A porous hollow ternary precursor and preparation method thereof

By forming a porous hollow structure in the ternary positive electrode material, the problem of structural failure of the material under cyclic charge and discharge is solved, the rate performance and cycle stability are improved, and the material life is extended.

CN116199274BActive Publication Date: 2024-11-15ZHEJIANG MEIDU HITRANS LITHIUM BATTERY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211712123.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-11-15
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The change in the material volume and side reactions of the ternary positive electrode material under long-term high current cycle charge and discharge lead to structural damage, resulting in rapid attenuation of the circulation capacity, and the long transmission distance of lithium ions leads to electrochemical polarization, affecting the rate performance and cyclic stability.

Method used

The dissolution method is used to form a porous hollow structure inside the ternary precursor. Through the co-deposition reaction of nickel, cobalt, manganese inorganic salts and inorganic aluminum alkali solution, the reaction pH and stirring speed are controlled to form a nickel, cobalt, manganese ternary shell structure, and the The aluminum hydroxide in the core is dissolved in a strong alkali environment to form a porous hollow structure.

Benefits of technology

It improves the microstructure stability of the material, shortens the lithium ion transmission distance, reduces electrochemical polarization, improves rate performance and cycle stability, and extends the cycle life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116199274B_ABST
    Figure CN116199274B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of positive electrode materials for lithium-ion batteries, and in particular to a porous hollow ternary precursor and a preparation method thereof. The method comprises: 1) introducing a ternary mixed solution of nickel, cobalt and manganese, an inorganic aluminum alkali solution, a complexing agent and a precipitant into a reactor for co-deposition to prepare a nickel, cobalt, manganese and aluminum quaternary core structure; 2) after the core particle size reaches the target particle size, the inorganic aluminum alkali solution is stopped from being introduced and the nickel, cobalt and manganese ternary shell structure is continuously co-deposited; 3) after the overall particle size reaches the target particle size, the reacted material is placed in a strong alkaline solution and stirred so that the aluminum hydroxide in the core is dissolved to form a porous hollow structure, and a porous hollow ternary precursor is obtained after washing, separation and drying. The present invention can accurately control the core growth size through the reaction time, thereby accurately controlling the size of the finished porous hollow structure, and the prepared precursor has excellent rate performance and cycle stability, and does not require the addition of additional equipment, is easy to operate, and is suitable for industrial industrialization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a porous hollow ternary precursor prepared by a dissolution method and a preparation method thereof. Background Art

[0002] The main industrialized cathode materials for lithium-ion batteries are lithium manganese oxide, lithium cobalt oxide, lithium iron phosphate and ternary cathode materials. Among them, ternary cathode materials are widely used in power, digital, energy storage and other fields due to their high energy density, long cycle life, safety and environmental protection. Ternary cathode materials are sintered by mixing ternary precursors (nickel cobalt manganese hydroxide / nickel cobalt aluminum hydroxide) with lithium salts (lithium hydroxide / lithium carbonate), and the sintering process has little effect on the performance of the ternary precursor. The morphology and particle size of the ternary cathode material are inherited from the ternary precursor. Therefore, 70% of the performance of the ternary cathode material is determined by the quality of the ternary precursor.

[0003] How to ensure the specific capacity of ternary positive electrode materials while having excellent rate performance and cycle stability is a research hotspot for ternary positive electrode materials. In particular, with the rapid development of fast charging technology, higher requirements are placed on the structural stability of ternary positive electrode materials. The volume change of the material produced by the ternary positive electrode materials under long-term high-current cyclic charging and discharging and the side reactions between the ternary positive electrode materials and the electrolyte will cause the destruction of the material structure and lead to the rapid decay of its cycle capacity. If a loose porous hollow structure is formed inside the ternary positive electrode material, the structural damage caused by the volume change of the material and the side reactions can be effectively alleviated. At the same time, the hollow internal structure can shorten the lithium ion transmission distance of the ternary positive electrode material during the charging and discharging process, accelerate the ion migration rate and effectively reduce the electrochemical polarization. Therefore, it is very necessary to prepare a porous hollow ternary precursor. Summary of the invention

[0004] The present invention aims to overcome the deficiencies of the prior art and provide a porous hollow ternary precursor and a method for preparing the same. In the preparation process of the ternary precursor, a porous hollow structure is formed inside the ternary precursor by a dissolution method to enhance the microstructural stability of the material and improve the electrochemical properties of the material. The first object of the present invention is to provide a porous hollow ternary precursor. The second object of the present invention is to provide a method for preparing a porous hollow ternary precursor.

[0005] The technical solution adopted by the present invention to solve the above problems is:

[0006] The present invention provides a method for preparing a porous hollow ternary precursor, comprising the following steps:

[0007] (1) preparing a ternary mixed metal salt solution using nickel, cobalt and manganese inorganic salts; preparing an inorganic aluminum base solution; preparing a precipitant aqueous solution; and preparing a complexing agent aqueous solution;

[0008] (2) filling the reactor and the concentrator with pure water and circulating the water, introducing a protective gas, introducing a complexing agent aqueous solution and a precipitant aqueous solution to adjust the complexing agent concentration and the first pH, and controlling the reaction temperature;

[0009] Under the first stirring speed condition, the ternary mixed metal salt solution, the inorganic aluminum base solution, the complexing agent aqueous solution and the precipitant aqueous solution are simultaneously introduced into the reaction kettle, and the reaction pH is controlled to be adjusted stepwise to the second pH;

[0010] When the particle size of the reactants reaches the target particle size of the inner core, the inorganic aluminum alkali solution is stopped, and the reaction pH is adjusted to the third pH, and the rotation speed is adjusted to the second stirring speed to continue co-deposition to prepare the nickel-cobalt-manganese ternary outer shell structure, and the reaction is stopped when the overall particle size reaches the target particle size;

[0011] (3) After the reacted material is allowed to stand, the supernatant is removed, and a strong alkaline solution is added and stirred to dissolve the aluminum hydroxide in the inner core to form a porous hollow structure; after post-treatment, a porous hollow ternary precursor is obtained.

[0012] Preferably, the nickel, cobalt and manganese inorganic salts in step (1) are one or more of the corresponding sulfates, nitrates and chlorides; more preferably, the nickel inorganic salt is one or more of nickel sulfate, nickel nitrate and nickel chloride, the cobalt inorganic salt is one or more of cobalt sulfate, cobalt nitrate and cobalt chloride, and the manganese inorganic salt is one or more of manganese sulfate, manganese nitrate and manganese chloride.

[0013] Preferably, the total concentration of metals (nickel, cobalt, and manganese) in the ternary mixed metal salt solution in step (1) is 80 to 120 g / L.

[0014] Preferably, the ratio of nickel, cobalt and manganese in the ternary mixed metal salt solution in step (1) conforms to the formula Ni x Co y Mn (1-x-y) (OH)2, where 0 <x<1,0<y<1。

[0015] Preferably, the inorganic aluminum in the inorganic aluminum alkali solution in step (1) is one or more of sodium aluminate and aluminum sulfate; more preferably, the aluminum concentration in the inorganic aluminum alkali solution in step (1) is 20 to 80 g / L, the alkali is sodium hydroxide, and the pH value is 13.00 to 13.50.

[0016] Preferably, the precipitant in step (1) is one or more of sodium hydroxide and potassium hydroxide. More preferably, the concentration of the precipitant aqueous solution in step (1) is 120-440 g / L.

[0017] Preferably, the complexing agent in step (1) is one or more of ammonia water and ethylenediaminetetraacetic acid. More preferably, the concentration of the complexing agent aqueous solution in step (1) is 85-200 g / L.

[0018] Preferably, the volume of the reactor in step (2) is 1 to 10 m 3 More preferably, the volume of the concentrator in step (2) is 0.1 to 3 m 3 .

[0019] Preferably, the protective gas in step (2) is one or more of nitrogen or helium.

[0020] Preferably, the reaction temperature in step (2) is 50-70°C;

[0021] Preferably, the concentration of the reaction complexing agent in step (2) is 2.0 to 6.5 g / L;

[0022] Preferably, the first pH of the reaction in step (2) is 11.80-12.10;

[0023] Preferably, the first stirring speed in step (2) is 200 to 260 rpm;

[0024] Preferably, in step (2), the pumping flow rate of the ternary mixed metal salt solution is 30 to 600 L / h;

[0025] Preferably, in step (2), the inorganic aluminum alkali solution is pumped in at a flow rate of 15 to 400 L / h;

[0026] Preferably, the second pH in step (2) is 10.50-11.00;

[0027] Preferably, the step (2) is to reduce the pH by 0.02 pH per hour;

[0028] Preferably, the target particle size of the kernel in step (2) is 2.0 to 5.0 μm;

[0029] Preferably, the third pH in step (2) is 10.80-11.20;

[0030] Preferably, the second stirring speed in step (2) is 110 to 160 rpm;

[0031] Preferably, in step (2), the overall particle size reaches a target particle size of 3.0 to 15.0 μm, and is not less than the target particle size of the core.

[0032] Preferably, the standing time in step (3) is 2 to 4 hours.

[0033] Preferably, the strong base added in step (3) is at least one of sodium hydroxide and potassium hydroxide; more preferably, the mass concentration of the strong base sodium hydroxide solution is 32%, and the added volume is 0.5 to 5m 3 ; More preferably, the stirring time in step (3) is 10 to 24 hours.

[0034] Preferably, the post-treatment includes washing, centrifuging, drying, batch mixing, screening, and iron removal of the dissolved material to obtain a porous hollow ternary precursor;

[0035] More preferably, the water washing temperature is 60 to 85°C;

[0036] More preferably, the drying temperature is 100-150°C.

[0037] Preferably, the size of the porous hollow structure inside the ternary precursor obtained by the preparation method is 2 to 5 nm; more preferably, the overall particle size of the ternary precursor is 3.0 to 15.0 μm, and the particle size distribution is 0.3 to 0.8; more preferably, the tap density of the ternary precursor is 1.0 to 2.1 g / cm 3 More preferably, the BET of the ternary precursor is 5 to 15 m 2 / g.

[0038] The present invention also provides a porous hollow ternary precursor prepared by any of the above preparation methods, wherein the size of the porous hollow structure inside the precursor is 2-5 nm, the particle size is 3.0-15.0 μm, the particle size distribution is 0.3-0.8, and the tap density is 1.0-2.1 g / cm 3 , BET is 5~15m 2 / g.

[0039] The present invention prepares a nickel-cobalt-manganese-aluminum quaternary core structure by passing a ternary mixed solution of nickel-cobalt-manganese, an inorganic aluminum alkali solution, a complexing agent and a precipitant into a reactor for co-deposition, stops passing the inorganic aluminum alkali solution after the core particle size reaches the target particle size, and continues co-deposition to prepare a nickel-cobalt-manganese ternary shell structure, and then places the reacted material in a strong alkaline solution and stirs it after the overall particle size reaches the target particle size so that the aluminum hydroxide in the core is dissolved to form a porous hollow structure, and a porous hollow ternary precursor is obtained after washing, separation and drying. The present invention can accurately control the porosity of the internal porous hollow structure by adjusting the aluminum content of the core, and the prepared precursor has excellent rate performance and cycle stability.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] In the technical solution described in the present invention, the characteristics of aluminum amphoteric metals are utilized, and deviated acid radicals or aluminum ions are used as aluminum sources. A nickel-cobalt-manganese-aluminum hydroxide core is prepared under weakly alkaline conditions through co-precipitation reaction and nickel-cobalt-manganese metal ions. Aluminum hydroxide is evenly distributed in the core, and the core particle size can be precisely controlled. After reaching the required size, the aluminum source is stopped, and a nickel-cobalt-manganese hydroxide ternary shell structure is prepared by co-precipitation. After the co-precipitation is completed, the prepared particles are stirred in a strong alkaline environment to dissolve the aluminum hydroxide in the core and form a porous hollow structure inside the particles;

[0042] In the technical solution of the present invention, the core growth size can be precisely controlled by the reaction time, thereby precisely controlling the size of the finished porous hollow structure. The proportion of aluminum hydroxide in the core can be precisely controlled by the aluminum source pumping rate, thereby precisely controlling the porosity of the finished porous hollow structure.

[0043] Compared with the existing conventional ternary precursor preparation technology, the porous hollow ternary precursor prepared by the technical solution of the present invention can be industrialized without adding additional equipment, and has broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1-1 , Figure 1-2 This is a scanning electron microscope image of a porous hollow ternary precursor prepared by the dissolution method in Example 1;

[0045] Figure 2-1 , Figure 2-2 This is a scanning electron microscope image of a porous hollow ternary precursor prepared by the dissolution method in Example 2;

[0046] Figure 3-1 , Figure 3-2 This is a scanning electron microscope image of a porous hollow ternary precursor prepared by the dissolution method in Example 3;

[0047] Figure 4-1 , Figure 4-2 This is a scanning electron microscope image of the porous hollow ternary precursor prepared by the dissolution method in Comparative Example 1. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described in detail below through specific embodiments and in combination with the accompanying drawings. Obviously, the following embodiments are only some embodiments of the present invention, not all embodiments. It should be pointed out that all embodiments made by those skilled in the art without departing from the main concept of the present invention and making non-essential changes are still within the protection scope of the present invention.

[0049] The present invention provides a porous hollow ternary precursor prepared by a dissolution method and a preparation method thereof, wherein the steps of the preparation method are as follows:

[0050] Nickel, cobalt and manganese inorganic salts are used according to the ratio of nickel, cobalt and manganese.x Co y Mn (1-x-y) (OH)2 is used to prepare a ternary metal mixed solution with a total metal salt concentration of 80 to 120 g / L; an inorganic aluminum salt is used to prepare an aluminum concentration of 20 to 80 g / L, and the pH value of the solution is adjusted to 13.00 to 13.50 with sodium hydroxide to obtain an inorganic aluminum alkali solution; a precipitant aqueous solution with a concentration of 120 to 440 g / L is prepared; and a complexing agent aqueous solution with a concentration of 85 to 200 g / L is prepared;

[0051] The volume is 1~10m 3 The reactor volume is 0.1~3m 3 The concentrator is filled with pure water and circulated, and a protective gas is introduced. The complexing agent aqueous solution and the precipitant aqueous solution are introduced to adjust the complexing agent concentration in the system to 2.0-6.5 g / L and the first pH to 11.80-12.10, and the reaction temperature is controlled to be 50-70°C; under the condition of a first stirring speed of 200-260 rpm, the nickel-cobalt-manganese ternary mixed solution is pumped in at a flow rate of 30-600 L / h, the inorganic aluminum alkali solution is pumped in at a flow rate of 15-400 L / h, and the complexing agent aqueous solution and the precipitant aqueous solution are pumped in. At the same time, the reaction kettle was introduced, and the reaction pH was controlled to decrease by 0.02 stepwise per hour to adjust to the second pH of 10.50-11.00. When the particle size of the reactant reached the target particle size of the inner core of 2.0-5.0 μm, the inorganic aluminum alkali solution was stopped, and the reaction pH was adjusted to the third pH of 10.80-11.20. The rotation speed was adjusted to the second stirring speed of 110-160 rpm to continue co-deposition to prepare the nickel-cobalt-manganese ternary shell structure. The reaction was stopped after the overall particle size reached the target particle size of 3.0-15.0 μm.

[0052] The reacted material is discharged into the aging kettle, and after standing for 2 to 4 hours, the supernatant is removed, and 0.5 to 5 ml of 32% sodium hydroxide solution is added. 3 , and stirred for 10 to 24 hours to dissolve the aluminum hydroxide in the inner core to form a porous hollow structure;

[0053] The dissolved material is washed and centrifuged at a temperature of 60-85°C, dried at 100-150°C, mixed, sieved, and iron removed to obtain a porous hollow ternary precursor. The size of the porous hollow structure inside the precursor is 2-5nm, the particle size is 3.0-15.0μm, the particle size distribution is 0.3-0.8, and the tap density is 1.0-2.1g / cm 3 , BET is 5~15m 2 / g.

[0054] Example 1

[0055] Nickel, cobalt and manganese inorganic salts are used according to the ratio of nickel, cobalt and manganese. 0.90 Co 0.05 Mn0.05 (OH)2 is used to prepare a ternary metal mixed solution with a total metal salt concentration of 90g / L; sodium aluminate is used to prepare a sodium hydroxide solution with an aluminum concentration of 50g / L and a pH value of 13.20; a sodium hydroxide aqueous solution with a concentration of 400g / L; and an ammonia aqueous solution with a concentration of 95g / L;

[0056] The volume is 2m 3 The reactor volume is 0.5m 3 The concentrator is filled with pure water and circulated, and nitrogen is introduced. The complexing agent aqueous solution and the precipitating agent aqueous solution are introduced to adjust the complexing agent concentration to 4.0 g / L and the first pH to 11.90, and the reaction temperature is controlled to be 60°C; under the condition of a first stirring speed of 200 rpm, the nickel-cobalt-manganese ternary mixed solution is pumped at a flow rate of 50 L / h, the sodium aluminate alkaline solution is pumped at a flow rate of 30 L / h, and the complexing agent aqueous solution and the precipitating agent aqueous solution are simultaneously introduced into the reactor, and the reaction pH is controlled to decrease by 0.02 per hour in a stepwise manner to adjust to a second pH of 11.00, and when the reactant particle size reaches the inner core target particle size of 4.0 μm, the sodium aluminate solution is stopped, and the reaction pH is adjusted to a third pH of 10.90, the rotation speed is adjusted to a second stirring speed of 120 rpm to continue co-deposition to prepare a nickel-cobalt-manganese ternary shell structure, and the reaction is stopped after the overall particle size reaches the target particle size of 10.5 μm.

[0057] The reacted material was discharged into the aging kettle, and after standing for 2 hours, the supernatant was removed and 2m sodium hydroxide solution with a concentration of 32% was added. 3 The mixture was stirred for 20 hours to dissolve the aluminum hydroxide in the inner core and form a porous hollow structure;

[0058] The dissolved material is washed and centrifuged at 70°C, dried at 120°C, batch mixed, sieved, and iron removed to obtain a porous hollow ternary precursor.

[0059] The ternary precursor material prepared in Example 1 of the present invention was subjected to scanning electron microscopy testing, and the test results are as follows: Figure 1-1 , Figure 1-2 As shown, it can be seen that there is a 4.0 micron porous hollow structure in the center of the ternary precursor material prepared in Example 1 of the present invention.

[0060] The D50 of the porous hollow ternary precursor prepared in Example 1 of the present invention is 10.42 μm.

[0061] The particle size distribution of the porous hollow ternary precursor prepared in Example 1 of the present invention is 0.38.

[0062] The tap density of the porous hollow ternary precursor prepared in Example 1 of the present invention is 1.82 g / cm 3 .

[0063] The BET of the porous hollow ternary precursor prepared in Example 1 of the present invention is 8.33m 2 / g.

[0064] Example 2

[0065] Nickel, cobalt and manganese inorganic salts are used according to the ratio of nickel, cobalt and manganese. 0.88 Co 0.08 Mn0.04(OH)2 is used to prepare a ternary metal mixed solution with a total metal salt concentration of 120g / L; sodium aluminate is used to prepare a sodium hydroxide solution with an aluminum concentration of 40g / L and a pH value of 13.20; a sodium hydroxide aqueous solution with a concentration of 200g / L is prepared; and an ammonia aqueous solution with a concentration of 95g / L is prepared;

[0066] The volume is 2m 3 The reactor volume is 0.5m 3 The concentrator is filled with pure water and circulated, and nitrogen is introduced. The complexing agent aqueous solution and the precipitating agent aqueous solution are introduced to adjust the complexing agent concentration to 3.0 g / L and the first pH to 12.00, and the reaction temperature is controlled to be 65°C; under the condition of a first stirring speed of 260 rpm, the nickel-cobalt-manganese ternary mixed solution is pumped at a flow rate of 50 L / h, the sodium aluminate alkaline solution is pumped at a flow rate of 20 L / h, and the complexing agent aqueous solution and the precipitating agent aqueous solution are simultaneously introduced into the reactor, and the reaction pH is controlled to decrease by 0.02 per hour in a stepwise manner to adjust to a second pH of 10.90, and when the reactant particle size reaches the target inner core particle size of 2.0 μm, the sodium aluminate solution is stopped, and the reaction pH is adjusted to a third pH of 10.80, the rotation speed is adjusted to a second stirring speed of 130 rpm, and co-deposition is continued to prepare a nickel-cobalt-manganese ternary shell structure, and the reaction is stopped after the overall particle size reaches the target particle size of 10.0 μm.

[0067] The reacted material was discharged into the aging kettle, and after standing for 2 hours, the supernatant was removed and 2m sodium hydroxide solution with a concentration of 32% was added. 3 The mixture was stirred for 20 hours to dissolve the aluminum hydroxide in the inner core and form a porous hollow structure;

[0068] The dissolved material is washed and centrifuged at 70°C, dried at 120°C, batch mixed, sieved, and iron removed to obtain a porous hollow ternary precursor.

[0069] The ternary precursor material prepared in Example 2 of the present invention was tested by scanning electron microscopy. The test results are as follows: Figure 2-1 , Figure 2-2 As shown, it can be seen that there is a 2.0 micron porous hollow structure in the center of the ternary precursor material prepared in Example 2 of the present invention.

[0070] The D50 of the porous hollow ternary precursor prepared in Example 2 of the present invention is 9.98 μm.

[0071] The particle size distribution of the porous hollow ternary precursor prepared in Example 2 of the present invention is 0.38.

[0072] The tap density of the porous hollow ternary precursor particles prepared in Example 2 of the present invention is 1.95 g / cm 3 .

[0073] The BET of the porous hollow ternary precursor particles prepared in Example 2 of the present invention is 6.49 m 2 / g.

[0074] Example 3

[0075] Nickel, cobalt and manganese inorganic salts are used according to the ratio of nickel, cobalt and manganese. 0.65 Co 0.15 Mn 0.20 (OH)2 is used to prepare a ternary metal mixed solution with a total metal salt concentration of 90g / L; sodium aluminate is used to prepare a sodium hydroxide solution with an aluminum concentration of 50g / L and a pH value of 13.20; a sodium hydroxide aqueous solution with a concentration of 200g / L; and an ammonia aqueous solution with a concentration of 170g / L;

[0076] The volume is 8m 3 The reactor volume is 2m 3 The concentrator is filled with pure water and circulated, and nitrogen is introduced. The complexing agent aqueous solution and the precipitating agent aqueous solution are introduced to adjust the complexing agent concentration to 4.5 g / L and the first pH to 12.30, and the reaction temperature is controlled to be 60°C; under the condition of a first stirring speed of 240 rpm, the nickel-cobalt-manganese ternary mixed solution is pumped at a flow rate of 600 L / h, the sodium aluminate alkaline solution is pumped at a flow rate of 200 L / h, and the complexing agent aqueous solution and the precipitating agent aqueous solution are simultaneously introduced into the reactor, and the reaction pH is controlled to decrease by 0.02 per hour in a stepwise manner to adjust to a second pH of 11.00, and when the reactant particle size reaches the inner core target particle size of 2.0 μm, the sodium aluminate solution is stopped, and the reaction pH is adjusted to a third pH of 10.70, and the rotation speed is adjusted to a second stirring speed of 160 rpm to continue co-deposition to prepare a nickel-cobalt-manganese ternary shell structure, and the reaction is stopped after the overall particle size reaches the target particle size of 3.5 μm.

[0077] The reacted material was discharged into the aging kettle, and after standing for 4 hours, the supernatant was removed and 5 mL of sodium hydroxide solution with a concentration of 32% was added. 3 The mixture was stirred for 15 h to dissolve the aluminum hydroxide in the inner core to form a porous hollow structure;

[0078] The dissolved material is washed and centrifuged at 70°C, dried at 120°C, batch mixed, sieved, and iron removed to obtain a porous hollow ternary precursor.

[0079] The ternary precursor material prepared in Example 3 of the present invention was tested by scanning electron microscopy. The test results are as follows: Figure 3-1 , Figure 3-2 As shown, it can be seen that there is a 2.0 micron porous hollow structure in the center of the ternary precursor material prepared in Example 3 of the present invention.

[0080] The D50 of the porous hollow ternary precursor prepared in Example 3 of the present invention is 3.48 μm;

[0081] The particle size distribution of the porous hollow ternary precursor prepared in Example 3 of the present invention is 0.69 μm

[0082] The tap density of the porous hollow ternary precursor prepared in Example 3 of the present invention is 1.76 g / cm 3 .

[0083] The BET of the porous hollow ternary precursor prepared in Example 3 of the present invention is 9.86m 2 / g.

[0084] Comparative Example 1

[0085] Nickel, cobalt and manganese inorganic salts are used according to the ratio of nickel, cobalt and manganese. 0.84 Co 0.12 Mn 0.04 (OH)2 prepares a ternary metal mixed solution with a total metal salt concentration of 90g / L; prepares a sodium hydroxide solution with a concentration of 200g / L; prepares an ammonia solution with a concentration of 170g / L;

[0086] The volume is 8m 3 The reactor volume is 2m 3 The concentrator was filled with pure water and circulated, and nitrogen was introduced. The complexing agent aqueous solution and the precipitant aqueous solution were introduced to adjust the complexing agent concentration to 4.5 g / L and the first pH to 12.20, and the reaction temperature was controlled to be 65°C; under the condition of a first stirring speed of 240 rpm, the nickel-cobalt-manganese ternary mixed solution was pumped into the reactor at a flow rate of 600 L / h, the complexing agent aqueous solution and the precipitant aqueous solution were simultaneously introduced into the reactor, the reaction pH was controlled to decrease by 0.02 stepwise per hour to adjust to a second pH of 10.85, and the reaction was stopped after the particle size reached the target particle size of 3.8 μm.

[0087] The reacted material was discharged into the aging kettle, and after standing for 4 hours, the supernatant was removed and 0.5 m sodium hydroxide solution with a concentration of 32% was added. 3 and stirred for 2h;

[0088] The material is washed and centrifuged at 70°C, dried at 120°C, batch mixed, sieved, and iron removed to obtain a porous hollow ternary precursor.

[0089] The ternary precursor material prepared in comparative example 3 of the present invention was subjected to scanning electron microscopy test, and the test results are as follows: Figure 4-1 , Figure 4-2As shown, it can be seen that the ternary precursor material prepared in Comparative Example 1 of the present invention has no porous hollow structure in the center.

[0090] The D50 of the porous hollow ternary precursor prepared in Comparative Example 1 of the present invention is 3.74 μm;

[0091] The particle size distribution of the porous hollow ternary precursor prepared in Comparative Example 1 of the present invention is 0.70 μm

[0092] The tap density of the porous hollow ternary precursor prepared in Comparative Example 1 of the present invention is 1.79 g / cm 3 .

[0093] The BET of the porous hollow ternary precursor prepared in Comparative Example 1 of the present invention is 6.81m 2 / g.

[0094] The above-described embodiments are only preferred solutions of the present invention and are not intended to limit the present invention in any form. Other variations and modifications are possible without exceeding the technical solutions described in the claims.

Claims

1. A method for preparing a porous hollow ternary precursor, characterized in that: The steps include: (1) preparing a ternary mixed metal salt solution using nickel, cobalt and manganese inorganic salts; preparing an inorganic aluminum base solution; preparing a precipitant aqueous solution; and preparing a complexing agent aqueous solution; (2) filling the reactor and the concentrator with pure water and circulating the water, introducing a protective gas, introducing a complexing agent aqueous solution and a precipitant aqueous solution, adjusting the complexing agent concentration and the first pH, and controlling the reaction temperature; Under the first stirring speed condition, the ternary mixed metal salt solution, the inorganic aluminum base solution, the complexing agent aqueous solution and the precipitant aqueous solution are simultaneously introduced into the reaction kettle, and the reaction pH is controlled to be adjusted stepwise to the second pH; When the particle size of the reactants reaches the target particle size of the inner core, the inorganic aluminum alkali solution is stopped, and the reaction pH is adjusted to the third pH, and the rotation speed is adjusted to the second stirring speed to continue co-deposition to prepare the nickel-cobalt-manganese ternary outer shell structure, and the reaction is stopped when the overall particle size reaches the target particle size; (3) allowing the reacted material to stand, removing the supernatant, adding a strong alkaline solution and stirring to form a porous hollow structure; and obtaining a porous hollow ternary precursor after post-treatment; Wherein, the inorganic aluminum in the inorganic aluminum alkali solution in step (1) is one or more of sodium aluminate and aluminum sulfate; In step (2), the reaction temperature is 50-70° C.; the concentration of the reaction complexing agent is 2.0-6.5 g / L; the first reaction pH is 11.80-12.10; In step (2), the first stirring speed is 200-260 rpm; the second pH is 10.50-11.00; the step-wise method is to reduce the pH by 0.02 pH per hour; In step (2), the target particle size of the core is 2.0 to 5.0 μm; the third pH is 10.80 to 11.20; the second stirring speed is 110 to 160 rpm; and the overall particle size reaches the target particle size of 3.0 to 15.0 μm.

2. The method for preparing a porous hollow ternary precursor according to claim 1, characterized in that: In the step (1), the nickel, cobalt and manganese inorganic salts are one or more of the corresponding sulfates, nitrates and chlorides, the total metal concentration in the ternary mixed metal salt solution is 80-120 g / L, and the ratio of nickel, cobalt and manganese conforms to the formula Ni x Co y Mn (1-x-y) (OH)2, where 0 <x<1,0<y<1。 3. The method for preparing a porous hollow ternary precursor according to claim 1, characterized in that: In step (1), the aluminum concentration in the inorganic aluminum alkali solution is 20 to 80 g / L, and the pH value is 13.00 to 13.

50.

4. The method for preparing a porous hollow ternary precursor according to claim 1, characterized in that: In the step (1), the precipitant is one or more of sodium hydroxide and potassium hydroxide, and the concentration is 120-440 g / L.

5. The method for preparing a porous hollow ternary precursor according to claim 1, characterized in that: In the step (1), the complexing agent is one or more of ammonia water and ethylenediaminetetraacetic acid, and the concentration is 85-200 g / L.

6. The method for preparing a porous hollow ternary precursor according to claim 1, characterized in that: In the step (2), the pumping flow rate of the ternary mixed metal salt solution is 30 to 600 L / h; the pumping flow rate of the inorganic aluminum alkali solution is 15 to 400 L / h.

7. The method for preparing a porous hollow ternary precursor according to claim 1, characterized in that: The strong base added in step (3) is at least one of sodium hydroxide and potassium hydroxide, and the stirring time is 10 to 24 hours.

8. A porous hollow ternary precursor prepared by the preparation method according to any one of claims 1 to 7.