A 6XXX aluminum alloy and preparation method thereof
By forming ultrafine subcrystals and nano-scale reinforced phases in 6XXX aluminum alloy, combined with thermal deformation treatment, the problem of grain boundary orientation difference regulation in the prior art is solved, and the fatigue performance and corrosion resistance of the material are significantly improved.
Patent Information
- Application Number
- CN202310223111.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-09
AI Technical Summary
The existing 6XXX aluminum alloys are difficult to effectively reduce the fatigue crack propagation rate in regulating the grain boundary orientation difference, resulting in insufficient fatigue performance.
By forming a large number of ultrafine subcrystals and nano-scale reinforced phases in aluminum alloys, combined with thermal deformation treatment, the grain boundary orientation difference is controlled less than 5°, and the composition design is optimized to obtain small angles through homogenization and solution/aging treatment processes. Ultrafine subcrystalline structure and fine diffuse phases inhibit recrystallization and grain growth.
It significantly improves the strength, fatigue resistance and corrosion resistance of aluminum alloy, reduces the spreading rate of fatigue cracks, enhances the bonding ability of grain boundaries, and extends the forward distance of fatigue cracks.
Smart Images

Figure CN116200631B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to a 6XXX aluminum alloy and a preparation method thereof. Background Art
[0002] At present, aluminum alloy is the preferred material for lightweight automobiles, especially automobile chassis parts. Among aluminum alloys, 6XXX aluminum alloy is easy to process, has good corrosion resistance, good welding performance and medium strength, which is very suitable for automobile chassis. Because automobile chassis parts work under alternating stress for a long time, the alloy used to prepare the parts is required to have good fatigue performance.
[0003] Researchers use equal channel angular extrusion or other violent deformation methods to obtain high-density dislocations or fine recrystallized structures to improve the strength of the alloy, thereby improving the fatigue performance of the alloy. The current methods to improve the fatigue resistance of aluminum alloys can be summarized as follows: one is to strengthen the yield strength of the body, thereby increasing the critical stress for fatigue crack initiation; the other is to refine the grain size, increase the distance to resist fatigue crack propagation, and thus reduce its propagation rate.
[0004] However, different grain boundaries have different abilities to resist crack growth, and thus have different effects on fatigue crack growth rate. Currently, there is still a gap in regulating the misorientation of grain boundaries to reduce fatigue crack growth rate. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a 6XXX aluminum alloy and a preparation method thereof, so as to form a large number of ultrafine subgrains and nano-scale strengthening phases in the aluminum alloy structure and improve the strength, fatigue resistance and corrosion resistance of the 6XXX aluminum alloy.
[0006] To achieve the above-mentioned object, the present invention provides a 66XXX aluminum alloy, wherein the aluminum alloy comprises the following components in percentage by mass: Si: 0.4-1.4, Mg: 0.4-1.2, Cu: 0-0.6, Mn: 0.2-0.8, Cr: 0.1-0.4, Ti≤0.03, Fe≤0.15, Zr≤0.2, Zn≤0.2, Ni≤0.01, Mo≤0.01, V≤0.01, single impurity≤0.02, total impurity≤0.1, and the balance is Al;
[0007] After the aluminum alloy is melt-cast and homogenized, a uniformly distributed nano-scale dispersed phase is formed inside the aluminum alloy grains. After thermal deformation, the ultrafine subgrains with a grain boundary orientation difference of less than 5° in the internal grains account for more than 50%, and the low orientation difference subgrains with a grain boundary orientation difference of less than 10 μm account for more than 60%.
[0008] Preferably, in the aluminum alloy composition, the total amount of Mn and Cr does not exceed 0.9%.
[0009] Preferably, the nanoscale dispersed phase comprises a nanoscale Al3X dispersed phase, wherein X is selected from one or more of Ni, Ti, Zr, Mo, and V.
[0010] Preferably, the nanoscale dispersed phase comprises a nanoscale Al(FeMnY)Si dispersed phase, wherein Y is selected from Cr and / or Cu.
[0011] Preferably, the size of the dispersed phase is 20-350 nm.
[0012] Preferably, in the crystal grains, the proportion of ultrafine subgrains with a grain boundary orientation difference of less than 5° is greater than 55%, and the proportion of low orientation difference subgrains with a grain boundary orientation difference of less than 10 μm is greater than 75%.
[0013] The present invention also provides a method for preparing a 6XXX aluminum alloy, comprising the following preparation steps:
[0014] S1, melting and homogenizing the aluminum alloy ingredients;
[0015] S2, thermally deforming the aluminum alloy under certain processing conditions to form an ultrafine sub-grain structure with a small orientation difference in the treated aluminum alloy profile;
[0016] S3. Perform solid solution or aging treatment on the aluminum alloy profile.
[0017] Preferably, the homogenization process in S2 includes:
[0018] Homogenization treatment at 240-420°C for 5-11h;
[0019] Homogenization treatment at 520-575°C for 9-16h;
[0020] The cooling is performed at a cooling rate of 90-810°C / h.
[0021] Preferably, the heating rate during the homogenization treatment is ≤3°C / min, and the cooling is performed at a cooling rate of 100-810°C / h to below 100°C.
[0022] Preferably, the heat treatment in S3 is a forging treatment, the forging temperature during the forging treatment is 500-550° C., the deformation rate is 0.001-10.5 / s, and the deformation amount is 0.45-0.95.
[0023] The present invention obtains a subgrain deformation structure with a 0-5° orientation difference in the structure of the 6XXX aluminum alloy. Since the small-angle grain boundary with an orientation difference of 0-5° has a large binding energy, more energy is required per unit area to tear the fatigue crack when it expands along it. Therefore, the small orientation difference and the fine subgrain structure not only reduce the width of the striations of each fatigue expansion, but also increase the advancing distance of the fatigue crack, thereby reducing the expansion rate of the fatigue crack.
[0024] The present invention further obtains the small-angle ultrafine subgrain structure from a process approach, by using a large number of fine and evenly distributed Al3X and Al(FeMnY)Si dispersed phases of 20-300nm in size and combining the migration of subgrain boundaries with a hot deformation process, refining the subgrain size and controlling the deformed structure to a ratio of 50-90%, and obtaining subgrains with an orientation difference of 0-5° in the deformed structure.
[0025] The present invention further optimizes the alloy composition design so that the dispersed phase precipitated in the matrix is coherent with the matrix, thereby obtaining a large number of fine dispersed phases. The distribution uniformity of the dispersed phase is improved through a bipolar homogenization process, and the dispersed phase is made to obtain a large number of fine subgrains with small orientation differences through thermal deformation, and the occurrence of recrystallization is suppressed. And through the thermal deformation process, dislocations are accumulated near the grain boundary to provide a nucleation position for the precipitated phase, thereby reducing the grain boundary non-precipitation zone PFZ, further improving the grain boundary strength, and further suppressing the generation and expansion of fatigue cracks. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic flow diagram of a method for preparing 6XXX aluminum alloy of the present invention;
[0027] Figure 2 Schematic diagram of the distribution of dispersed phase in the aluminum alloy structure of Example 1 of the present invention;
[0028] Figure 3 is a schematic diagram of the SN curve in the aluminum alloy structure of Example 1 of the present invention;
[0029] Figure 4 is a subgrain structure diagram of the aluminum alloy of Example 1 of the present invention;
[0030] Figure 5 It is a schematic diagram of the subgrain orientation distribution in the aluminum alloy structure of Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. The structural, method, or functional changes made by ordinary technicians in the field according to these embodiments are all included in the protection scope of the present invention.
[0032] Example 1
[0033] The 6xxx aluminum alloy proposed in this embodiment includes the following components in mass percentage: Si: 0.4, Mg: 0.4, Cu: 0.3, Mn: 0.4, Cr: 0.2, Ti: 0.03, Fe: 0.15, Zn: 0.2, Zr: 0.2, Ni: 0.01, Mo: 0.01, V: 0.01, single impurity ≤ 0.02, total impurities ≤ 0.1, and the balance is Al.
[0034] The preparation method of the 6xxx aluminum alloy, combined with Figure 1 As shown, the preparation steps include:
[0035] Step 1: batching, batching the ingredients according to the mass percentage of the aluminum alloy, and producing round ingots through processes such as refining, standing and melting.
[0036] Step 2: homogenization treatment, according to the first stage homogenization treatment at a temperature of 240°C for 5 hours, and then the second stage homogenization treatment at a temperature of 520°C for 9 hours, followed by strong wind cooling at a cooling rate of 100°C / h, to obtain an aluminum alloy ingot with uniformly distributed nano-scale dispersed phases, including Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases, such as Figure 2 The diagram shows the distribution of the dispersed phase. Figure 2 It can be seen that the dispersed phase is fine and uniform.
[0037] In the semi-continuous casting process, alloy elements will form micro-segregation in the crystal, which will cause uneven distribution of dispersed phases, thereby reducing the regulatory effect on the subsequent subgrain size. Therefore, in addition to considering the elimination of component segregation and casting stress, homogenization also focuses on the formation and control of dispersed phases. The alloy composition determines the type and total volume fraction of nano-scale Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases, and the homogenization system determines the distribution and size of nano-scale Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases. The present invention requires that nano-scale Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases are uniformly distributed inside the aluminum alloy grains, and their size after homogenization is 20-350nm.
[0038] Step 3: Forging heat treatment of the aluminum alloy ingot. Forging heat treatment is another determining factor for the formation and size of ultrafine subgrains. In this embodiment, the forging temperature is maintained at 500°C, the heating gradient is controlled at 10°C / min, the forging rate should be controlled at 0.001 / s; the forging amount is 0.45 for forging hot deformation treatment. Since the formation of PFZ (Precipitation Free Zone, grain boundary no precipitation zone) is due to the lack of nucleation particles near the grain boundary of the precipitated phase, the present invention introduces dislocations near the grain boundary through a hot deformation process, provides nucleation particles for the precipitated phase and reduces PFZ, thereby strengthening the bonding ability of the grain boundary to inhibit the generation and expansion of fatigue cracks. After forging, the material has a fine grain structure and no recrystallization occurs. After solution and aging treatment, recrystallization and grain growth occur. Many grain growths are hindered by the dispersed phase, forming a large number of small-sized and small-orientation-different subgrains, thereby providing a large number of small-angle grain boundaries for the material.
[0039] Step 4: Aging treatment: the forging material should be kept at 165℃ for 8 hours in the aging furnace, and then air-cooled after being taken out of the furnace. According to the aging process system, the forging material should be quenched after aging.
[0040] After aging, the fatigue performance and microstructure are tested. The results of fatigue testing of forged materials are as follows Figure 3 As shown in the SN curve (loading stress-loading force cycle number curve), the measured fatigue strength is 157.5MPa, and the calculated fatigue strength is 148.0MPa.
[0041] The deformation structure of WHS extruded profiles was characterized by EBSD. Figure 4 , 5 As shown, the substructure orientation difference results show that the alloy structure has 82% deformation structure, of which small-angle subgrain structure (ultrafine subgrain structure with orientation difference <5°) accounts for 67%, and grains with low orientation difference less than 10μm account for 82%. A large amount of ultrafine subgrain structure ensures the fatigue resistance of the product.
[0042] Example 2
[0043] The 6xxx aluminum alloy proposed in this embodiment includes the following components in mass percentage: Si: 1.0, Mg: 0.9, Cu: 0.5, Mn: 0.5, Cr: 0.2, Ti: 0.02, Fe: 0.10, Zn: 0.1, Zr: 0.1, Ni: 0.01, Mo: 0.01, V: 0.01, single impurity ≤ 0.02, total impurities ≤ 0.1, and the balance is Al.
[0044] The preparation method of the 6xxx aluminum alloy comprises the following preparation steps:
[0045] Step 1: batching, batching the ingredients according to the mass percentage of the aluminum alloy, and producing round ingots through processes such as refining, standing and melting.
[0046] Step 2: homogenization treatment, homogenization treatment, according to the first stage homogenization treatment at a temperature of 350°C for 8 hours, and then at a temperature of 550°C for 12 hours. After that, strong wind cooling at a cooling rate of 400°C / h is performed to obtain uniformly distributed nano-scale dispersed phases, including aluminum alloy ingots such as Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases.
[0047] Step 3: Heat treatment of aluminum alloy ingots during forging, keep the forging temperature at 525℃, control the heating gradient at 40℃ / min, and control the forging rate at 2.5 / s; keep the forging volume at 0.6 for forging process conditions for hot deformation treatment. Step 4: Aging treatment, keep the forging material at 170℃ in the aging furnace for 10 hours, and air cool it out of the furnace. According to the aging process system, the forging material is quenched after aging.
[0048] After aging, the fatigue properties and microstructure were tested. The fatigue strength of the forged material was 157.5 MPa and the calculated fatigue strength was 148.0 MPa.
[0049] The microstructure was measured and the substructure orientation difference results showed that the alloy structure had 82.1% deformation structure, of which there were a large number of small-angle subgrains (ultrafine subgrains with orientation difference <5°), accounting for 67.5%, and the proportion of grains with low orientation difference less than 10μm reached 82.8%. A large number of ultrafine subgrains ensure the fatigue resistance of the product.
[0050] Example 3
[0051] The 6xxx aluminum alloy proposed in this embodiment includes the following components in mass percentage: Si: 1.4, Mg: 1.2, Cu: 0.8, Mn: 0.8, Cr: 0.4, Ti: 0.03, Fe: 0.15, Zn: 0.2, Zr: 0.2, Ni: 0.01, Mo: 0.01, V: 0.01, single impurity ≤ 0.02, total impurities ≤ 0.1, and the balance is Al.
[0052] Step 1: batching, batching the ingredients according to the mass percentage of the aluminum alloy, and producing round ingots through processes such as refining, standing and melting.
[0053] Step 2: homogenization treatment, according to the first stage homogenization treatment at a temperature of 350°C for 8 hours, and then the second stage homogenization treatment at a temperature of 550°C for 12 hours, followed by strong wind cooling at a cooling rate of 810°C / h to obtain uniformly distributed nano-scale dispersed phases, including aluminum alloy ingots such as Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases.
[0054] Step 3: Forge the aluminum alloy ingot, keep the forging temperature at 525°C, the heating gradient should be controlled at 40°C / min, the forging rate should be controlled at 2.5 / s; the forging volume is maintained at 0.6.
[0055] Step 4: Aging treatment: the forgings are kept at 170℃ for 10 hours in the aging furnace before aging for 12 hours, and then air-cooled after being taken out of the furnace. According to the aging process system, the forgings are quenched after aging.
[0056] After aging, the fatigue properties and microstructure were tested. The fatigue strength of the forged material was 159.5MPa and the calculated fatigue strength was 153.0MPa.
[0057] The microstructure was measured and the substructure orientation difference results showed that the alloy structure had 82.6% deformation structure, of which small-angle subgrain structure (ultrafine subgrain structure with orientation difference <5°) accounted for 67.8%, and grains with low orientation difference less than 10μm accounted for 82.9%. A large amount of ultrafine subgrain structure ensures the fatigue resistance of the product.
[0058] Example 4
[0059] Step 1: Ingredients are prepared according to the following mass percentages: Si: 1.0, Mg: 0.9, Cu: 0.5, Mn: 0.81, Cr: 0.4, Ti: 0.02, Fe: 0.10, Zn: 0.1, Zr: 0.1, Ni: 0.01, Mo: 0.01, V: 0.01, single impurity ≤ 0.02, total impurity ≤ 0.1, and the balance is Al. The above ingredients are refined, placed, melted, and cast to produce round ingots.
[0060] Step 2: homogenization treatment, according to the first stage homogenization treatment at a temperature of 350°C for 8 hours, and then the second stage homogenization treatment at a temperature of 550°C for 12 hours, followed by strong wind cooling at a cooling rate of 400°C / h to obtain an aluminum alloy ingot with uniformly distributed nano-scale Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases.
[0061] Step 3: Forging the aluminum alloy ingot, maintaining the forging temperature at 525°C, the heating gradient at 40°C / min, the forging rate at 2.5 / s; and the forging amount at 0.6.
[0062] Step 4: Aging treatment: the forgings are kept at 170℃ for 10 hours in the aging furnace before aging for 12 hours, and then air-cooled after being taken out of the furnace. According to the aging process system, the forgings are quenched after aging.
[0063] After aging, the fatigue properties and microstructure were tested. The fatigue strength of the forged material was 119.5MPa and the calculated fatigue strength was 113.1MPa.
[0064] The microstructure was measured and the substructure orientation difference results showed that the alloy structure had 84% deformation structure, of which small-angle subgrain structure (ultrafine subgrain structure of <5°) accounted for 47.7%, and grains with low orientation difference less than 10μm accounted for 42.6%. This is because the total amount of Mn and Cr in this embodiment exceeds the range of 0.9%.
[0065] Example 5
[0066] Step 1: Ingredients are prepared according to the following mass percentages: Si: 1.0, Mg: 0.9, Cu: 0.5, Mn: 0.5, Cr: 0.2, Ti: 0.02, Fe: 0.10, Zn: 0.1, Zr: 0.1, Ni: 0.01, Mo: 0.01, V: 0.01, single impurity ≤ 0.02, total impurity ≤ 0.1, and the balance is Al. The above ingredients are refined, placed, melted, and cast to produce round ingots.
[0067] Step 2: homogenization treatment, according to the first stage homogenization treatment at a temperature of 430°C for 12 hours, and then the second stage homogenization treatment at a temperature of 580°C for 17 hours, followed by strong wind cooling at a cooling rate of 400°C / h to obtain an aluminum alloy ingot with uniformly distributed nano-scale Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases.
[0068] Step 3: Forging the aluminum alloy ingot, maintaining the forging temperature at 555°C, the heating gradient at 40°C / min, the forging rate at 10.6 / s; and the forging amount at 0.96.
[0069] Step 4: Aging treatment: the forgings are kept at 170℃ for 10 hours in the aging furnace before aging for 12 hours, and then air-cooled after being taken out of the furnace. According to the aging process system, the forgings are quenched after aging.
[0070] After aging, the fatigue properties and microstructure were tested. The fatigue strength of the forged material was measured to be 99.4 MPa and the calculated fatigue strength was 97.9 MPa.
[0071] The microstructure was measured and the substructure orientation difference results showed that the structure had 82.9% deformed structure, of which small-angle subgrain structure (ultrafine subgrain structure of <5°) accounted for 37.7%, and grains with low orientation difference less than 10μm accounted for 42.7%. This is because the temperature of the homogenization treatment in this embodiment exceeds the temperature range set by the present invention.
[0072] Example 6
[0073] Step 1: Ingredients are prepared according to the following mass percentages: Si: 1.0, Mg: 0.9, Cu: 0.5, Mn: 0.5, Cr: 0.2, Ti: 0.02, Fe: 0.10, Zn: 0.1, Zr: 0.1, Ni: 0.01, Mo: 0.01, V: 0.01, single impurity ≤ 0.02, total impurity ≤ 0.1, and the balance is Al. The above ingredients are refined, placed, melted, and cast to produce round ingots.
[0074] Step 2: homogenization treatment, according to the first stage homogenization treatment at a temperature of 230°C for 4 hours, and then the second stage homogenization treatment at a temperature of 510°C for 8 hours, followed by strong wind cooling at a rate of 400°C / h to obtain an aluminum alloy ingot with uniformly distributed nano-scale Al3(NiTiZrMoV) and Al(FeMnCrCu)Si dispersed phases.
[0075] Step 3: Forging the aluminum alloy ingot, maintaining the forging temperature at 495°C, the heating gradient at 40°C / min, the forging rate at 0.0009 / s; and the forging amount at 0.44.
[0076] Step 4: Aging treatment: the forgings are kept at 170℃ for 10 hours in the aging furnace before aging for 12 hours, and then air-cooled after being taken out of the furnace. According to the aging process system, the forgings are quenched after aging.
[0077] After aging, the fatigue properties and microstructure were tested. The fatigue strength of the forged material was measured to be 99.6 MPa and the calculated fatigue strength was 96.1 MPa.
[0078] The microstructure was measured and the results of substructure orientation difference showed that the deformed structure had 73.2% deformed structure, of which small-angle subgrain structure (ultrafine subgrain structure of <5°) accounted for 48.2%, and grains with low orientation difference less than 10μm accounted for 43.1%. This is because the heat treatment process in this embodiment exceeds the range set by the present invention.
[0079] The present invention controls the formation of nano-scale dispersed phases by component design, and obtains the target grain structure by combining the hot deformation process, thereby achieving the process of inhibiting recrystallization and grain growth. Under the unified solution / aging treatment process, the comparative implementation cases of other component samples did not reach the target yield strength and fatigue strength, as shown in other comparative examples 1-6 in Table 1 below.
[0080]
[0081]
[0082]
[0083] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A 6XXX aluminum alloy, It is characterized in that The aluminum alloy comprises the following components in mass percentage: Si: 0.4-1.4, Mg: 0.4-1.2, Cu: 0-0.6, Mn: 0.2-0.8, Cr: 0.1-0.4, Ti≤0.03, Fe≤0.15, Zr≤0.2, Zn≤0.2, Ni≤0.01, Mo≤0.01, V≤0.01, Mn+Cr≤0.9, single impurity≤0.02, total impurity≤0.1, and the balance is Al; After the aluminum alloy is melt-cast and homogenized, a uniformly distributed nano-scale dispersed phase is formed inside the aluminum alloy grains; after thermal deformation treatment, the deformed structure in the alloy structure is controlled to be 50-90%, the proportion of ultrafine subgrains with a grain boundary orientation difference of less than 5° in the internal grains is greater than 50%, and the proportion of subgrains with an orientation difference of less than 10μm and less than 5° is greater than 60%.
2. The 6XXX aluminum alloy according to claim 1, It is characterized in that In the aluminum alloy composition, the total amount of Mn and Cr does not exceed 0.9%.
3. The 6XXX aluminum alloy according to claim 1, It is characterized in that The nano-scale dispersed phase includes nano-scale Al 3 X dispersed phase, wherein X is selected from one or more of Ni, Ti, Zr, Mo, and V.
4. The 6XXX aluminum alloy according to claim 1, It is characterized in that The nano-scale dispersed phase comprises a nano-scale Al(FeMnY)Si dispersed phase, wherein Y is selected from Cr and / or Cu.
5. The 6XXX aluminum alloy of claim 1, It is characterized in that The size of the dispersed phase is 20-350 nm.
6. The 6XXX aluminum alloy of claim 1, It is characterized in that In the crystal grains, the ultrafine subgrains with a grain boundary orientation difference of less than 5° account for more than 55%, and the subgrains with an orientation difference of less than 10 μm and less than 5° account for more than 75%.
7. A method for preparing the 6XXX aluminum alloy according to any one of claims 1 to 6, It is characterized in that The method comprises the following preparation steps: S1, melting and homogenizing the aluminum alloy ingredients; S2, thermally deforming the aluminum alloy under certain processing conditions to form an ultrafine sub-grain structure with a small orientation difference in the treated aluminum alloy profile; S3. Perform aging treatment on the aluminum alloy profile.
8. The method for preparing the 6XXX aluminum alloy according to claim 7, It is characterized in that The homogenization process in S1 includes: Homogenization treatment at 240-420°C for 5-11h; Homogenization treatment at 520-575°C for 9-16h; The cooling is performed at a cooling rate of 90-810°C / h.
9. The method for preparing the 6XXX aluminum alloy according to claim 8, It is characterized in that The heating rate during the homogenization treatment is ≤3°C / min, and the cooling is performed at a cooling rate of 100-810°C / h to below 100°C.
10. The method for preparing the 6XXX aluminum alloy according to claim 7, It is characterized in that The thermal deformation in S2 is a forging process, the forging temperature during the forging process is 500-550° C., the deformation rate is 0.001-10.5 / s, and the deformation amount is 0.45-0.95.