still good.
[0064] Table 4H2La 0.05 T i 0.95 Adsorption performance of O3 after 7 cycles
[0065]
[0066] Example 4: Figure 1 , Figure 2 , Figure 3a , Figure 3b , Figure 3c , Figure 4 , Figure 5 , Figure 6a , Figure 6b , Figure 6c , Figure 7 , Figure 8 , Figure 9a , Figure 9b , Fig.9c , Fig.10 , Fig.11 , Fig.12a , Figure 12b , Fig.12c and Fig.13 As shown, a method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity includes the following steps for preparing a lithium metatitanate adsorbent:
[0067] The lithium source, lanthanum salt and titanium source were mixed in a molar ratio of 2.4:0.08:0.92, that is, 627.29g of lithium stearate (analytical grade), 43.34g of La2(CO3)3·8H2O (analytical grade) and 81.04g (chemically pure) of titanic acid were dry mixed in a ball mill for 1.7h, poured into 1353.01g of an aqueous solution with a polyvinyl alcohol content of 8% at a solid-liquid ratio of 1:1.8, and then stirred with a stirrer for 5h to obtain a sol, and then dried in an oven at 195°C for 9h to obtain a gel, and then the gel was transferred to a muffle furnace for programmed temperature calcination at a heating rate of 8°C / min. First, it was raised to 600°C and calcined for 7h, then raised to 850°C and calcined for 7h, cooled, and ground to obtain the adsorbent precursor Li2La 0.08 T i 0.92 O3. Then use 0.08mol HCl to acidify it, add 100g of adsorbent precursor into 4L of acid solution, and when the pH value rises, continue to add hydrochloric acid to ensure that its concentration is 0.08mol, then change the acid solution twice, and finally the pH does not change, the acidification is completed, a total of 12h, and wash to obtain H2La 0.08 Ti 0.92 O3.Li2La 0.08 T i 0.92 XRD of O3 Figure 8 Its microstructure and element distribution are shown in Figure 9. Table 5 Li2La 0.08 T i 0.92 Atomic content ratio of each element in O3.
[0068] Table 5 Li2La0.08 T i 0.92 Atomic content of O3
[0069] element Atomic Percent O 82.94 Ti 15.34 La 1.72 Total 100
[0070] The H2La obtained above 0.08 T i 0.92 10g of O3 adsorbent was added to the test brine. The adsorbent had an effect on Li + The changes in adsorption capacity are as follows Fig.10 As shown in Table 6, the adsorption capacity after 3 hours is 21.56 mg / g, and the adsorption capacity after 96 hours is 67.69 mg / g. From the adsorption trend, it can be observed that the adsorption rate is high in the first 3 hours, and after 24 hours, the adsorption rate tends to be flat. It was subjected to 7 cycles of adsorption, as shown in Table 6. In the 7th cycle, the adsorption capacity after 96 hours is 64.05 mg / g, and the adsorption performance is still good.
[0071] Table 6H2La 0.08 T i 0.92 Adsorption performance of O3 after 7 cycles
[0072]
[0073] Example 5: Figure 1 , Figure 2 , Figure 3a , Figure 3b , Figure 3c , Figure 4 , Figure 5 , Figure 6a , Figure 6b , Figure 6c , Figure 7 , Figure 8 , Figure 9a , Figure 9b , Fig.9c , Fig.10 , Fig.11 , Fig.12a , Figure 12b , Fig.12c and Fig.13 As shown, a method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity includes the following steps for preparing a lithium metatitanate adsorbent:
[0074] The lithium source, lanthanum salt and titanium source were mixed in a molar ratio of 2.5:0.1:0.9, that is, 726.03g of lithium stearate (analytical grade), 60.20g of La2(CO3)3·8H2O (analytical grade) and 88.09g (chemically pure) of titanic acid were dry mixed in a ball mill for 2h, poured into 1748.64g of an aqueous solution with a polyvinyl alcohol content of 10% at a solid-liquid ratio of 1:2, and then stirred with a stirrer for 6h to obtain a sol, and then dried in an oven at 200°C for 10h to obtain a gel, and then the gel was transferred to a muffle furnace for programmed temperature calcination at a heating rate of 10°C / min, first raised to 650°C, calcined for 8h, then raised to 900°C, calcined for 8h, cooled, and ground to obtain the adsorbent precursor Li2La 0.1 T i 0.9 O3. Then use 0.11mol HCl to acidify it, add 100g of adsorbent precursor into 4L of acid solution, and when the pH value rises, continue to add hydrochloric acid to ensure that its concentration is 0.1mol, then change the acid solution twice, and finally the pH does not change, the acidification is completed, a total of 10h, wash to get H2La 0.1 T i 0.9 O3.Li2La 0.1 T i 0.9 XRD of O3 Fig.11 The microstructure and element distribution of the adsorbent are shown in Figure 12. Table 7 is Li2La 0.1 T i 0.9 Atomic content ratio of each element in O3.
[0075] Table 7 Li2La 0.1 T i 0.9 Atomic content of O3
[0076] element Atomic Percent O 80.03 Ti 17.35 La 2.26 Total 100
[0077] Material adsorption test steps: The H2La 0.1 T i 0.9 10g of O3 adsorbent was added to the test brine. The adsorbent was + The changes in adsorption capacity are as follows Fig.13 As shown in Table 8, the adsorption capacity after 3 hours is 22.41 mg / g, and the adsorption capacity after 48 hours is 68.21 mg / g. The adsorption rate in the first 3 hours is relatively high, and after 12 hours, the adsorption rate tends to be flat. After 7 cycles of adsorption, as shown in Table 8, the adsorption capacity after 48 hours in the 7th cycle is 64.27 mg / g, and the adsorption performance is still good.
[0078] Table 8H2La 0.1 T i 0.9 Adsorption performance of O3 after 7 cycles
[0079]
[0080] As described above, the embodiments of the present invention are described in detail, but it is obvious to those skilled in the art that many variations are possible as long as they do not deviate from the inventive point and effect of the present invention. Therefore, all such variations are also included in the protection scope of the present invention.
Claims
1. A method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity, characterized in that , comprising the following steps: dry mixing a lithium source, a lanthanum salt and a titanium source, pouring them into a polyvinyl alcohol aqueous solution, stirring, beating and drying, entering a first stage of heating and calcining, and then entering a second stage of heating and calcining to obtain a precursor for acidification to obtain an adsorbent; the lithium source, the lanthanum salt used for doping and the titanium source are dry stirred and mixed for 1-2 hours in a molar ratio of Li:La:Ti=2.1-2.5:0.01-0.1:0.99-0.9, wherein the lithium source is lithium stearate LiC 18 H 35 O2, the lanthanum salt is lanthanum carbonate La2(CO3)3·8H2O, and the titanium source is metatitanate H2TiO3; the dry mixing method is a combination of a pulverizer mixing or a ball mill mixing; the mixed materials are poured into a 5%-10% polyvinyl alcohol aqueous solution and stirred for 3-6 hours to obtain a sol, the solid-liquid content is 1kg solid to 1-2kg liquid, and then dried at 185-200°C for 6-10 hours using a drying device to obtain a gel; the gel is transferred to a muffle furnace for a first stage of programmed temperature calcination, the heating rate is 2-10°C / min, first raised to 550-650°C, calcined for 4-8 hours, and then in the second stage of programmed temperature rise to 700-900°C and calcined for 4-8 hours, thereby obtaining Li2La with high specific surface area, small size and large adsorption capacity x Ti (1-x) O3 precursor; soak the precursor in 0.01-0.1mol acid solution for 10-20h to acidify Li + Replaced to obtain lithium adsorbent H2La x Ti (1-x) O3, wherein the acid solution is hydrochloric acid or sulfuric acid.
2. The method for preparing a titanium-based lithium adsorbent precursor with high adsorption capacity according to claim 1, characterized in that , also contains the following steps: the obtained lithium adsorbent is subjected to an adsorption capacity test, and the test brine parameters are that 1L of ultrapure water contains 1.60g of lithium carbonate, 7.61g of sodium bicarbonate, 10.58g of anhydrous sodium sulfate, 11.86g of anhydrous sodium carbonate, and 78.31g of sodium chloride, and the feed ratio during the test is 10g / L.